Low-cost high-toughness heat-resistant austenite alloy steel and manufacturing method and application thereof

CN118880198APending Publication Date: 2024-11-01SHANGHAI RES INST OF MATERIALS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410921603.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

[0007]本发明提供一种低成本高强韧耐热奥氏体合金钢及其制造方法与应用,以解决上述背景技术中介绍的技术问题:传统热作模具钢的热膨胀系数低,富含Cr和Ni元素的沉淀硬化型奥氏体合金钢的成本高、塑韧性不足

Benefits of technology

[0080]1、与传统热作模具钢(如H13钢)相比较,本发明钢种具有高热膨胀系数,并且同时具有良好的高温抗氧化性和热稳定性。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004936882970000171
    Figure BDA0004936882970000171
  • Figure BDA0004936882970000181
    Figure BDA0004936882970000181
  • Figure BDA0004936882970000191
    Figure BDA0004936882970000191
Patent Text Reader

Abstract

The invention relates to low-cost high-toughness heat-resistant austenite alloy steel and a manufacturing method and application thereof. The high-toughness heat-resistant austenite alloy steel comprises the following chemical components in percentage by mass: 0.45% < = C < = 0.75%, 10.0% < = Mn < = 16.0%, 3.0% < = Cr < = 6.5%, 1.5% < = Al < = 4.0%, 1.0% < = Ni < = 5.0%, Si < = 1.5%, 0.6% < = V < = 1.4%, Mo < = 3.0%, Cu < = 4.0%, Nb < = 1.0%, N < = 0.03%, P < = 0.03%, S < = 0.10% and the balance of Fe and inevitable impurity elements. Wherein the mass percentages of Ni, Mn, C, Cr, Al, V and Nb further meet the following relations: Ni + 0.5 Mn + 30C > = 1.1, Cr + 6Al-2.0%, Cr + Al > = 6.0%, V + 0.7 and Nb < = 1.8%, and Ni + 0.5 Mn + 30C > = 1.1, Cr + 6Al-2.0%, Cr + Al > = 6.0%, V + 0.7 and Nb < = 0.8%. The high-toughness heat-resistant austenite alloy steel is prepared through the processes of casting, hot working and solid solution aging treatment. The austenite alloy steel has the advantages of being low in cost, high in toughness, high in thermal expansion coefficient, good in thermal stability and oxidation resistance and the like, the room temperature hardness of the austenite alloy steel is larger than or equal to 38 HRC, and the room temperature hardness is larger than or equal to 36 HRC after heat preservation is conducted for 24 h at 700 DEG C; and the average linear expansion coefficient alpha m (25, 400) is greater than 17.5 * 10 <-6 > / DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high-strength steel, and in particular relates to a low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel and a manufacturing method and application thereof. Background Art

[0002] The machinery manufacturing industry is constantly developing in the direction of efficient and high-precision processing. Mechanical equipment parts (such as clamping tool holders and drive shafts of CNC machine tool systems) are increasingly using high-strength and ultra-high-strength steel materials. Mutually matched parts can be tightly connected through heat assembly, which makes the structure of mechanical equipment compact, and significantly improves the operating safety and processing accuracy. Here, the mutually matched parts are respectively referred to as containing parts and contained parts. For example, heat shrinkable tool holders (containing parts, which are usually made of high-strength steel) for high-speed CNC machine tools have been widely used because of their high clamping accuracy and large clamping force for machining tools (contained parts), large bending stiffness, and good dynamic balancing performance; the use of heat shrinkable tool holders helps to improve the efficiency of CNC cutting and increase the service life of machine tool spindles and machining tools.

[0003] Thermal assembly is to use the difference in thermal expansion coefficients between the material of the containing part and the material of the contained part to achieve the assembly connection between the containing part and the contained part. The material of the containing part usually has high thermal expansion characteristics, and the thermal expansion coefficient of the containing part material is significantly higher than the thermal expansion coefficient of the contained part material. In terms of geometric dimensions, the inner diameter of the containing part is smaller than the outer diameter of the contained part at room temperature. The thermal assembly process is described as follows: during assembly, the containing part is heated, and the inner diameter of the containing part expands due to heat, so that the contained part can be smoothly placed in the inner hole of the containing part. After cooling, the containing part shrinks and is squeezed and connected with the contained part; during disassembly, the containing part and the contained part are heated at the same time. Since the thermal expansion coefficient of the containing part material is higher than that of the contained part material, the inner diameter of the containing part is larger than the outer diameter of the contained part at high temperature, so that the contained part can be easily removed. In addition, since the parts used as mechanical equipment often undergo repeated hot loading and unloading during their service life, the containing part material usually also needs to have the characteristics of high strength and good high-temperature oxidation resistance and thermal stability. In order to maintain the thermal assembly accuracy of components, the material of the containing parts should not experience obvious strength decay and surface oxidation after multiple heating cycles.

[0004] At present, the materials used for hot-assembly enclosures are mostly hot-working die steel (such as H13 steel). The above steel is usually martensitic alloy steel with a low thermal expansion coefficient, which will result in high heating temperature required for enclosures during hot assembly. As a result, the inner hole of the enclosure is prone to plastic deformation and surface oxidation during hot assembly, and the strength of the enclosure material decays significantly after multiple loading and unloading, thereby reducing the assembly accuracy, operation safety and processing accuracy of mechanical equipment.

