Micro-nano dual-scale particle reinforced nickel-silicon brass and preparation method thereof
By forming the structural structure of micro-nano double-scale particles in nickel silicon brass, the problem of insufficient strong plasticity of the existing nickel silicon brass matrix is solved, and its strength and toughness and wear resistance are significantly improved. It is suitable for high-strength wear-resistant components Development.
Patent Information
- Application Number
- CN202410970809.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing nickel-silicon brass matrix Cu-Zn solid solution has insufficient strong plasticity, resulting in insufficient strength and toughness, which cannot meet the mechanical performance requirements of high-strength wear-resistant components.
Micron-scale NiAl(Si) primary phase particles were prepared by in-situ self-generating method, and combined with isothermal heat treatment and quenching process, uniformly distributed nano-scale NiAl(Si) precipitation phase was formed in the Cu-Zn solid solution matrix to form micro-nano double- Microstructure structures of scale particle reinforcement.
It significantly improves the strength and wear resistance of nickel-silicon brass, achieves high tensile strength and elongation, and is suitable for the development and preparation of new high-strength wear-resistant components.
Smart Images

Figure CN118880106A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and relates to a high-strength wear-resistant copper alloy, and specifically to a micro-nano dual-scale particle reinforced nickel-silicon brass and a preparation method thereof. Background Art
[0002] Nickel-silicon brass refers to a multi-element alloy system composed of a small amount of alloying elements such as Ni, Al, Mn, Si, and Fe added to the Cu-Zn alloy. It has a composite structure composed of a Cu-Zn solid solution matrix and hard phase particles, showing excellent mechanical properties, thermal conductivity, and wear resistance. It has a wide and urgent application demand in the fields of high-strength wear-resistant parts such as transmission synchronous gear rings, bearings, bushings, and brake pads. Among them, the matrix, as the main component of nickel-silicon brass, plays a role in dispersing loads and protecting hard phase particles during service, and transfers loads to the hard phase in the form of shear force. Therefore, the strength and plasticity of the matrix directly affect the mechanical properties of nickel-silicon brass.
[0003] However, the matrix of the nickel-silicon brass currently prepared is a single Cu-Zn solid solution. Although it has good plasticity, it lacks toughness. The reason is that a large amount of alloying elements in the Cu-Zn solid solution only improve the alloy strength by solid solution strengthening, which is not enough for the service requirements of the product. Summary of the invention
[0004] In view of this, in order to solve this problem, the present invention discloses a micro-nano dual-scale particle reinforced nickel-silicon brass and a preparation method thereof. On the basis of preparing micron-sized NiAl(Si) particle reinforced nickel-silicon brass by an in-situ autogenous method, uniformly distributed nano-sized NiAl(Si) particles are formed in a Cu-Zn solid solution matrix by a method combining isothermal heat treatment with a quenching process, thereby significantly improving the toughness of the matrix. The present invention ultimately forms a microstructure of synergistic reinforcement of micron-sized NiAl(Si) primary phase particles and nano-sized NiAl(Si) precipitation phase particles, thereby significantly improving the toughness and wear resistance of nickel-silicon brass.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] The first object of the present invention is to provide a method for preparing a micro-nano dual-scale particle reinforced nickel-silicon brass, firstly synthesizing micron-sized NiAl(Si) primary phase particles in nickel-silicon brass by an in-situ autogenous method, and then forming uniformly distributed nano-sized NiAl(Si) precipitation phase particles in a Cu-Zn solid solution matrix by a method combining isothermal heat treatment with a quenching process, so as to prepare a high-strength and high-elongation micro-nano dual-scale particle reinforced nickel-silicon brass; the method specifically comprises the following steps:
[0007] 1) The prefabricated alloy composition of the micro-nano dual-scale particle reinforced nickel-silicon brass: 53.5-58.5wt.% Cu, 3.5-3.8wt.% Al, 5.0-8.5wt.% Ni, 1.5-2.5wt.% Si, 0.2-0.4wt.% Mn, 0.4-0.6wt.% Fe, and the balance is Zn;
[0008] 2) pure Cu, pure Al, pure Zn, pure Ni, pure Fe, Cu-Mn master alloy and Cu-Si master alloy with the surface oxide scale removed are mixed according to the mass percentage in step 1), and placed in a drying oven at a temperature of 60 to 80° C. for drying;
[0009] 3) Under argon protection, the pure Cu in step 2) is heated in a medium frequency induction furnace until it is melted, and when the melt temperature is 1200-1300° C., pure Ni, pure Fe, Cu-Mn master alloy, Cu-Si master alloy and pure Al are added in sequence;
[0010] 4) Continue heating until the material added in step 3) is completely melted, keep the melt temperature at 1200-1300° C., apply electromagnetic stirring for 40-50 seconds to ensure that the alloy elements are evenly diffused in the alloy melt;
[0011] 5) The temperature of the alloy melt is controlled at 1080-1130° C. by adjusting the heating power, and the pure Zn block in step 2) is wrapped with Cu foil and pressed into the alloy melt in multiple times to prevent the Zn block from directly contacting the high-temperature melt and causing burning. During this period, the melt temperature must be strictly controlled to avoid excessive temperature causing serious flame spurting of the melt and causing a large amount of Zn burning;
[0012] 6) After the pure Zn block is completely added to the alloy melt, electromagnetic stirring is applied for 40 to 50 seconds, and the temperature of the alloy melt is increased to 1140 to 1150°C twice, and flame spraying and degassing are performed;
[0013] 7) After the melt is sprayed, let it stand for 10 to 20 seconds, and then cast the alloy melt into a cylindrical graphite mold preheated to 200 to 250°C to cool;
[0014] 8) The alloy ingot obtained in step 7) is placed in a muffle furnace at a temperature of 830-870° C. for isothermal heat treatment for 0.5-1 h. After the isothermal heat treatment, the ingot is placed in water for rapid cooling to obtain the target nickel-silicon brass.
