Low-alloy high-strength cast steel bucket tooth and preparation method thereof

By using low alloy high-strength cast steel in excavator bucket teeth, combined with cheap elements and heat treatment technology, the problems of hardness, wear resistance and cost in the prior art are solved, and the mechanical performance and service life are significantly improved.

CN118880182APending Publication Date: 2024-11-01ZHENGZHOU COAL MASCH GREEN MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411372005.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing excavator bucket teeth materials are mainly high manganese steel and low-carbon martensitic steel, which have problems such as low hardness, poor strength and wear resistance, high production costs and short service life. Foreign low-carbon martensitic steel It contains expensive copper, nickel and other elements, resulting in less significant improvement in mechanical properties.

Method used

Low alloy high-strength cast steel is used to replace expensive elements by using cheap silicon and manganese elements, and adding ferrochrome, ferrosilicon, trace B, Sn and Ti, to obtain excellent tempered martensite structure through heat treatment process, and improve the bucket The strength, hardness and tensile strength of the teeth.

Benefits of technology

It achieves low production costs and significantly improves the mechanical properties of the bucket teeth, and has a service life of 2 to 3 times higher than traditional technology, and maintains mechanical properties in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880182A_ABST
    Figure CN118880182A_ABST
Patent Text Reader

Abstract

The invention discloses a low-alloy high-strength cast steel bucket tooth and a preparation method thereof, and belongs to the technical field of bucket tooth cast steel. The cast steel bucket tooth comprises the following chemical components in percentage by weight: 0.19%-0.23% of C, 0.30%-0.60% of Si, 0.70%-1.00% of Mn, 0.90%-1.20% of Cr, 0.40%-0.50% of Mo, 0.03%-0.05% of Ti, less than 0.080% of B, less than 0.007% of Sn, 0.03%-0.08% of RE, less than or equal to 0.010% of P, less than or equal to 0.007% of S and the balance of Fe and inevitable impurities. The preparation method comprises the following steps: smelting according to the chemical component proportion, casting into a bucket tooth casting, and carrying out heat treatment including normalizing, quenching and low-temperature tempering to obtain the bucket tooth. According to the preparation method, the actual production cost is combined, the content of precious metal is reduced, and the raw material cost is reduced to the maximum extent; in actual use, the steel plate has high strength, high hardness and high tensile strength, and the service life of the steel plate is prolonged by 2-3 times compared with that of a traditional technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bucket tooth cast steel, and in particular to a low-alloy high-strength cast steel bucket tooth and a preparation method thereof. Background Art

[0002] Excavators are widely used in mining machinery, civil engineering, water conservancy projects and municipal engineering, among which bucket teeth are key vulnerable parts on excavators. In recent years, with the rapid development of mining machinery and water conservancy projects, the use of excavators has also increased day by day, and the consumption of bucket teeth has increased rapidly. A large-scale water conservancy project or a medium-sized mine generally uses more than ten excavators at the same time, and the annual consumption of bucket teeth is as high as hundreds of tons, with a value of more than one million yuan. Bucket teeth are in direct contact with materials such as ore, rock, soil or sand and gravel. When they first come into contact with the materials, the rapid movement of the materials causes the bucket teeth to be subjected to a strong impact, and they must withstand a certain bending moment during the process of loading the materials.

[0003] At present, domestic bucket teeth of various excavators used in the market are mainly made of high manganese steel, which generally has defects such as low hardness, poor toughness and wear resistance, and short service life; while foreign bucket teeth are mainly made of low-carbon martensitic steel, most of which contain expensive alloy elements such as copper and nickel, requiring complex heat treatment, high energy consumption, long production cycle, high production cost, and also have disadvantages such as poor toughness and easy breakage during use.

[0004] CN202311205188.9 discloses a wear-resistant steel with high hardness and excellent impact toughness and a preparation method thereof. The preparation method includes repeated temperature control during smelting, casting, normalizing, isothermal quenching and tempering. The chemical composition and mass percentage of the obtained wear-resistant steel are C: 0.25-0.42%, Si: 1.0-2.0%, Mn: 0.8-1.5%, Cr: 1.2-1.6%, Ni: 0.5-1.0%, Mo: 0.3-0.5%, Cu: 0.4-0.7%, RE: 0.03-0.08%, P≤0.032%, S≤0.040%, and the balance is Fe and unavoidable impurities; and (Mn+Ni+Cu)≥2.0%. In this method, by optimizing the alloy component content and rationally designing the isothermal quenching process below the Ms point, the martensite + metastable austenite steel can maintain high hardness while still having excellent toughness, overcoming the shortcomings of traditional technology. With both high hardness and excellent impact toughness, the martensitic wear-resistant steel exhibits better wear resistance under high stress than traditional water-quenched martensitic steel and isothermal quenched bainitic steel. However, the wear-resistant steel still uses expensive elements such as nickel and copper, resulting in excessively high production costs, and the mechanical properties of the obtained wear-resistant steel are not significantly improved.

[0005] To this end, the present invention is specially proposed to solve the above-mentioned technical problems. Summary of the invention

[0006] The purpose of the present invention is to provide a low-alloy high-strength cast steel bucket tooth and a preparation method thereof, which has a lower production cost in practical applications by using cheap silicon and manganese elements instead of expensive elements such as nickel and copper; at the same time, by adding ferrochrome, ferrosilicon and trace amounts of B, Sn, and Ti, the ratio of each element is reasonably adjusted to improve the heat treatment performance of the material; through the heat treatment process, an excellent tempered martensite structure is finally obtained, and the strength, hardness, tensile strength and other mechanical properties of the bucket tooth are improved.