[0005] The applicant of the present invention has developed a precipitation-hardened austenitic alloy steel with high thermal expansion, thermal stability and oxidation resistance (see patent CN112301283B for details) for manufacturing heat-fitting enclosures. Due to the high thermal expansion characteristics, the enclosure made of the precipitation-hardened austenitic alloy steel can be heat-fitted at a relatively low temperature, thereby further suppressing the occurrence of obvious plastic deformation, surface oxidation and material strength attenuation at the assembly part of the enclosure. However, the austenitic alloy steel is rich in Cr and Ni elements (in terms of mass percentage, the Cr content is between 8.5% and 11.9%, and the Ni content is between 3.5% and 7.7%). On the one hand, the Cr element rich in the alloy steel is easy to combine with the C element to form chromium carbide, and the chromium carbide is easy to distribute at the austenite grain boundary, thereby significantly reducing the toughness of the alloy steel; on the other hand, adding too much Cr and Ni elements will significantly increase the cost of the alloy steel.

[0006] In summary, in view of the unfavorable properties of existing alloy steels for hot assembly (the low thermal expansion coefficient of traditional hot working die steel, the high cost and insufficient plastic toughness of precipitation hardening austenitic alloy steel rich in Cr and Ni elements), it is urgent to develop a low-cost, high-strength and heat-resistant alloy steel with high expansion characteristics for manufacturing hot assembly containing parts. The developed new alloy steel needs to have higher thermal expansion performance than conventional hot working die steel; it needs to have low cost advantages and enhanced toughness compared to precipitation hardening austenitic alloy steel rich in Cr and Ni elements. Summary of the invention

[0007] The present invention provides a low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel and a manufacturing method and application thereof to solve the technical problems introduced in the above background technology: the traditional hot working die steel has a low thermal expansion coefficient, and the precipitation-hardening austenitic alloy steel rich in Cr and Ni elements has a high cost and insufficient plasticity and toughness.

[0008] The first aspect of the present invention provides a low-cost, high-strength and tough heat-resistant austenitic alloy steel, the second aspect provides a method for manufacturing the low-cost, high-strength and tough heat-resistant austenitic alloy steel, and the third aspect provides an application of the low-cost, high-strength and tough heat-resistant austenitic alloy steel.

[0009] The purpose of the present invention can be achieved through the following technical solutions.

[0010] A first aspect of the present invention provides a low-cost, high-strength, high-toughness, heat-resistant austenitic alloy steel, wherein the alloy steel has a high thermal expansion coefficient.

[0011] A low-cost, high-strength, tough, heat-resistant austenitic alloy steel, the chemical composition mass percentage of which is: 0.45%≤C≤0.75%, 10.0%≤Mn≤16.0%, 3.0%≤Cr≤6.5%, 1.5%≤Al≤4.0%, 1.0%≤Ni≤5.0%, Si≤1.5%, 0.6%≤V≤1.4%, Mo≤3.0%, Cu≤4.0%, Nb≤1.0%, N≤0.03%, P≤0.03%, S≤0.10%, and the rest are Fe and unavoidable impurity elements; wherein the element mass percentages of Ni, Mn, C, Cr and Al, V and Nb elements also need to satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%;

[0012] The matrix structure of the low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel is a single austenite structure and second phase particles dispersed in the austenite matrix;

[0013] The second phase particles include two or more of MX-type carbides and carbonitrides formed between C and V and Nb elements, carbides formed between C and Cr elements, Cu particles, and intermediate compounds formed between Ni and Al elements.

[0014] The properties of the low-cost, high-strength, and heat-resistant austenitic alloy steel meet the following requirements: room temperature hardness ≥ 38HRC, room temperature hardness ≥ 36HRC after being kept at 700°C for 24 hours; average linear expansion coefficient α m(25,400) >17.5×10 -6 / ℃.

[0015] In the component design of the present invention, the role of each component is as follows.

[0016] C: C is a strong austenite stabilizing element. The C element can significantly improve the strength of alloy steel: on the one hand, C improves the strength of alloy steel through the solid solution strengthening mechanism; on the other hand, C mainly combines with Nb and V elements to form fine and dispersed second phase particles (MX carbides and carbonitrides) in the steel matrix, and improves the strength of alloy steel through precipitation strengthening. In addition, C combines with Cr elements to form chromium carbides, which can improve the strength of alloy steel to a certain extent; however, chromium carbides are easily distributed at the austenite grain boundaries, which has the adverse effect of weakening the toughness of alloy steel. When the C content is lower than 0.45%, ferrite phase will appear in the alloy steel, the room temperature hardness of the steel is too low (often less than 38HRC), and the thermal stability of the steel is low due to the insufficient number of MX second phase particles in the steel (the room temperature strength of the steel will decay as the steel is repeatedly heated). Too high a C content will reduce the toughness and corrosion resistance of the alloy steel. The present invention controls the C content to 0.45% to 0.75%.