[0015] It should be noted that the present invention innovatively proposes a method for improving the mechanical properties of nickel-silicon brass by forming micro-nano dual-scale hard phase particles in nickel-silicon brass. First, a micron-sized NiAl(Si) primary phase-reinforced nickel-silicon brass is prepared by an in-situ autogenous method, and then spherical NiAl(Si) precipitation phase particles with a size of about tens of nanometers are formed in a Cu-Zn solid solution matrix by a method combining isothermal heat treatment with a quenching process, which significantly improves the toughness of the matrix, and synergistically improves the strength, hardness and wear resistance of nickel-silicon brass by combining NiAl(Si) primary phase particles. The micro-nano dual-scale particle-reinforced nickel-silicon brass prepared by the present invention has high tensile strength (580-670MPa) and elongation (4.0-5.3%), which is of great significance to the design and development of new high-strength and wear-resistant nickel-silicon brass.
[0016] The second object of the present invention is to provide a micro-nano dual-scale particle reinforced nickel-silicon brass prepared by the method described above.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The nickel-silicon brass prepared by the present invention has a microstructure of synergistic reinforcement of micron-sized NiAl(Si) primary phase particles and nano-sized NiAl(Si) precipitation phase particles, wherein the micron-sized primary phase provides the alloy with higher hardness and wear resistance, while the nano-sized precipitation phase further improves the toughness of the matrix, thereby achieving synergistic strengthening of the alloy. Mechanical property testing has found that the prepared micro-nano dual-scale particle-reinforced nickel-silicon brass has higher tensile strength and elongation.
[0019] (2) The present invention innovatively designs and obtains a synergistically reinforced organizational structure of dual-scale hard phase particles in nickel-silicon brass by combining isothermal heat treatment with quenching process, thereby effectively improving the strength and toughness of nickel-silicon brass. This has a significant promoting effect on the development and preparation of new high-strength and wear-resistant nickel-silicon brass. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0021] Figure 1 Microstructure images of the micro-nano dual-scale particle reinforced nickel-silicon brass prepared in Example 1: (a) low-magnification microstructure image, (b) high-magnification microstructure image.
[0022] Figure 2The stress-strain curve of the micro-nano dual-scale particle reinforced nickel-silicon brass prepared in Example 1.
[0023] Figure 3 Microstructure images of the micro-nano dual-scale particle reinforced nickel-silicon brass prepared in Example 2: (a) low-magnification microstructure image, (b) high-magnification microstructure image.
[0024] Figure 4 The stress-strain curve of the micro-nano dual-scale particle reinforced nickel-silicon brass prepared in Example 2. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0027] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0028] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0029] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0030] The invention discloses a high-strength and high-elongation micro-nano dual-scale particle reinforced nickel-silicon brass and a preparation method thereof.
