Method for promoting refining of TiC phase in Ni-based high-temperature alloy and inhibiting grain boundary segregation of Mo element through Y microalloying
By adding trace Y elements to nickel-based high-temperature alloys, the TiC phase refinement and suppressing Mo element segregation are solved, and the performance reduction caused by Mo element segregation in high-temperature alloys is significantly improved, and the tensile strength and elongation of the alloy are improved. Component uniformity and processing properties.
Patent Information
- Application Number
- CN202410568386.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-01
AI Technical Summary
During the solidification process of high-temperature alloys, refractory elements such as Mo elements often lead to element segregation between dendrites, forming large Mo-rich phases, reducing the service performance of the alloy. Subsequent heat treatment or plastic processing cannot completely eliminate this segregation, affecting The composition uniformity and processing properties of the alloy.
By adding trace Y elements to the nickel-based high-temperature alloy, the refinement of TiC phase and suppressing the grain boundary segregation of Mo elements, the Y element microalloy nickel-based high-temperature alloy is prepared by vacuum arc melting furnace and copper mold process to ensure the elemental Even distribution and organizational structure.
The room temperature tensile ultimate tensile strength and elongation of the alloy are significantly improved, the ultimate tensile strength is improved by 9.3%, the elongation is improved by 81.4%, and macrosegregation is reduced, which improves component uniformity and processing performance.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature alloy material preparation, and in particular to a method for promoting TiC phase refinement in a Ni-based high-temperature alloy and inhibiting Mo element grain boundary segregation. Background Art
[0002] According to the difference of its main alloying elements, high-temperature alloys can be divided into iron-based, cobalt-based and nickel-based high-temperature alloys. Compared with the other two alloys, nickel-based high-temperature alloys are the most commonly used, mainly because they have the following advantages: nickel-based alloys have higher high-temperature strength due to the solid solution strengthening effect of adding elements such as W, Mo, Nb, the precipitation strengthening effect of adding elements such as Al and Ti to form Ni3 (Al, Ti) phase (γ′ precipitation phase), and the grain boundary strengthening effect of adding elements such as C and B; the addition of antioxidant elements such as Cr and Al to nickel-based alloys can form a stable and dense oxide film with oxygen, which can effectively prevent further erosion of metal materials by oxygen and corrosive media, and improve the material's antioxidant and corrosion resistance; nickel-based alloys have a lower density and are suitable for some applications that require lightweight design; nickel-based alloys have excellent processing performance, and can be manufactured through casting, cold processing, hot processing and other processes. Complex parts and structures meet the needs of various complex applications. Therefore, nickel-based high-temperature alloys have a wide range of application value in the preparation of key hot end components such as combustion chambers, turbine blades, turbine disks, gas turbines, etc., and are the preferred material for the preparation of aircraft engines.
[0003] Cast high-temperature alloys are widely used in high-temperature alloys due to their simple manufacturing methods and low costs. During the solidification process of high-temperature alloys, due to the redistribution of solute elements, refractory elements such as Mo elements often undergo element segregation between dendrites to form coarse Mo-rich phases, resulting in reduced service performance of the alloy. In addition, this type of element segregation cannot be completely eliminated even in subsequent heat treatment or plastic processing methods. In the present invention, the addition of trace Y elements can improve the morphology of the TiC phase in the alloy, inhibit the segregation of the Mo element, improve the solidification uniformity of the high-temperature alloy, and play a positive role in eliminating or weakening macroscopic segregation and improving the composition uniformity of the alloy. It is also the best way to improve alloy processing and service performance. Summary of the invention
[0004] The purpose of the present invention is to propose a method for promoting TiC phase refinement and inhibiting Mo element grain boundary segregation in Ni-based high-temperature alloy by Y element microalloying according to the element system composition characteristics of Ni-based high-temperature alloy.
[0005] The technical solution provided by the present invention is as follows:
[0006] A Y element microalloyed nickel-based high-temperature alloy, the chemical composition and corresponding mass percentage content of which are: Mo: 7.6-9.0wt%, Cr: 14.5-16.5wt%, Co: 9.0-10.0wt%, Ti: 3.4-3.8wt%, Al: 3.9-4.4wt%, Fe: ≤0.5wt%, Nb: ≤0.25wt%, Hf: ≤0.25wt%, Si: ≤0.2wt%, W: ≤0.2wt%, S: ≤0.015wt%, P: ≤0.015wt%, Mn: ≤0.2wt%, C: 0.12-0.18wt%, B: 0.004-0.008wt%, Y: 0.05-0.1wt%, and the balance is Ni.
[0007] The Y-element microalloyed nickel-based high-temperature alloy provided by the above technical solution has a uniformly distributed organizational structure. Compared with the traditional K423 alloy, the ultimate tensile strength is increased by 9.3% and the elongation is increased by 81.4% under room temperature tensile test.
[0008] The present invention also provides a method for preparing the above-mentioned Y element alloyed nickel-based high-temperature alloy, comprising the following steps: mixing the ingredients according to the chemical composition and content of the above-mentioned Y element micro-alloyed nickel-based high-temperature alloy, smelting in a vacuum arc melting furnace, casting the ingot using a copper mold process, and using the cast material to obtain the Y element micro-alloyed nickel-based high-temperature alloy.