[0017] Mn: Mn is an austenite stabilizing element, which can replace the precious metal element Ni, and is helpful to obtain a single austenite structure of alloy steel and reduce the cost of alloy steel. Mn combines with the S element in steel to form MnS, which can improve the cutting performance of alloy steel. However, too high a Mn content will reduce the corrosion resistance and weldability of alloy steel. The present invention controls the Mn content to 10.0% to 16.0%.

[0018] Cr: Cr is an important element in the present invention for improving the high temperature oxidation resistance and corrosion resistance of alloy steel (Cr can form a protective film on the surface of alloy steel). If the Cr content is too low (less than 3.0%), the corrosion resistance and high temperature oxidation resistance of the alloy steel will be poor. However, Cr is a ferrite forming element, and too high a Cr content will form a ferrite structure in the steel; and too much Cr content will easily form a large amount of chromium carbides at the austenite grain boundaries, thereby significantly reducing the toughness of the alloy steel. In addition, adding too much Cr will significantly increase the cost of the alloy steel. The present invention controls the Cr content to 3.0% to 6.5%.

[0019] Al: Al is an important element in the present invention to improve the high-temperature oxidation resistance and corrosion resistance of alloy steel. Adding Al element promotes the formation of Al2O3 passivation film on the alloy surface, thereby improving the high-temperature oxidation resistance and corrosion resistance of alloy steel. In addition, Al can combine with Ni to form fine intermetallic compound particles, which plays a role in strengthening the austenite matrix of alloy steel. In addition, partial substitution of Cr with Al can reduce the precipitation and enrichment of chromium carbides at the austenite grain boundaries of alloy steel while ensuring the oxidation resistance and corrosion resistance of alloy steel, thereby significantly improving the plasticity and toughness of alloy steel; at the same time, substitution of Cr with Al can improve the linear expansion coefficient of alloy steel and reduce the cost of alloy steel. However, Al is a ferrite-forming element, and too much Al is easy to form ferrite in steel; and when the Al content is too high, the welding performance and manufacturability of alloy steel will be reduced. The present invention controls the Al content to 1.5% to 4.0%.

[0020] In the present invention, in order to ensure that the alloy steel has good high-temperature oxidation resistance and corrosion resistance, the mass percentages of Cr and Al elements need to be controlled to satisfy: Cr+Al≥6.0%.

[0021] Ni: Ni is an austenite stabilizing element, which helps the alloy steel matrix obtain a single austenite structure and keeps the steel grade with good plasticity and toughness. Ni can promote the stability of the Cr-containing passivation film, thereby improving the corrosion resistance and high-temperature oxidation resistance of the alloy steel. Ni can also improve the corrosion resistance of steel in alkaline media. Furthermore, Ni can combine with Al to form a fine intermetallic compound particle phase, which plays a role in strengthening the austenite matrix. However, Ni is a precious alloy element, and adding too much Ni will significantly increase the cost of the alloy steel. The present invention controls the Ni content to be 1.0% to 5.0%.

[0022] Si: Si element has a strong solid solution strengthening effect and helps to improve the fluidity of molten steel. Si can improve the high temperature oxidation resistance of alloy steel. On the one hand, the addition of Si can promote the formation of Cr2O3 on the surface. On the other hand, the SiO2 oxide layer reduces the diffusion rate of iron atoms and oxygen atoms, slows down the oxidation process of steel, and thus improves the oxidation resistance of alloy steel. However, Si is a ferrite forming element. Too much Si is easy to form ferrite structure in steel, and too much Si will reduce the plasticity and welding performance of alloy steel. The present invention controls the Si content to be no more than 1.5%.

[0023] V: V is a strong carbide and (or) carbonitride forming element. It combines with C and N elements to form fine and dispersed MX type second phase particles, thereby significantly improving the strength and thermal stability of alloy steel. V preferentially combines with C in steel to reduce the precipitation of chromium carbides at austenite grain boundaries, thereby improving the corrosion resistance and toughness of steel. Furthermore, adding V can refine the grain structure of alloy steel. When the V content is too low, the precipitated second phase content is small, which is not enough to make the room temperature hardness of the alloy steel ≥38HRC. However, too much V will lead to excessive precipitation phase content, thereby reducing the plastic toughness of the alloy steel. The present invention controls the V content to 0.6% to 1.4%.

[0024] Nb: Nb is a strong carbide and (or) carbonitride forming element. It forms fine MX-type second phase particles by combining with C and N elements, thereby significantly improving the strength and thermal stability of alloy steel and refining the grains. Nb preferentially combines with C in steel to reduce the precipitation of chromium carbides at austenite grain boundaries, thereby improving the corrosion resistance and toughness of steel. The present invention controls the Nb content to be no more than 1.0%.

[0025] In the present invention, a composite addition of Nb and V can be adopted to effectively achieve the effects of grain refinement and precipitation hardening; and the effect of the composite addition of Nb and V is often greater than the effect of adding Nb or V alone. When the addition amount of Nb and V is too low (0.7Nb+V<0.8%), the content of the precipitated second phase is small, which is not enough to make the room temperature hardness of the alloy steel ≥38HRC; when the addition amount of Nb and V is too high (0.7Nb+V>1.8%), the content of the precipitated second phase is large, thereby significantly reducing the plastic toughness of the alloy steel.