[0007] In order to achieve the above-mentioned object, the present invention provides a low-alloy high-strength cast steel bucket tooth, which contains, by weight percentage: C: 0.19%-0.23%, Si: 0.30-0.60%, Mn: 0.70%-1.00%, Cr: 0.90%-1.20%, Mo: 0.40%-0.50%, Ti: 0.03%-0.05%, B < 0.080%, Sn < 0.007%, RE: 0.03%-0.08%, P ≤ 0.010%, S ≤ 0.007%, and the balance is Fe and unavoidable impurities.

[0008] Preferably, the low alloy high strength cast steel bucket tooth contains, by weight percentage, the following: C: 0.20% to 0.21%, Si 0.40%, Mn 0.85%, Cr 0.95%, Mo 0.45%, Ti 0.04%, B < 0.079%, Sn < 0.007%, RE: 0.03% to 0.08%, P ≤ 0.010%, S ≤ 0.007%, and the remainder is Fe and unavoidable impurities.

[0009] Preferably, in the low alloy high strength cast steel bucket tooth, the percentage content of S element S≤0.005%, and the percentage content of P element P≤0.007%.

[0010] The main functions and effects of the chemical elements in the low-alloy high-strength cast steel bucket teeth of the present invention are as follows: C: Carbon is the element that contributes most to the strength of steel and also the element that affects plasticity the most. If the carbon content is too high, the martensite structure after quenching is easy to grow and the structure is relatively coarse, which will cause the material to brittlely fracture when the bucket tooth is subjected to a large impact force. Therefore, the low-alloy high-strength cast steel bucket tooth of the present invention adopts a lower carbon content to achieve better wear resistance. Specifically, the carbon content is selected in the range of 0.19% to 0.23%. Preferably, the carbon content is selected in the range of 0.20% to 0.21%.

[0011] Si: Most of the silicon element is dissolved in ferrite, which can cause solid solution strengthening of ferrite and improve the hardness and strength of low alloy steel. Its effect is second only to P. Si is an element that reduces the austenite phase region and can be dissolved in Fe3C, causing carbide instability, hindering the precipitation and aggregation of cementite, thereby improving the hardenability of low alloy steel. Therefore, the silicon content of the low alloy high strength cast steel bucket tooth of the present invention is selected in the range of 0.30% to 0.60%. Preferably, the silicon content is selected to be 0.40%.

[0012] Mn: Adding manganese to steel can promote grain boundary refinement and optimize the location and number of grain boundaries. This helps to increase the toughness and ductility of cast steel and prevent cracks and fractures. Therefore, the manganese content of the low-alloy high-strength cast steel bucket tooth of the present invention is selected in the range of 0.70% to 1.00%. Preferably, the manganese content is selected to be 0.85%.

[0013] Cr: Chromium is one of the main alloying elements of wear-resistant low alloy steel. In the cast state, as the Cr content increases, the hardness increases and the impact toughness decreases. After the normalizing + quenching + tempering heat treatment process, due to the effect of Cr, the amount of residual austenite in the matrix structure increases, but with Mn and Si, the hardenability and toughness can be greatly improved. Therefore, the chromium content of the low-alloy high-strength cast steel bucket tooth of the present invention is selected in the range of 0.90% to 1.20%. Preferably, the chromium content is selected to be 0.95%.

[0014] Ti: Titanium can interact with C in steel to produce granular titanium carbides. This titanium carbide is evenly distributed and can refine the grain size of cast steel, increase the displacement resistance of grain boundaries, and achieve the effect of improving the strength and toughness of steel. At the same time, titanium can react with sulfur to form titanium sulfide (TiS) inclusions. These titanium sulfide inclusions are easy to float during the cooling of molten steel and can be removed through subsequent refining processes, thereby reducing the sulfur content in steel. The addition of titanium can alleviate the segregation of manganese, thereby improving the uniformity and comprehensive performance of steel. Therefore, the titanium content of the low-alloy high-strength cast steel bucket tooth of the present invention is selected in the range of 0.03% to 0.05%. Preferably, the titanium content is selected to be 0.04%.

[0015] Mo: Mo has a solid solution strengthening effect on ferrite. It can be dissolved in ferrite, austenite and carbide in low alloy steel, and can also improve the hardenability of low alloy steel. When it coexists with Cr, it can reduce or inhibit the temper brittleness caused by other elements. However, Mo is a precious metal, and its excessive content will lead to an increase in production costs. Therefore, the molybdenum content of the low alloy high strength cast steel bucket tooth of the present invention is selected in the range of 0.40% to 0.50%. Preferably, the molybdenum content is selected to be 0.45%.

[0016] B: Adding an appropriate amount of boron to steel can improve the adverse effect of cast steel cracking. In addition, adding an appropriate amount of boron can form a boron passivation layer with high hardness, high toughness and high corrosion resistance, which can significantly improve the corrosion resistance of steel. Therefore, the boron content of the low-alloy high-strength cast steel bucket tooth of the present invention is selected in the range of B < 0.080%. Preferably, the boron content is selected as B < 0.079%.

[0017] Sn: The addition of tin can further achieve the purpose of maintaining the mechanical properties of cast steel bucket teeth for a long time even in a humid environment. Tin can form a protective film on the surface of cast steel, which can resist the erosion of the external environment and improve the corrosion resistance of cast steel. This is especially important when bucket teeth are used in harsh environmental conditions. In addition, tin can play a certain role in grain refinement in steel. Fine grains can effectively hinder the movement of dislocations, thereby improving the strength and hardness of the material, and also enhancing its wear resistance. Therefore, the selection range of tin content of the low-alloy high-strength cast steel bucket teeth of the present invention is Sn<0.007%.