[0009] Specifically, a yttrium single substance block with a purity of 99.99% and a finished K423 alloy are used as raw materials, the surface of the raw materials is polished by a grinder and sandpaper to remove surface oxides, ultrasonic cleaning is performed in anhydrous alcohol, and vacuum drying is performed in a vacuum drying oven at a temperature of 40 to 60° C. for 1 to 2 hours before use.
[0010] Specifically, the required K423 alloy and yttrium single substance block are weighed according to the composition ratio, and the raw materials are configured; the configured raw materials are placed and smelted in an arrangement of K423 alloy at the bottom and yttrium at the top.
[0011] Specifically, when the metal is smelted, the vacuum is evacuated to a vacuum degree of 4×10 -3 Pa, fill with inert gas argon for purge, repeat purge 2 to 3 times, and then evacuate to a vacuum degree of 2.5×10 -3 Pa, fill with inert gas argon until the pressure in the furnace is -0.05~-0.1Mpa, and the smelting current is 200~250A during smelting.
[0012] Specifically, a vacuum arc furnace is used to melt copper mold casting to perform repeated melting, and the number of melting times is 6 to 8 times. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1This is an optical microscope photo of the grain structure of the alloy ingot in the comparative example of the present invention and Example 1-2.
[0014] Figure 2 The scanning electron microscope photos of the grain structure of the alloy ingot in the comparative example of the present invention and Example 1-2 are
[0015] Figure 3 This is a microstructure photo of the interdendritic crystals in Example 1 of the present invention.
[0016] Figure 4 This is a microstructure photo of the interdendritic crystals in Example 1 of the present invention.
[0017] Figure 5 This is a microstructure photo of the interdendritic crystals in the comparative example of the present invention. DETAILED DESCRIPTION
[0018] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0019] Example 1
[0020] Preparation of Nickel-Based Superalloy Containing Trace Y Element
[0021] The preparation method described in this example is: use yttrium single substance block with a purity of 99.99% and finished K423 alloy as raw materials, grind the surface of the raw materials with a grinder and sandpaper to remove surface oxides, and then ultrasonically clean them in anhydrous alcohol, and then vacuum dry them in a vacuum drying oven at 40°C for 2h for use. The ingredients are prepared according to the following mass percentages: 0.05wt% Y, and the remainder is K423 alloy. Use a vacuum arc melting furnace for smelting. First, put the single substance Y and K423 alloy into a water-cooled copper crucible in the furnace chamber, and first evacuate the vacuum to a vacuum degree of 4×10 -3 Pa, fill with argon gas for purge, repeat purge 3 times, and evacuate to a vacuum degree of 2.5×10 -3 Pa, then fill with argon to -0.05Mpa for alloy melting, the arc starting current is 60A, the melting current is 200A, after the melting is completed, the ingot is turned over after rapid water cooling, and after repeated melting 8 times, a nickel-based high-temperature alloy ingot is obtained in a water-cooled copper crucible.
[0022] The prepared experiment was subjected to a room temperature tensile test (using a WDT-5 universal testing machine to perform a room temperature tensile test). The ultimate tensile strength of the sample of Example 1 of the present invention was 1160.5 MPa, and the elongation was 13.0%.
[0023] Example 2
[0024] Preparation of Nickel-Based Superalloy Containing Trace Y Element
[0025] The preparation method described in this example is: use yttrium single substance block with a purity of 99.99% and finished K423 alloy as raw materials, grind the surface of the raw materials with a grinder and sandpaper to remove surface oxides, and ultrasonically clean them in anhydrous alcohol, and then vacuum dry them in a vacuum drying oven at 40°C for 2 hours for use. The ingredients are prepared according to the following mass percentages: 0.1wt% Y, and the remainder is K423 alloy. Use a vacuum arc melting furnace for smelting. First, put the single substance Y and K423 alloy into a water-cooled copper crucible in the furnace chamber, and first evacuate the vacuum to a vacuum degree of 4×10 -3 Pa, fill with argon gas for purge, repeat purge 3 times, and evacuate to a vacuum degree of 2.5×10 -3 Pa, then fill with argon to -0.05Mpa for alloy melting, the arc starting current is 60A, the melting current is 200A, after the melting is completed, the ingot is turned over after rapid water cooling, and after repeated melting 8 times, a nickel-based high-temperature alloy ingot is obtained in a water-cooled copper crucible.
[0026] The prepared samples were subjected to a room temperature tensile test (using a WDT-5 universal testing machine for room temperature tensile test). The ultimate tensile strength of the sample in Example 1 of the present invention was 1134.8 MPa, and the elongation was 9.7%.