[0026] Mo: Mo can improve the corrosion resistance of alloy steel to reducing media, pitting corrosion and crevice corrosion, and at the same time, it is dissolved in the austenite matrix to improve the strength and thermal stability of alloy steel. However, Mo is a ferrite-forming element, and too much Mo is easy to form ferrite in steel, and Mo is expensive, thereby increasing production costs. The present invention controls the Mo content to be no more than 3.0%.

[0027] Cu: Cu is an austenite-forming element and can partially replace the precious element Ni to reduce production costs. When the Cu content is supersaturated, it will aggregate to form a copper-rich phase in the alloy steel matrix after solution aging treatment, thereby improving the room temperature strength and hardness of the steel. In addition, the addition of Cu can effectively improve the corrosion resistance of the alloy steel and reduce the cold work hardening tendency of the steel. However, adding too much Cu element will reduce the hot working performance of the steel. The present invention controls the Cu content to be no more than 4.0%.

[0028] N: N is easily combined with Al to form AlN inclusions in the steel matrix, thereby affecting the manufacturability and plasticity of the alloy steel. The present invention limits N to ≤ 0.03%.

[0029] P: P will increase the cold brittleness of steel and reduce the plasticity and welding performance of steel. In the present invention, P is controlled to be ≤ 0.03%.

[0030] S: S will make steel hot brittle and reduce its plasticity, toughness and welding performance; however, a proper amount of MnS in steel helps to enhance its cutting performance. The present invention controls S≤0.10%.

[0031] In the present invention, C, Mn, Ni austenite forming elements are mainly added, and the content of Cr and Al ferrite forming elements is controlled, and the addition amount of Ni, Mn, C, Cr and Al elements also needs to satisfy Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, so that the alloy steel matrix has a single austenite structure. At the same time, the above-mentioned component design makes the austenite structure of the alloy steel have a lower stacking fault energy, and the austenite structure contains more low-energy twin boundaries (the proportion of the low-energy twin boundaries is often higher than the proportion of low-energy twin boundaries in precipitation hardening austenitic alloy steel rich in Ni and Cr elements (such as the steel disclosed in patent CN112301283B)), thereby inhibiting the aggregation and distribution of carbides at low-energy twin boundaries and improving the plastic toughness of the alloy steel. In addition, by controlling the Cr element content (≤6.5wt%), the number of chromium carbides at the austenite grain boundaries is reduced, and the alloy steel is further made to have sufficient plastic toughness. In the present invention, when the room temperature hardness of the alloy steel is about 40HRC, the notch impact energy KV2 of the alloy steel is generally greater than 16J; and under the same room temperature hardness (about 40HRC) conditions, when the Cr content in the alloy steel is greater than 8.0wt%, the notch impact energy KV2 of the alloy steel is generally significantly lower than 16J.

[0032] In order to obtain a high linear expansion coefficient of alloy steel, in addition to making the matrix structure of the alloy steel a single austenite structure, it is also necessary to strictly control the chemical composition and key element content of the alloy steel. In the present invention, by adding Al and Mn elements and limiting the content of Cr, Mo and Si elements, the alloy steel has a higher linear expansion coefficient.

[0033] In order to make the alloy steel have high strength and good thermal stability, fine second-phase hard particles need to be evenly dispersed in the alloy steel matrix, and the above-mentioned second-phase hard particles do not coarsen significantly when the alloy steel is kept at 700℃ for 24 hours. Adding appropriate amounts of Nb and V strong carbide-forming elements to the steel, through solid solution and aging treatment, fine and dispersed MX-type carbides and carbonitrides are formed in the austenite matrix, thereby improving the strength of the alloy steel. The fine-scale MX phase has good thermal stability and can improve the high-temperature strength and thermal stability of the alloy steel. In addition, the intermediate compounds formed by Ni and Al and the Cu precipitation phase particles will also strengthen the austenite matrix of the alloy steel. In addition, the Mo element has a good solid solution strengthening effect, which can significantly improve the room temperature and high temperature strength of the alloy steel and increase the thermal stability of the alloy steel.

[0034] In order to make the alloy steel have good high temperature oxidation resistance, Al, Cr (and Si) elements are added to form a dense passivation film on the surface of the alloy steel.

[0035] In order to make the alloy steel have certain corrosion resistance, it is necessary to add appropriate amounts of Cr, Ni, Cu and Mo elements.

[0036] In one embodiment of the present invention, a low-cost, high-strength, tough, heat-resistant austenitic alloy steel has a chemical composition mass percentage of: 0.46%≤C≤0.74%, 10.1%≤Mn≤15.8%, 3.1%≤Cr≤6.4%, 1.6%≤Al≤3.8%, 1.1%≤Ni≤4.9%, 0.3%≤Si≤1.4%, 0.62%≤V≤1.32%, 0.5%≤Mo≤2.9%, Cu≤3.9%, Nb≤0.9%, N≤0.03%, P≤0.02%, S≤0.08%, and the rest are Fe and unavoidable impurity elements; wherein, the element mass percentages of Ni, Mn, C, Cr and Al, V and Nb elements must also satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%.