[0018] S and P: Both are harmful elements, which are easy to form grain boundary inclusions in low alloy steel, increase the brittleness of low alloy steel, and increase the cracking tendency during heat treatment. Therefore, their content should be controlled as low as possible. Therefore, the sulfur content of the low alloy high strength cast steel bucket tooth of the present invention is selected in the range of S≤0.007%; the phosphorus content is selected in the range of P≤0.010%. Preferably, the percentage content of S element S≤0.005% and the percentage content of P element P≤0.007% of the low alloy high strength cast steel bucket tooth prepared by the present invention.

[0019] RE: Rare earth elements can react with impurities such as sulfur and oxygen in steel to generate stable sulfides or oxides, thereby reducing the harmful effects of impurities in steel and reducing grain boundary embrittlement. Rare earth elements can refine grains, make the grain structure of steel more uniform, and help improve the mechanical properties and wear resistance of steel. In addition, rare earth elements can improve the high-temperature oxidation resistance of steel, especially in wear-resistant steel used in high-temperature environments, rare earth elements help to extend the service life of the material. Therefore, the rare earth element content of the low-alloy high-strength cast steel bucket tooth of the present invention is selected in the range of 0.03% to 0.08%.

[0020] The present invention also provides a method for preparing a low-alloy high-strength cast steel bucket tooth, comprising a smelting casting and a heat treatment process, specifically comprising the following steps: S1: Melting and Casting Melting and pouring into bucket tooth castings according to chemical composition ratio; S2: Heat treatment process of bucket tooth castings The bucket tooth casting is heated to 880-900°C and kept warm, and then air-cooled for normalizing; after normalizing, it is heated to 910-930°C and quenched by cooling with a water-soluble quenching liquid; after quenching, it is heated to 200-260°C and kept warm, and then cooled with air to obtain a low-alloy high-strength cast steel bucket tooth.

[0021] Preferably, the holding time of the normalizing is 0.5 to 1 h, and the holding time of the tempering is 2 to 3 h.

[0022] Preferably, the tempering temperature in step S2 is 230°C.

[0023] Preferably, step S1 specifically includes: S101 smelting: melt the raw material of cast steel in an electric furnace, and control the chemical composition by weight percentage to C: 0.19% ~ 0.23%, Si: 0.30 ~ 0.60%, Mn: 0.70% ~ 1.00%, Cr: 0.90% ~ 1.20%, Ti: 0.03% ~ 0.05%, Mo: 0.40% ~ 0.50%, P ≤ 0.010%, S ≤ 0.007%, the rest is Fe and unavoidable impurities; when the temperature of molten steel rises to 1550 ~ 1570 ℃, add 0.30% silicon block for deoxidation; S102 molten steel treatment: before tapping, crush the titanium, tin, and boron iron alloy into small pieces with a particle size of 5 to 8 mm and add them into the molten steel, and control the chemical composition by weight percentage to C: 0.19% to 0.23%, Si: 0.30 to 0.60%, Mn: 0.70% to 1.00%, Cr: 0.90% to 1.20%, Ti: 0.03% to 0.05%, Mo: 0.40% to 0.50%, P≤0.010%, S≤0.007%, B<0.080%, Sn<0.007%, RE: 0.03% to 0.08%, and the rest is Fe and unavoidable impurities; let the treated molten steel stand after slagging, wherein the molten steel temperature is 1530 to 1550℃; after alloying in the electric furnace, heat it up, and when the molten steel temperature reaches 1630 to 1640℃, tap it into the ladle; S103 casting and molding: the molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550~1570℃; S104 Insulation and Sand Dropping: After casting, the sand mold is kept warm and then the sand is dropped out of the box.

[0024] Preferably, in step S101, the raw material for casting steel is pig iron, scrap iron, etc.

[0025] Preferably, in step S102, the molten steel is left to stand for 1 to 2 hours after slagging.

[0026] Preferably, in step S102, the titanium, tin and boron-containing ferroalloy is crushed into small pieces with a particle size of 5 to 8 mm and added to the molten steel, and the chemical composition is further controlled by weight percentage to C: 0.20% to 0.21%, Si 0.40%, Mn 0.85%, Cr0.95%, Mo 0.45%, Ti 0.04%, B < 0.079%, Sn < 0.007%, RE: 0.03% to 0.08%, S ≤ 0.005%, P ≤ 0.007%, and the remainder of Fe and unavoidable impurities.

[0027] Preferably, in step S103, the principle of pouring the casting quickly and pouring the riser slowly is followed during pouring, and the pouring speed is well controlled to ensure the molding quality of the casting.

[0028] Preferably, in step S104, the insulation time is 24 to 72 hours.

[0029] Preferably, in step S104, when the following conditions are met, the unpacking and sanding operation is performed: when the residual heat temperature of the casting measured during unpacking is between 350 and 450°C, the sanding process is switched to sanding, and the residual heat is used to cut the pouring spout. The residual heat temperature must not be lower than 200°C. When it is lower than 200°C, the pouring spout can be cut only after heating in the furnace.

[0030] Preferably, the preparation method further includes welding repair, shot peening and polishing to eliminate surface defects of the alloy steel and further increase the service life of the bucket tooth plate.