[0031] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0032] Example 1
[0033] A method for preparing micro-nano dual-scale particle reinforced nickel-silicon brass, the method comprising the following steps:
[0034] 1) The prefabricated alloy composition of the micro-nano dual-scale particle reinforced nickel-silicon brass: 57.5wt.% Cu, 3.5wt.% Al, 7.5wt.% Ni, 2.1wt.% Si, 0.4wt.% Mn, 0.5wt.% Fe, and the balance Zn;
[0035] 2) pure Cu, pure Al, pure Zn, pure Ni, pure Fe, Cu-Mn master alloy and Cu-Si master alloy with surface oxide scale removed are prepared according to the mass percentage in step 1), and placed in a drying oven at a temperature of 80° C. for drying;
[0036] 3) Under argon protection, the pure Cu in step 2) is heated in a medium frequency induction furnace until it is melted, and when the melt temperature is 1290° C., pure Ni, pure Fe, Cu-Mn master alloy, Cu-Si master alloy and pure Al are added in sequence;
[0037] 4) Continue heating until the material added in step 3) is completely melted, keep the melt temperature at 1290° C., apply electromagnetic stirring for 50 seconds to allow the solute in the alloy melt to fully diffuse;
[0038] 5) The temperature of the alloy melt is controlled at 1100° C. by adjusting the heating power, and the pure Zn block in step 2) is wrapped with Cu foil and pressed into the alloy melt in multiple times. During this period, the melt temperature must be strictly controlled to avoid excessive temperature causing serious flame spurting of the melt and causing a large amount of Zn burning;
[0039] 6) After the pure Zn block is completely added to the alloy melt, electromagnetic stirring is applied for 40 seconds, and the temperature of the alloy melt is increased to 1140°C twice, and flame spraying and degassing are performed;
[0040] 7) After the melt is sprayed, let it stand for 20 seconds, and then cast the alloy melt into a cylindrical graphite mold preheated to 200°C to cool;
[0041] 8) The alloy ingot obtained in step 7) is placed in a muffle furnace at a temperature of 840° C. for isothermal heat treatment for 0.5 h. After the isothermal heat treatment, the ingot is placed in water for rapid cooling to obtain the target nickel-silicon brass.
[0042] The nickel-silicon brass prepared according to Example 1 forms a microstructure of synergistic reinforcement by micro-nano dual-scale particles, wherein the size of the micron-scale primary phase particles is 10-20 μm, and the size of the nano-scale precipitated phase is 80-120 nm; the prepared micro-nano dual-scale particle reinforced nickel-silicon brass has excellent mechanical properties with a tensile strength of 623 MPa and an elongation of 4.3%, providing a basis for its excellent wear resistance.
[0043] Example 2
[0044] A method for preparing micro-nano dual-scale particle reinforced nickel-silicon brass, the method comprising the following steps:
[0045] 1) The prefabricated alloy composition of the micro-nano dual-scale particle reinforced nickel-silicon brass: 59.5wt.% Cu, 3.8wt.% Al, 4.0wt.% Ni, 1.2wt.% Si, 0.4wt.% Mn, 0.4wt.% Fe, and the balance Zn;
[0046] 2) pure Cu, pure Al, pure Zn, pure Ni, pure Fe, Cu-Mn master alloy and Cu-Si master alloy with surface oxide scale removed are prepared according to the mass percentage in step 1), and placed in a drying oven at a temperature of 80° C. for drying;
[0047] 3) Under argon protection, the pure Cu in step 2) is heated in a medium frequency induction furnace until it is melted, and when the melt temperature is 1270° C., pure Ni, pure Fe, Cu-Mn master alloy, Cu-Si master alloy and pure Al are added in sequence;
[0048] 4) Continue heating until the material added in step 3) is completely melted, keep the melt temperature at 1270° C., apply electromagnetic stirring for 50 seconds to allow the solute in the alloy melt to fully diffuse;
[0049] 5) The temperature of the alloy melt is controlled at 1090° C. by adjusting the heating power, and the pure Zn block in step 2) is wrapped with Cu foil and pressed into the alloy melt in multiple times. During this period, the melt temperature must be strictly controlled to avoid excessive temperature causing serious flame spurting of the melt and causing a large amount of Zn burning;
[0050] 6) After the pure Zn block is completely added to the alloy melt, electromagnetic stirring is applied for 40 seconds, and the temperature of the alloy melt is increased to 1145°C twice, and flame spraying and degassing are performed;
[0051] 7) After the melt is sprayed, it is left to stand for 20 seconds, and the alloy melt is cast into a cylindrical graphite mold preheated to 220°C and cooled;
[0052] 8) The alloy ingot obtained in step 7) is placed in a muffle furnace at a temperature of 850° C. for isothermal heat treatment for 1.0 h. After the isothermal heat treatment, the ingot is placed in water for rapid cooling to obtain the target nickel-silicon brass.
[0053] The nickel-silicon brass prepared according to Example 2 forms a microstructure of synergistic reinforcement by micro-nano dual-scale particles, wherein the size of the micron-scale primary phase particles is 7 to 15 μm, and the size of the nano-scale precipitated phase is 90 to 150 nm; the prepared micro-nano dual-scale particle reinforced nickel-silicon brass has excellent mechanical properties with a tensile strength of 592 MPa and an elongation of 5.1%, providing a basis for its excellent wear resistance.