[0037] The second aspect of the present invention provides a method for manufacturing the above-mentioned low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel.

[0038] The first method for manufacturing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel comprises the following steps:

[0039] 1) Smelt and cast according to the following composition ratio to obtain a casting

[0040] The mass percentage of chemical composition is: 0.45%≤C≤0.75%, 10.0%≤Mn≤16.0%, 3.0%≤Cr≤6.5%, 1.5%≤Al≤4.0%, 1.0%≤Ni≤5.0%, Si≤1.5%, 0.6%≤V≤1.4%, Mo≤3.0%, Cu≤4.0%, Nb≤1.0%, N≤0.03%, P≤0.03%, S≤0.10%, and the rest are Fe and unavoidable impurity elements; among which, the mass percentage of Ni, Mn, C, Cr and Al, V and Nb elements must also satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%;

[0041] 2) Thermal deformation processing

[0042] The ingot is heated within a temperature range of 1050 to 1230°C, kept at this temperature for 1 to 6 hours, and then processed into bars or plates by hot rolling or forging;

[0043] 3) Heat treatment after deformation

[0044] Post-deformation heat treatment includes two processes: solution treatment and aging treatment. First, the bars or plates deformed by hot working are subjected to solution treatment, and then the bars or plates after solution treatment are subjected to aging treatment.

[0045] In one embodiment of the present invention, in step 2), the deformation pass temperature during hot rolling or forging is ≥850°C, and the ratio of the cross-sectional area of ​​the ingot before and after hot deformation is ≥2.0.

[0046] In one embodiment of the present invention, in step 3), the conditions for solution treatment are: solution temperature is 1100-1230°C, heat preservation is 1-5h, and then cooling to room temperature at a cooling rate of not less than 300°C / min.

[0047] In one embodiment of the present invention, in step 3), the aging treatment is performed under the following conditions: the aging temperature is 600-750° C., the temperature is kept for 2-50 hours, and then air-cooled to room temperature.

[0048] The design reasons for the manufacturing method of the first type of low-cost, high-strength and tough heat-resistant austenitic alloy steel are as follows:

[0049] (1) Thermal deformation processing technology

[0050] The alloy steel ingot is processed into bars or plates of required size by forging or hot rolling.

[0051] The heating temperature is 1050-1230°C. When the heating temperature exceeds 1230°C, the ingot will be overburned, the grain structure of the ingot will be coarse, and its hot working performance will be reduced; when the heating temperature is lower than 1050°C, the degree of homogenization of the ingot structure is not enough, and the deformation resistance of the ingot is too large, so it is difficult to produce bars or plates with no surface defects and specified dimensions.

[0052] The heating and holding time is 1 to 6 hours. If the holding time exceeds 6 hours, the grain structure inside the ingot will be coarse and the production efficiency will be affected; if the holding time is less than 1 hour, the temperature inside the ingot is not uniform and the degree of homogenization of the ingot structure is not sufficient.

[0053] In the manufacturing method of the alloy steel mentioned above of the present invention, the ratio of the cross-sectional areas before and after hot deformation of the ingot is controlled to be ≥2.0, in order to eliminate the internal structural heterogeneity and defects of the ingot; the deformation pass temperature is controlled to be above 850°C to complete the hot working of the ingot. If the deformation pass temperature is too low, the deformation resistance of the ingot will be too high, making it difficult to manufacture hot-worked deformed materials with required size specifications and without surface and edge defects.

[0054] (2) Solution and aging heat treatment

[0055] Solution treatment and aging treatment are key processes for obtaining the required mechanical properties of the alloy steel in the manufacturing method of the alloy steel of the present invention. The bars or plates after hot working are subjected to solution treatment (i.e., the alloy steel is heated to a high temperature zone and kept at a constant temperature, so that the second phase particles are dissolved into the solid solution and then rapidly cooled to obtain a supersaturated solid solution of the alloy steel), the solution temperature is 1100-1230°C, the temperature is kept for 1-5 hours, and then cooled to room temperature at a cooling rate of not less than 300°C / min. When the solution temperature is lower than 1100℃ and the holding time is less than 1h, the second phase particles formed in the previous solidification and hot working process in the alloy steel cannot be fully dissolved in the austenite matrix. This will lead to the material in the subsequent aging process. Due to the low supersaturation of Nb and V in austenite, it is difficult to precipitate fine second phase particles with sufficient volume content and dispersed distribution in the austenite matrix, so that the alloy steel cannot obtain the required strength, hardness (room temperature hardness ≥ 38HRC) and good high temperature thermal stability (room temperature hardness ≥ 36HRC after holding at 700℃ for 24h); at the same time, the coarse second phase particles formed during the solidification and hot working process will reduce the plasticity and toughness of the alloy steel. When the cooling rate after solution is less than 300℃ / min, the second phase particles precipitated during the cooling process will coarsen, which is also not conducive to improving the strength and high temperature thermal stability of the alloy steel. When the solution temperature is higher than 1230℃ and the holding time is too long, the grains of the alloy steel grow rapidly during the solution process, and the coarse microstructure will be unfavorable to the strength and plasticity and toughness of the alloy steel. In addition, too long solution time will affect production efficiency. In actual production, the solution temperature can be appropriately increased to shorten the solution holding time.