[0031] The heat treatment principle and effect of the present invention: After casting, the low-alloy high-strength cast steel bucket teeth of the present invention not only have large casting stress, but also have defects such as coarse grains and component segregation; the microstructure after normalizing is pearlite and ferrite, resulting in poor plasticity and toughness of the casting. Therefore, in order to improve the microstructure, a quenching process is further used to improve the mechanical properties; quenching at 910-930°C can obtain more uniform and fine austenite grains, and the tensile strength and hardness are improved, meeting the requirements for improving the performance of the bucket teeth. Finally, low-temperature tempering is used to obtain a tempered martensitic structure, which timely eliminates or partially eliminates the internal stress generated during quenching, so that the mechanical properties of the bucket teeth are not only hard and wear-resistant, high in strength, but also have high fatigue resistance, and the shaping and toughness of the bucket teeth are also better.

[0032] The present invention has the following beneficial effects: (1) The main alloying elements of the low-alloy high-strength cast steel bucket teeth of the present invention are cheap silicon and manganese elements, and do not contain expensive elements such as nickel and copper, which has a low production cost in practical applications. By adding ferrochrome, ferrosilicon and trace amounts of B, Sn, and Ti, and by rationally adjusting the ratio of each element, the heat treatment performance of the material is improved; through the heat treatment process, an excellent tempered martensite structure is obtained, and the strength, hardness, tensile strength and other mechanical properties of the bucket teeth are improved.

[0033] (2) The present invention adopts a normalizing-quenching-tempering heat treatment process, and normalizes at a temperature in the range of 880 to 900°C to eliminate casting stress and component segregation defects of the casting, and quenches at a temperature in the range of 910 to 930°C to obtain relatively uniform and fine austenite grains. Under low-temperature tempering conditions of 200 to 260°C (for example, 230°C), a tempered martensite structure is finally obtained, thereby timely eliminating or partially eliminating the internal stress generated during quenching. The bucket tooth has a uniform and good microstructure, high purity, fine grains and a dense structure, so that the bucket tooth has mechanical properties that are not only hard and wear-resistant, but also have high strength and fatigue resistance. The bucket tooth also has better shaping and toughness, thereby increasing the service life in daily life by 2 to 3 times compared with the traditional technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The present invention provides a low alloy high strength cast steel bucket tooth as-cast metallographic structure; Figure 2 The present invention discloses a heat-treated metallographic structure of a low-alloy high-strength cast steel bucket tooth. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0036] Example 1 A low alloy high strength cast steel bucket tooth and a method for manufacturing the same in this embodiment include the following steps: S1: Melting and Casting S101 smelting: melt cast steel raw materials such as pig iron and scrap iron in an electric furnace, control the chemical composition of cast steel by weight percentage to C: 0.19%, Si: 0.30%, Mn: 0.70%, Cr: 0.90%, Ti: 0.03%, Mo: 0.40%, P≤0.010%, S≤0.007%, the rest of Fe and unavoidable impurities, add 0.30% silicon block for deoxidation when the temperature of molten steel rises to 1550-1570℃; S102 molten steel treatment: before tapping, the titanium, tin, and boron-iron alloy is crushed into small pieces with a particle size of 5 to 8 mm, and the chemical composition in the cast steel is further controlled by weight percentage to C: 0.19%, Si: 0.30%, Mn: 0.70%, Cr: 0.90%, Ti: 0.03%, Mo: 0.40%, B < 0.080%, Sn < 0.007%, RE: 0.03%, P ≤ 0.010%, S ≤ 0.007%, and the balance is Fe and unavoidable impurities; the treated molten steel is allowed to stand for 60 minutes after slagging, wherein the molten steel temperature is 1530 to 1550°C; after alloying in the electric furnace, the temperature is raised, and the molten steel is tapped into the ladle when the temperature reaches 1630 to 1640°C; S103 pouring and molding: The molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550-1570℃. During pouring, the principle of pouring the casting quickly and pouring the riser slowly is followed, and the pouring speed is controlled to ensure the molding quality of the casting; S104 Insulation and Sand Dropping: After the casting is poured, the sand mold is kept warm for 24 hours, and then the sand is dropped out. When the residual heat temperature of the casting is 350-450℃, the sand is dropped out and the pouring head is cut by using the residual heat. The residual heat temperature shall not be lower than 200℃. If it is lower than 200℃, the pouring head can be cut only after heating in the furnace.

[0037] S2: The bucket tooth casting is heated to 880-900°C and kept at this temperature for 0.5-1 h, and then air-cooled for normalizing; after normalizing, it is heated to 910-930°C, and quenched by cooling with a water-soluble quenching liquid; after quenching, it is heated to 200-260°C and kept at this temperature for 2-3 h, and then air-cooled to obtain a low-alloy high-strength cast steel bucket tooth.

[0038] S3: The low-alloy high-strength cast steel bucket teeth of step S2 are subjected to welding repair, shot peening and polishing treatment to obtain low-alloy high-strength cast steel bucket teeth without surface defects.