[0027] Comparative Example
[0028] Remelting preparation of K423 alloy without Y element
[0029] The finished K423 alloy was selected as the raw material. The surface of the raw material was polished by a grinder to remove the surface oxide, and then ultrasonically cleaned in anhydrous alcohol, and then vacuum dried in a vacuum drying oven at 60°C for 2 h. The K423 alloy was first placed in a water-cooled copper crucible in the furnace chamber and vacuumed to a vacuum degree of 4×10 -3 Pa, fill with argon gas for purge, repeat purge 3 times, and evacuate to a vacuum degree of 2.5×10 -3 Pa, argon is filled to -0.05Mpa for alloy melting, the arc starting current is 60A, the melting current is 250A, and after the melting is completed, the ingot is turned over after rapid water cooling. After repeated melting for 6 times, a nickel-based high-temperature alloy ingot is obtained in a water-cooled copper crucible.
[0030] The prepared samples were subjected to a room temperature tensile test (using a WDT-5 universal testing machine to perform a room temperature tensile test). The ultimate tensile strength of the comparative example sample of the present invention was 1061.3 MPa, and the elongation was 7.2%.
[0031] The alloy ingots prepared in Examples 1-2 and the comparative example were subjected to tissue analysis and observation, specifically: a small sample of 5×5×2mm was cut from the alloy ingot by an electric spark wire cutting machine, the surface oxide scale was cleaned with sandpaper, and the sample surface was cleaned with water, and then mounted with a sample mounting machine to facilitate subsequent grinding and observation. The prepared metallographic sample was ground with #600-2000SiC sandpaper, and then mechanically polished with polishing pastes of particle sizes of 2.5μm and 0.5μm respectively. After the sample was ground and polished, it was placed in anhydrous ethanol for ultrasonic cleaning to remove the polishing paste powder remaining on the surface. The polished sample was chemically corroded with CuCl2, and the corrosive agent used was 5g CuCl2+100ml HCl+100ml C2H5OH, and the corrosion time was 30s. The metallographic structure of the corroded samples was observed using a metallographic microscope. The field emission scanning electron microscope used the secondary electron mode and backscattering mode to observe the microstructure and phase distribution, and the chemical composition of different phases was determined by the energy dispersive spectrometer attached to the scanning electron microscope.
[0032] By observation Figure 2 It can be seen that the average diameter of TiC in the comparative example is 12.4 μm, the average diameter of TiC in Example 1 is 5.4 μm, and the average diameter of TiC in Example 2 is 4.2 μm. Figure 2 As can be seen from (a), (b) and (c), the TiC content in Example 1-2 is also significantly reduced, which has the effect of refining the TiC primary phase.
[0033] By comparison Figures 3 to 5 It can be seen that the size and content of the interdendritic molybdenum-rich phase in Example 1-2 are significantly reduced, which has the effect of reducing element segregation.
[0034] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A Y-element microalloyed nickel-based high-temperature alloy, characterized in that: Its chemical composition and corresponding mass percentage content are: Mo: 7.6-9.0wt%, Cr: 14.5-16.5wt%, Co: 9.0-10.0wt%, Ti: 3.4-3.8wt%, Al: 3.9-4.4wt%, Fe: ≤0.5wt%, Nb: ≤0.25wt%, Hf: ≤0.25wt%, Si: ≤0.2wt%, W: ≤0.2wt%, S: ≤0.015wt%, P: ≤0.015wt%, Mn: ≤0.2wt%, C: 0.12-0.18wt%, B: 0.004-0.008wt%, Y: 0.05-0.1wt%, and the balance is Ni.
2. A method for preparing a Y-element microalloyed nickel-based high-temperature alloy according to claim 1, characterized in that: The following steps are involved: According to the chemical composition and content of the Y element microalloyed nickel-based high-temperature alloy, the alloy is smelted in a vacuum arc melting furnace, cast ingots are cast using a copper mold process, and the Y element microalloyed nickel-based high-temperature alloy is obtained by directly using the cast material.
3. The method for preparing the Y-element microalloyed nickel-based high-temperature alloy according to claim 2, characterized in that: Yttrium blocks with a purity of 99.99% and finished K423 alloy are used as raw materials. The surfaces of the raw materials are polished with a grinder and sandpaper to remove surface oxides. The raw materials are ultrasonically cleaned in anhydrous alcohol and vacuum dried in a vacuum drying oven at 40 to 60° C. for 1 to 2 hours before use.
4. The method for preparing the Y-element microalloyed nickel-based high-temperature alloy according to claim 2, characterized in that: The required K423 alloy and yttrium single substance block are weighed according to the composition ratio to prepare the raw materials; the prepared raw materials are placed and smelted in an arrangement of K423 alloy at the bottom and yttrium at the top.
5. The method for preparing the Y-element microalloyed nickel-based high-temperature alloy according to claim 2, characterized in that: When metal is smelted, vacuum is drawn to a vacuum degree of 4×10 -3 Pa, fill with inert gas argon for purge, repeat purge 2 to 3 times, and then evacuate to a vacuum degree of 2.5×10 -3 Pa, fill with inert gas argon until the pressure in the furnace is -0.05~-0.1Mpa, and the smelting current is 200~250A during smelting.
6. The method for preparing the Y-element microalloyed nickel-based high-temperature alloy according to any one of claims 2 to 5, characterized in that: The process of vacuum arc furnace melting and copper mold casting is adopted for repeated melting, and the number of melting times is 6 to 8 times.