[0056] In the manufacturing method of the alloy steel of the present invention, the material after solution treatment is subjected to aging treatment (i.e., the supersaturated solid solution of the alloy steel is placed under certain temperature conditions to cause dissolution and precipitation of a fine second phase, thereby improving the strength of the alloy steel), the aging temperature is 600-750°C, the temperature is kept for 2-50 hours, and then air-cooled to room temperature. When the aging temperature is lower than 600°C and the insulation time is less than 2 hours, the volume content of the second phase precipitated in the alloy steel matrix is ​​small, and the strength of the alloy steel is low; when the aging temperature is higher than 750°C and the aging time is too long, the second phase particles precipitate quickly and coarsen at a higher temperature, and the precipitation strengthening effect will be weakened. In addition, a too long aging time will affect production efficiency. In actual production, the aging temperature can be appropriately increased to shorten the aging insulation time. In the manufacturing method of the alloy steel of the present invention, the aging time is controlled not to exceed 50 hours.

[0057] The second method for manufacturing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel comprises the following steps:

[0058] 1) Smelt and cast according to the following composition ratio to obtain a casting

[0059] The mass percentage of chemical composition is: 0.45%≤C≤0.75%, 10.0%≤Mn≤16.0%, 3.0%≤Cr≤6.5%, 1.5%≤Al≤4.0%, 1.0%≤Ni≤5.0%, Si≤1.5%, 0.6%≤V≤1.4%, Mo≤3.0%, Cu≤4.0%, Nb≤1.0%, N≤0.03%, P≤0.03%, S≤0.10%, and the rest are Fe and unavoidable impurity elements; among which, the mass percentage of Ni, Mn, C, Cr and Al, V and Nb elements must also satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%;

[0060] 2) Thermal deformation processing

[0061] The hot deformation processing method includes forging and hot rolling. The ingot is first forged to form an intermediate slab or billet, and then the intermediate slab or billet is hot rolled into a plate or bar of the required size.

[0062] 3) Heat treatment after deformation

[0063] Post-deformation heat treatment includes two processes: solution treatment and aging treatment. First, the bars or plates deformed by hot working are subjected to solution treatment, and then the bars or plates after solution treatment are subjected to aging treatment.

[0064] In one embodiment of the present invention, in step 2), the process conditions for forging the blank are: heating the blank at 1050-1230°C, keeping it warm for 1-6 hours, and then forging the blank into an intermediate slab or a square billet, the forging deformation pass temperature is ≥850°C, and the ratio of the cross-sectional area of ​​the blank before and after forging is ≥1.5.

[0065] In one embodiment of the present invention, in step 2), the process conditions of hot rolling are: heating the intermediate slab or billet at 1050-1230°C, keeping warm for 1-6 hours, and then hot-rolling the intermediate slab or billet into plates or bars of required size specifications, the hot rolling deformation pass temperature is ≥850°C, and the ratio of the cross-sectional area of ​​the original ingot to the cross-sectional area of ​​the plate or bar after hot rolling is ≥2.0.

[0066] In one embodiment of the present invention, in step 3), the conditions for solution treatment are: solution temperature is 1100-1230°C, heat preservation is 1-5h, and then cooling to room temperature at a cooling rate of not less than 300°C / min.

[0067] In one embodiment of the present invention, in step 3), the aging treatment is performed under the following conditions: the aging temperature is 600-750° C., the temperature is kept for 2-50 hours, and then air-cooled to room temperature.

[0068] The reasons for designing the manufacturing method of the second type of low-cost, high-strength and tough heat-resistant austenitic alloy steel of the present invention are as follows:

[0069] (1) Thermal deformation processing technology

[0070] The alloy steel ingot is processed into bars or plates of required size through a deformation method combining forging and hot rolling.

[0071] When forging the blank, the heating temperature is 1050-1230℃, and the heating and holding time is 1-6h. When the heating temperature exceeds 1230℃, the blank will be overburned, the blank grain structure will be coarse, and its hot working performance will be reduced; when the heating temperature is lower than 1050℃, the blank structure homogenization is insufficient, and the blank deformation resistance is too large, so it is difficult to process a forged blank with no surface defects and a specified size. When the holding time exceeds 6h, the internal grain structure of the blank will be coarse and affect the production efficiency; when the holding time is lower than 1h, the internal temperature of the blank is not uniform, and the degree of homogenization of the blank structure is insufficient. The present invention controls the ratio of the cross-sectional area before and after the blank forging to be ≥1.5, so as to basically eliminate the internal structure non-uniformity and defects of the blank, and provide a good blank structure for subsequent hot rolling; the forging pass temperature is controlled to be above 850℃. If the forging pass temperature is too low, the blank deformation resistance will be too high, so it is difficult to manufacture a forged blank with the required size and no surface and edge defects.