[0039] Example 2 A low alloy high strength cast steel bucket tooth and a method for manufacturing the same in this embodiment include the following steps: S1: Melting and Casting S101 smelting: melt cast steel raw materials such as pig iron and scrap iron in an electric furnace, control the chemical composition of cast steel by weight percentage to C: 0.19%, Si: 0.30%, Mn: 0.70%, Cr: 0.90%, Ti: 0.03%, Mo: 0.40%, P≤0.010%, S≤0.007%, the rest of Fe and unavoidable impurities, add 0.30% silicon block for deoxidation when the temperature of molten steel rises to 1550-1570℃; S102 molten steel treatment: before tapping, the titanium, tin, and boron-iron alloy is crushed into small pieces with a particle size of 5 to 8 mm, and the chemical composition in the cast steel is further controlled by weight percentage to C: 0.20%, Si: 0.40%, Mn: 0.85%, Cr: 0.95%, Ti: 0.04%, Mo: 0.45%, B < 0.079%, Sn < 0.007%, RE: 0.03%, P ≤ 0.007%, S ≤ 0.005%, and the remaining Fe and unavoidable impurities; the treated molten steel is allowed to stand for 60 minutes after slagging, wherein the molten steel temperature is 1530 to 1550°C; after alloying in the electric furnace, the temperature is raised, and the molten steel is tapped into the ladle when the temperature reaches 1630 to 1640°C; S103 pouring and molding: The molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550-1570℃. During pouring, the principle of pouring the casting quickly and pouring the riser slowly is followed, and the pouring speed is controlled to ensure the molding quality of the casting; S104 Insulation and Sand Dropping: After the casting is poured, the sand mold is kept warm for 24 hours, and then the sand is dropped out. When the residual heat temperature of the casting is 350-450℃, the sand is dropped out and the pouring head is cut by using the residual heat. The residual heat temperature shall not be lower than 200℃. If it is lower than 200℃, the pouring head can be cut only after heating in the furnace.

[0040] S2: The bucket tooth casting is heated to 880-900°C and kept at this temperature for 0.5-1 h, and then air-cooled for normalizing; after normalizing, it is heated to 910-930°C, and quenched by cooling with a water-soluble quenching liquid; after quenching, it is heated to 200-260°C and kept at this temperature for 2-3 h, and then air-cooled to obtain a low-alloy high-strength cast steel bucket tooth.

[0041] S3: The low-alloy high-strength cast steel bucket teeth of step S2 are subjected to welding repair, shot peening and polishing treatment to obtain low-alloy high-strength cast steel bucket teeth without surface defects.

[0042] Example 3 A low alloy high strength cast steel bucket tooth and a method for manufacturing the same in this embodiment include the following steps: S1: Melting and Casting S101 smelting: melt cast steel raw materials such as pig iron and scrap iron in an electric furnace, control the chemical composition of cast steel by weight percentage to C: 0.23%, Si: 0.60%, Mn: 1.00%, Cr: 1.20%, Ti: 0.05%, Mo: 0.50%, P≤0.010%, S≤0.007%, the rest of Fe and unavoidable impurities, add 0.30% silicon block for deoxidation when the temperature of molten steel rises to 1550-1570℃; S102 molten steel treatment: before tapping, the titanium, tin, and boron-iron alloy is crushed into small pieces with a particle size of 5 to 8 mm, and the chemical composition in the cast steel is further controlled by weight percentage to C: 0.23%, Si: 0.60%, Mn: 1.00%, Cr: 1.20%, Ti: 0.05%, Mo: 0.50%, B < 0.080%, Sn < 0.007%, RE: 0.08%, P ≤ 0.010%, S ≤ 0.007%, and the remaining Fe and unavoidable impurities; the treated molten steel is allowed to stand for 60 minutes after slagging, wherein the molten steel temperature is 1530 to 1550°C; after alloying in the electric furnace, the temperature is raised, and the molten steel is tapped into the ladle when the temperature reaches 1630 to 1640°C; S103 pouring and molding: The molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550-1570℃. During pouring, the principle of pouring the casting quickly and pouring the riser slowly is followed, and the pouring speed is controlled to ensure the molding quality of the casting; S104 Insulation and Sand Dropping: After the casting is poured, the sand mold is kept warm for 24 hours, and then the sand is dropped out. When the residual heat temperature of the casting is 350-450℃, the sand is dropped out and the pouring head is cut by using the residual heat. The residual heat temperature shall not be lower than 200℃. If it is lower than 200℃, the pouring head can be cut only after heating in the furnace.

[0043] S2: The bucket tooth casting is heated to 880-900°C and kept at this temperature for 0.5-1 h, and then air-cooled for normalizing; after normalizing, it is heated to 910-930°C, and quenched by cooling with a water-soluble quenching liquid; after quenching, it is heated to 200-260°C and kept at this temperature for 2-3 h, and then air-cooled to obtain a low-alloy high-strength cast steel bucket tooth.

[0044] S3: The low-alloy high-strength cast steel bucket teeth of step S2 are subjected to welding repair, shot peening and polishing treatment to obtain low-alloy high-strength cast steel bucket teeth without surface defects.

[0045] Example 4 A low alloy high strength cast steel bucket tooth and a method for manufacturing the same in this embodiment include the following steps: S1: Melting and Casting S101 smelting: melt cast steel raw materials such as pig iron and scrap iron in an electric furnace, control the chemical composition of cast steel by weight percentage to C: 0.23%, Si: 0.60%, Mn: 1.00%, Cr: 1.20%, Ti: 0.05%, Mo: 0.40%, P≤0.010%, S≤0.007%, the rest of Fe and unavoidable impurities, add 0.30% silicon block for deoxidation when the temperature of molten steel rises to 1550-1570℃; S102 molten steel treatment: before tapping, the titanium, tin, and boron-iron alloy is crushed into small pieces with a particle size of 5 to 8 mm, and the chemical composition in the cast steel is further controlled by weight percentage to C: 0.21%, Si: 0.40%, Mn: 0.85%, Cr: 0.95%, Ti: 0.04%, Mo: 0.45%, B < 0.079%, Sn < 0.007%, RE: 0.08%, P ≤ 0.007%, S ≤ 0.005%, and the remaining Fe and unavoidable impurities; the treated molten steel is allowed to stand for 60 minutes after slagging, wherein the molten steel temperature is 1530 to 1550°C; after alloying in the electric furnace, the temperature is raised, and the molten steel is tapped into the ladle when the temperature reaches 1630 to 1640°C; S103 pouring and molding: The molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550-1570℃. During pouring, the principle of pouring the casting quickly and pouring the riser slowly is followed, and the pouring speed is controlled to ensure the molding quality of the casting; S104 Insulation and Sand Dropping: After the casting is poured, the sand mold is kept warm for 24 hours, and then the sand is dropped out. When the residual heat temperature of the casting is 350-450℃, the sand is dropped out and the pouring head is cut by using the residual heat. The residual heat temperature shall not be lower than 200℃. If it is lower than 200℃, the pouring head can be cut only after heating in the furnace.