[0054] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing micro-nano dual-scale particle reinforced nickel-silicon brass, characterized in that: Firstly, micron-sized NiAl(Si) primary phase particles are synthesized in nickel-silicon brass by an in-situ autogenous method, and then uniformly distributed nano-sized NiAl(Si) precipitation phase particles are formed in a Cu-Zn solid solution matrix by a method combining isothermal heat treatment with a quenching process, so as to prepare a high-strength and high-elongation micro-nano dual-scale particle reinforced nickel-silicon brass; the method specifically comprises the following steps: 1) The prefabricated alloy composition of the micro-nano dual-scale particle reinforced nickel-silicon brass: 53.5-58.5wt.% Cu, 3.5-3.8wt.% Al, 5.0-8.5wt.% Ni, 1.5-2.5wt.% Si, 0.2-0.4wt.% Mn, 0.4-0.6wt.% Fe, and the balance is Zn; 2) pure Cu, pure Al, pure Zn, pure Ni, pure Fe, Cu-Mn master alloy and Cu-Si master alloy with surface oxide scale removed are prepared according to the mass percentage in step 1), and then dried for standby use; 3) Under argon protection, the pure Cu in step 2) is heated in a medium frequency induction furnace until it is melted, and pure Ni, pure Fe, Cu-Mn master alloy, Cu-Si master alloy and pure Al are added in sequence; heating is continued until the added materials are completely melted, and then the temperature is kept and electromagnetic stirring is applied to allow the solute in the alloy melt to fully diffuse; 4) Wrapping the pure Zn block in step 2) with Cu foil and pressing it into the alloy melt in multiple times, during which the melt temperature must be strictly controlled to avoid excessive temperature causing severe flame spurting of the melt and causing a large amount of Zn burning; 5) After the pure Zn block is completely added to the alloy melt, electromagnetic stirring is applied, and the temperature is increased for flame spraying and degassing; 6) After the melt is sprayed with fire, it is allowed to stand still, and the alloy melt is cast into a preheated mold and cooled to obtain an alloy ingot; 7) The alloy ingot obtained in step 6) is isothermally heat treated and then rapidly cooled in water to obtain the target nickel-silicon brass.
2. The method for preparing the micro-nano dual-scale particle reinforced nickel-silicon brass according to claim 1, characterized in that: In the step 3), pure Ni, pure Fe, Cu-Mn master alloy, Cu-Si master alloy and pure Al are added in sequence when the melt temperature is 1200-1300° C.; after the materials are completely melted, they are kept at 1200-1300° C., and electromagnetic stirring is applied for 40-50 seconds to ensure that the alloy elements are evenly diffused in the alloy melt.
3. The method for preparing the micro-nano dual-scale particle reinforced nickel-silicon brass according to claim 1, characterized in that: In the step 4), the pure Zn block is wrapped with Cu foil and then pressed into the alloy melt, and the melt temperature is 1080-1130°C.
4. The method for preparing the micro-nano dual-scale particle reinforced nickel-silicon brass according to claim 1, characterized in that: In the step 5), the flame spraying degassing operation is as follows: the temperature of the alloy melt is increased twice to 1140-1150° C., and flame spraying degassing is performed.
5. The method for preparing the micro-nano dual-scale particle reinforced nickel-silicon brass according to claim 1, characterized in that: In the step 6), the standing time is 10 to 20 seconds, and the preheating mold is a cylindrical graphite mold preheated to 200 to 250°C.
6. The method for preparing the micro-nano dual-scale particle reinforced nickel-silicon brass according to claim 1, characterized in that: In the step 7), the isothermal heat treatment temperature is 830-870° C., and the isothermal heat treatment time is 0.5-1 h.
7. A micro-nano dual-scale particle reinforced nickel-silicon brass prepared by the method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Cu-Ni-Si alloy for electronic material
CN102822364A
Copper alloy matrix material and preparation method thereof
CN105018783A
Copper alloy formula for manufacturing bottle clamp
CN110863123A
Copper-nickel-silicon-aluminum alloy and preparation method thereof
CN112853149A
Preparation method of micro-nano dual-scale TiC particle reinforced aluminum matrix composite material
CN113416861A
Cited By
Cu-Zn-Ti-Si alloy synergistically strengthened by primary phase and hypoeutectic structure and preparation method for regulating components and cooling speed of Cu-Zn-Ti-Si alloy
CN121250175A
Cu-zn-ti-si alloy with primary phase and hypoeutectic structure synergistically reinforced and preparation method thereof with component and cooling speed regulation
CN121250175B