[0072] During hot rolling, the forging blank is heated at 1050-1230°C and kept warm for 1-6 hours. When the heating temperature exceeds 1230°C, the forging blank will be overburned, and the grain structure of the forging blank will be coarse, thereby reducing its hot working performance; when the heating temperature is lower than 1050°C, the deformation resistance of the forging blank is too large, making it difficult to process a bar or plate with no surface defects and a specified size. When the holding time exceeds 6 hours, the grain structure inside the forging blank will be coarse and affect the production efficiency; when the holding time is lower than 1 hour, the temperature inside the forging blank is not easy to be uniform. The present invention controls the hot rolling pass temperature to be above 850°C. If the hot rolling pass temperature is too low, the deformation resistance of the material will be too high, making it difficult to manufacture a bar or plate with the required size and specifications and without surface and edge defects. The ratio of the cross-sectional area of ​​the original ingot to the cross-sectional area of ​​the plate or bar after hot rolling is controlled to be ≥2.0, so that the material structure is uniform after hot rolling.

[0073] The combination of forging and hot rolling is suitable for preparing alloy steel bars or plates with high requirements for organizational uniformity.

[0074] (2) Solution and aging heat treatment

[0075] The bars or plates after hot working are subjected to solid solution treatment to obtain a supersaturated solid solution of alloy steel. The solid solution temperature is 1100-1230℃, and the temperature is kept for 1-5 hours, and then cooled to room temperature at a cooling rate of not less than 300℃ / min. When the solid solution temperature is lower than 1100℃ and the holding time is less than 1h, the second phase particles formed in the previous solidification and hot working process in the alloy steel cannot be fully dissolved in the austenite matrix, which will lead to the material in the subsequent aging process. Due to the low supersaturation of Nb and V in austenite, it is difficult to precipitate fine second phase particles with sufficient volume content and dispersed distribution in the austenite matrix, so that the alloy steel cannot obtain the required strength, hardness (room temperature hardness ≥38HRC) and good high temperature thermal stability (room temperature hardness ≥36HRC after holding at 700℃ for 24h); at the same time, the coarse second phase particles formed during the solidification and hot working process will reduce the plasticity and toughness of the alloy steel. When the cooling rate after solution treatment is less than 300℃ / min, the second phase particles precipitated during the cooling process will coarsen, which is also not conducive to improving the strength and high-temperature thermal stability of the alloy steel. When the solution temperature is higher than 1230℃ and the holding time is too long, the grains of the alloy steel grow rapidly during the solution process, and the coarse microstructure is not conducive to the strength and plasticity of the alloy steel. In addition, too long a solution time will affect production efficiency. In actual production, the solution temperature can be appropriately increased to shorten the solution holding time.

[0076] The material after solution treatment is subjected to aging treatment at an aging temperature of 600-750°C, kept at this temperature for 2-50 hours, and then air-cooled to room temperature. When the aging temperature is lower than 600°C and the holding time is less than 2 hours, the volume content of the second phase precipitated in the alloy steel matrix is ​​small, and the strength of the alloy steel is low; when the aging temperature is higher than 750°C and the aging time is too long, the second phase precipitates and coarsens at a higher temperature quickly, and the precipitation strengthening effect is weakened. In addition, a too long aging time will affect production efficiency. In actual production, the aging temperature can be appropriately increased to shorten the aging holding time. The present invention controls the aging time to not exceed 50 hours.

[0077] The present invention adopts the above-mentioned composition design, heat processing process and heat treatment process, and the matrix structure of the prepared alloy steel bar or plate is a single austenite structure and second phase particles dispersed in the austenite matrix. The second phase particles include two or more of MX carbides and carbonitrides formed between C and V, Nb elements, chromium carbides formed between C and Cr elements, Cu particles, and intermediate compounds formed between Ni and Al elements, and MX carbides and carbonitrides are mainly used. The austenitic alloy steel has high strength, good thermal stability and high temperature oxidation resistance, and its room temperature hardness is ≥38HRC, and the room temperature hardness is ≥36HRC after being kept at 700°C for 24 hours. The average linear expansion coefficient of the austenitic alloy steel is α m(25,400) >17.5×10 -6 / ℃.

[0078] The third aspect of the present invention provides an application of low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel, which is suitable for but not limited to the manufacture of containing parts that are repeatedly loaded and unloaded using thermal assembly methods in mechanical equipment, such as heat shrinkable tool handles of CNC machine tool system components.

[0079] Compared with the prior art, the present invention has the following beneficial effects:

[0080] 1. Compared with traditional hot working die steel (such as H13 steel), the steel of the present invention has a high thermal expansion coefficient and also has good high temperature oxidation resistance and thermal stability.

[0081] 2. Compared with precipitation-hardening austenitic alloy steels rich in Cr and Ni elements, the steel of the present invention has the advantages of low cost and enhanced plasticity and toughness.