[0046] S2: The bucket tooth casting is heated to 880-900°C and kept at this temperature for 0.5-1 h, and then air-cooled for normalizing; after normalizing, it is heated to 910-930°C, and quenched by cooling with a water-soluble quenching liquid; after quenching, it is heated to 200-260°C and kept at this temperature for 2-3 h, and then air-cooled to obtain a low-alloy high-strength cast steel bucket tooth.

[0047] S3: The low-alloy high-strength cast steel bucket teeth of step S2 are subjected to welding repair, shot peening and polishing treatment to obtain low-alloy high-strength cast steel bucket teeth without surface defects.

[0048] Example 5 A low alloy high strength cast steel bucket tooth and a method for manufacturing the same in this embodiment include the following steps: S1: Melting and Casting S101 smelting: melt cast steel raw materials such as pig iron and scrap iron in an electric furnace, control the chemical composition of cast steel by weight percentage to C: 0.21%, Si: 0.45%, Mn: 0.85%, Cr: 1.00%, Ti: 0.04%, Mo: 0.45%, P≤0.010%, S≤0.007%, the rest of Fe and unavoidable impurities, add 0.30% silicon block for deoxidation when the temperature of molten steel rises to 1550-1570℃; S102 molten steel treatment: before tapping, the titanium, tin, and boron-iron alloy is crushed into small pieces with a particle size of 5 to 8 mm, and the chemical composition in the cast steel is further controlled by weight percentage to C: 0.21%, Si: 0.45%, Mn: 0.85%, Cr: 1.00%, Ti: 0.04%, Mo: 0.45%, B < 0.080%, Sn < 0.007%, RE: 0.05%, P ≤ 0.010%, S ≤ 0.007%, and the balance is Fe and unavoidable impurities; the treated molten steel is allowed to stand for 60 minutes after slagging, wherein the molten steel temperature is 1530 to 1550°C; after alloying in the electric furnace, the temperature is raised, and the molten steel is tapped into the ladle when the temperature reaches 1630 to 1640°C; S103 pouring and molding: The molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550-1570℃. During pouring, the principle of pouring the casting quickly and pouring the riser slowly is followed, and the pouring speed is controlled to ensure the molding quality of the casting; S104 Insulation and Sand Dropping: After the casting is poured, the sand mold is kept warm for 24 hours, and then the sand is dropped out. When the residual heat temperature of the casting is 350-450℃, the sand is dropped out and the pouring head is cut by using the residual heat. The residual heat temperature shall not be lower than 200℃. If it is lower than 200℃, the pouring head can be cut only after heating in the furnace.

[0049] S2: The bucket tooth casting is heated to 880-900°C and kept at this temperature for 0.5-1 h, and then air-cooled for normalizing; after normalizing, it is heated to 910-930°C, and quenched by cooling with a water-soluble quenching liquid; after quenching, it is heated to 200-260°C and kept at this temperature for 2-3 h, and then air-cooled to obtain a low-alloy high-strength cast steel bucket tooth.

[0050] S3: The low-alloy high-strength cast steel bucket teeth of step S2 are subjected to welding repair, shot peening and polishing treatment to obtain low-alloy high-strength cast steel bucket teeth without surface defects.

[0051] Example 6 A low alloy high strength cast steel bucket tooth and a method for preparing the same in this embodiment include the following steps: S1: Melting and Casting S101 smelting: melt cast steel raw materials such as pig iron and scrap iron in an electric furnace, control the chemical composition of cast steel by weight percentage to C: 0.21%, Si: 0.45%, Mn: 0.85%, Cr: 1.00%, Ti: 0.04%, Mo: 0.45%, P≤0.010%, S≤0.007%, the rest of Fe and unavoidable impurities, add 0.30% silicon block for deoxidation when the temperature of molten steel rises to 1550-1570℃; S102 molten steel treatment: before tapping, the titanium, tin, and boron-iron alloy is crushed into small pieces with a particle size of 5 to 8 mm, and the chemical composition in the cast steel is further controlled by weight percentage to C: 0.205%, Si: 0.40%, Mn: 0.85%, Cr: 0.95%, Ti: 0.04%, Mo: 0.45%, B < 0.079%, Sn < 0.007%, RE: 0.05%, P ≤ 0.007%, S ≤ 0.005%, and the balance is Fe and unavoidable impurities; the treated molten steel is allowed to stand for 60 minutes after slagging, wherein the molten steel temperature is 1530 to 1550°C; after alloying in the electric furnace, the temperature is raised, and the molten steel is tapped into the ladle when the temperature reaches 1630 to 1640°C; S103 pouring and molding: The molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550-1570℃. During pouring, the principle of pouring the casting quickly and pouring the riser slowly is followed, and the pouring speed is controlled to ensure the molding quality of the casting; S104 Insulation and sand removal: After the casting is poured, the sand mold is kept warm for 2 hours, and then the sand is removed from the mold. When the residual heat temperature of the casting is 350-450℃, the sand removal process is started, and the residual heat is used to cut the pouring head. The residual heat temperature shall not be lower than 200℃. If it is lower than 200℃, the pouring head can be cut only after heating in the furnace.

[0052] S2: The bucket tooth casting is heated to 880-900°C and kept at this temperature for 0.5-1 h, and then air-cooled for normalizing; after normalizing, it is heated to 910-930°C, and quenched by cooling with a water-soluble quenching liquid; after quenching, it is heated to 200-260°C and kept at this temperature for 2-3 h, and then air-cooled to obtain a low-alloy high-strength cast steel bucket tooth.

[0053] S3: The low-alloy high-strength cast steel bucket teeth of step S2 are subjected to welding repair, shot peening and polishing treatment to obtain low-alloy high-strength cast steel bucket teeth without surface defects.

[0054] Comparative Example 1 A cast steel bucket tooth and a preparation method thereof in this comparative example include the following steps: S1: Melting and Casting S101 smelting: melt cast steel raw materials such as pig iron and scrap iron in an electric furnace, control the chemical composition of cast steel in weight percentage to C: 0.23%, Si: 0.60%, Mn: 1.00%, Cr: 1.20%, Ti: 0.05%, Mo: 0.50%, P≤0.010%, S≤0.007%, and the balance of Fe and inevitable impurities; add 0.30% silicon blocks for deoxidation when the temperature of molten steel rises to 1550-1570℃; let the molten steel stand for 60 minutes after slagging, wherein the molten steel temperature is 1530-1550℃; raise the temperature after alloying in the electric furnace, and tap the steel into the ladle when the temperature of molten steel reaches 1630-1640℃; S103 pouring and molding: The molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550-1570℃. During pouring, the principle of pouring the casting quickly and pouring the riser slowly is followed, and the pouring speed is controlled to ensure the molding quality of the casting; S104 Insulation and sand removal: After the casting is poured, the sand mold is kept warm for an appropriate time of 2 hours, and then the sand is removed from the box. When the residual heat temperature of the casting is 350-450℃ during unpacking, the sand is removed and the residual heat is used to cut the pouring head. The residual heat temperature shall not be lower than 200℃. If it is lower than 200℃, the pouring head can be cut only after heating in the furnace.

[0055] S2: The bucket tooth casting is heated to 880-900°C and kept at this temperature for 0.5-1 h, and then air-cooled for normalizing; after normalizing, it is heated to 910-930°C, and quenched by cooling with a water-soluble quenching liquid; after quenching, it is heated to 200-260°C and kept at this temperature for 2-3 h, and then air-cooled to obtain a low-alloy high-strength cast steel bucket tooth.

[0056] S3: The low-alloy high-strength cast steel bucket teeth of step S2 are subjected to welding repair, shot peening and polishing treatment to obtain low-alloy high-strength cast steel bucket teeth without surface defects.

[0057] Comparative Example 2 A cast steel bucket tooth and a preparation method thereof in this comparative example include the following steps: S1: Melting and Casting S101 smelting: melt cast steel raw materials such as pig iron and scrap iron in an electric furnace, control the chemical composition of cast steel in weight percentage to C: 0.23%, Si: 0.60%, Mn: 1.00%, Cr: 1.20%, Ti: 0.05%, Mo: 0.50%, P≤0.010%, S≤0.007%, and the balance of Fe and inevitable impurities; add 0.30% silicon blocks for deoxidation when the temperature of molten steel rises to 1550-1570℃; let the molten steel stand for 60 minutes after slagging, wherein the molten steel temperature is 1530-1550℃; raise the temperature after alloying in the electric furnace, and tap the steel into the ladle when the temperature of molten steel reaches 1630-1640℃; S103 pouring and molding: The molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550-1570℃. During pouring, the principle of pouring the casting quickly and pouring the riser slowly is followed, and the pouring speed is controlled to ensure the molding quality of the casting; S104 Insulation and sand removal: After the casting is poured, the sand mold is kept warm for 2 hours, and then the sand is removed from the mold. When the residual heat temperature of the casting is 350-450℃, the sand removal process is started, and the residual heat is used to cut the pouring head. The residual heat temperature must not be lower than 200℃. If it is lower than 200℃, the pouring head can be cut only after heating in the furnace.

[0058] S3: The low alloy high strength cast steel bucket tooth casting of step S1 is subjected to welding repair, shot peening and polishing treatment to obtain a low alloy high strength cast steel bucket tooth without surface defects.

[0059] The mechanical properties of the materials obtained in the above examples 1-6 and comparative examples 1-2 were tested, and the results are shown in the following table: It can be seen from the table that, compared with the comparative example, the low alloy high strength cast steel bucket tooth of the present invention improves the heat treatment performance of the material by adding ferrochrome, ferrosilicon and trace amounts of B, Sn, and Ti, and by reasonably adjusting the ratio of each element; by adopting the normalizing-quenching-tempering heat treatment process, an excellent tempered martensite structure is finally obtained, and the bucket tooth has uniform and good microstructure, high purity, fine grains and dense structure, thereby improving the strength, hardness, tensile strength and other mechanical properties of the bucket tooth.

[0060] The mechanical properties of the low alloy cast steel in Example 2 of the present invention are the best, and its chemical composition comprises by weight percentage: C: 0.20%, Si: 0.40%, Mn: 0.85%, Cr: 0.95%, Ti: 0.04%, Mo: 0.45%, B < 0.080%, Sn < 0.007%, RE: 0.03-0.08%, P ≤ 0.007%, S ≤ 0.005%, and the balance Fe and unavoidable impurities; its mechanical properties are: yield strength 1040 MPa, tensile strength 1520 MPa, elongation 20%, cross-sectional reduction rate 35%, impact absorption energy 52 J, impact toughness 73 J, and hardness 293 HB. Figure 1 and 2 The as-cast metallographic structure and heat-treated metallographic structure of the low-alloy high-strength cast steel bucket tooth in Example 2 are shown in the figure. As can be seen from the figure, after the heat treatment process, an excellent tempered martensite structure is obtained.

[0061] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed in the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A low alloy high strength cast steel bucket tooth, characterized in that: The cast steel bucket tooth contains, by weight percentage, the following: C: 0.19%-0.23%, Si: 0.30%-0.60%, Mn: 0.70%-1.00%, Cr: 0.90%-1.20%, Mo: 0.40%-0.50%, Ti: 0.03%-0.05%, B<0.080%, Sn<0.007%, RE: 0.03%-0.08%, P≤0.010%, S≤0.007%, and the balance is Fe and unavoidable impurities.

2. The low alloy high strength cast steel bucket tooth according to claim 1, characterized in that: The cast steel bucket tooth contains, by weight percentage, the following: C: 0.20%-0.21%, Si 0.40%, Mn 0.85%, Cr 0.95%, Mo 0.45%, Ti 0.04%, B<0.079%, Sn<0.007%, RE: 0.03%-0.08%, P≤0.010%, S≤0.007%, and the balance is Fe and unavoidable impurities.

3. The low alloy high strength cast steel bucket tooth according to claim 2, characterized in that: In the low-alloy high-strength cast steel bucket tooth, the percentage content of S element S≤0.005%, and the percentage content of P element P≤0.007%.

4. The method for preparing a low alloy high strength cast steel bucket tooth according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: Melting and Casting Melting and pouring into bucket tooth castings according to chemical composition ratio; S2: Heat treatment process of bucket tooth castings The bucket tooth casting is heated to 880-900°C and kept warm, then air-cooled for normalizing; after normalizing, heated to 910-930°C, and quenched by cooling with a water-soluble quenching liquid; after quenching, heated to 200-260°C and kept warm, then cooled with air to obtain the low-alloy high-strength cast steel bucket tooth.

5. The preparation method according to claim 4, characterized in that: Step S1 includes the following steps: S101 smelting: melt the raw material of cast steel in an electric furnace, and control the chemical composition by weight percentage to C: 0.19% ~ 0.23%, Si: 0.30 ~ 0.60%, Mn: 0.70% ~ 1.00%, Cr: 0.90% ~ 1.20%, Ti: 0.03% ~ 0.05%, Mo: 0.40% ~ 0.50%, P ≤ 0.010%, S ≤ 0.007%, the rest is Fe and unavoidable impurities; when the temperature of molten steel rises to 1550 ~ 1570 ℃, add 0.30% silicon block for deoxidation; S102 molten steel treatment: before tapping, crush the titanium, tin, and boron-iron alloy into small pieces with a particle size of 5 to 8 mm and add them into the molten steel, and control the chemical composition by weight percentage to C: 0.19% to 0.23%, Si: 0.30 to 0.60%, Mn: 0.70% to 1.00%, Cr: 0.90% to 1.20%, Ti: 0.03% to 0.05%, Mo: 0.40% to 0.50%, P≤0.010%, S≤0.007%, B<0.080%, Sn<0.007%, RE: 0.03-0.08%, and the rest is Fe and unavoidable impurities; let the treated molten steel stand after slagging, wherein the molten steel temperature is 1530 to 1550℃; after alloying in the electric furnace, heat it up, and tap it into the ladle when the molten steel temperature reaches 1630 to 1640℃; S103 casting and molding: the molten steel is poured into the sand mold by a bottom pouring ladle, and the pouring temperature is 1550~1570℃; S104 Insulation and Sand Dropping: After casting, the sand mold is kept warm and then the sand is dropped out of the box.

6. The preparation method according to claim 5, characterized in that: In step S102, the chemical composition is further controlled by weight percentage to C: 0.20% ~ 0.21%, Si 0.40%, Mn 0.85%, Cr 0.95%, Ti 0.04%, Mo 0.45%, B < 0.079%, Sn < 0.007%, RE: 0.03% ~ 0.08%, S ≤ 0.005%, P ≤ 0.007%, and the remainder is Fe and unavoidable impurities.

7. The preparation method according to claim 5, characterized in that: In step S104, the insulation time is 24 to 72 hours.

8. The preparation method according to claim 5, characterized in that: In step S104, when the following conditions are met, the unpacking and sand removal operation is carried out: when the residual heat temperature of the casting is measured at 350-450°C during unpacking, the sand removal process is switched to sand removal, and the residual heat is used to cut the pouring head. The residual heat temperature must not be lower than 200°C. If it is lower than 200°C, the casting is heated in the furnace and then the pouring head is cut.

9. The preparation method according to claim 4, characterized in that: The normalizing holding time is 0.5 to 1 h, the tempering holding time is 2 to 3 h, and the tempering temperature is 230°C.

10. The preparation method according to claim 4, characterized in that: It also includes welding repair, shot peening and polishing steps.

Citation Information

Cited By

  • Cast steel for low-alloy hydraulic support and preparation method and welding process of cast steel

    CN121109896A