[0082] 3. The manufacturing process involved in the present invention can be completed on the existing alloy steel production line without making major adjustments, so the present invention has a good prospect for promotion and application. DETAILED DESCRIPTION

[0083] A low-cost, high-strength, tough, and heat-resistant austenitic alloy steel, the chemical composition mass percentage of which is: 0.45%≤C≤0.75%, 10.0%≤Mn≤16.0%, 3.0%≤Cr≤6.5%, 1.5%≤Al≤4.0%, 1.0%≤Ni≤5.0%, Si≤1.5%, 0.6%≤V≤1.4%, Mo≤3.0%, Cu≤4.0%, Nb≤1.0%, N≤0.03%, P≤0.03%, S≤0.10%, and the rest are Fe and unavoidable impurity elements; wherein the element mass percentages of Ni, Mn, C, Cr, Al, V, and Nb elements also need to satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%.

[0084] The first method for manufacturing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel comprises the following steps:

[0085] 1) Smelt and cast according to the following composition ratio to obtain a casting

[0086] The mass percentage of chemical composition is: 0.45%≤C≤0.75%, 10.0%≤Mn≤16.0%, 3.0%≤Cr≤6.5%, 1.5%≤Al≤4.0%, 1.0%≤Ni≤5.0%, Si≤1.5%, 0.6%≤V≤1.4%, Mo≤3.0%, Cu≤4.0%, Nb≤1.0%, N≤0.03%, P≤0.03%, S≤0.10%, and the rest are Fe and unavoidable impurity elements; among which, the mass percentage of Ni, Mn, C, Cr and Al, V and Nb elements must also satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%.

[0087] 2) Thermal deformation processing

[0088] The ingot is heated at 1050-1230℃, kept warm for 1-6 hours, and then hot processed into bars or plates. The hot deformation processing method is hot rolling or forging. The deformation pass temperature is ≥850℃, and the ratio of the cross-sectional area of ​​the ingot before and after hot deformation is >9.

[0089] 3) Heat treatment after deformation

[0090] Heat treatment after deformation includes two processes: solution treatment and aging treatment. First, the bars or plates after hot working deformation are subjected to solution treatment at a solution temperature of 1100-1230°C, kept at this temperature for 1-5 hours, and then cooled to room temperature at a cooling rate of not less than 300°C / min. Then, the solution treated materials are subjected to aging treatment at an aging temperature of 600-750°C, kept at this temperature for 2-50 hours, and then air cooled to room temperature.

[0091] The second method for manufacturing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel comprises the following steps:

[0092] 1) Smelt and cast according to the following composition ratio to obtain a casting

[0093] The mass percentage of chemical composition is: 0.45%≤C≤0.75%, 10.0%≤Mn≤16.0%, 3.0%≤Cr≤6.5%, 1.5%≤Al≤4.0%, 1.0%≤Ni≤5.0%, Si≤1.5%, 0.6%≤V≤1.4%, Mo≤3.0%, Cu≤4.0%, Nb≤1.0%, N≤0.03%, P≤0.03%, S≤0.10%, and the rest are Fe and unavoidable impurity elements; among which, the mass percentage of Ni, Mn, C, Cr and Al, V and Nb elements must also satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%.

[0094] 2) Thermal deformation processing

[0095] Hot working includes two parts: forging and hot rolling.

[0096] The ingot is heated at 1050-1230℃, kept warm for 1-6 hours, and then forged into a slab or billet. The forging deformation pass temperature is ≥850℃, and the ratio of the cross-sectional area of ​​the ingot before and after forging is >3;

[0097] The forging billet is heated at 1050-1230℃, kept warm for 1-6 hours, and then hot rolled into bars or plates. The hot rolling deformation pass temperature is ≥850℃, and the ratio of the cross-sectional area of ​​the original billet to the cross-sectional area of ​​the plate or bar after hot rolling is >12.

[0098] 3) Heat treatment after deformation

[0099] Heat treatment after deformation includes two processes: solution treatment and aging treatment. First, the hot-processed bars or plates are subjected to solution treatment at a temperature of 1100-1230°C, kept at this temperature for 1-5 hours, and then cooled to room temperature at a cooling rate of not less than 300°C / min. Then, the solution-treated materials are subjected to aging treatment at a temperature of 600-750°C, kept at this temperature for 2-50 hours, and then air-cooled to room temperature.

[0100] The present invention is described in detail below with reference to specific embodiments.

[0101] Table 1 shows the chemical composition mass percentage of the steel grades of the embodiment of the present invention and the comparative example; Table 2 shows the manufacturing process of the steel grades of the embodiment of the present invention and the comparative example; Table 3 shows the room temperature hardness, room temperature hardness after being kept at 700°C for 24 hours and average linear expansion coefficient α of the steel grades of the embodiment of the present invention and the comparative example m(25,400) .

[0102] The content ratio of each component in Examples 1-11 and Comparative Examples 1-2 is designed according to Table 1. In the examples, the mass percentages of Ni, Mn, C, Cr and Al elements satisfy the relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%.

[0103] Table 1 (Unit: wt%)

[0104]

[0105] The steel material with the composition shown in Table 1 is made into a cast billet after smelting and casting. The cast billet is heated at a heating temperature of 1150°C and kept warm for 2 hours, and hot working deformation is completed under the condition that the pass temperature is not lower than 880°C. The hot working methods of the embodiments and comparative examples, and the ratio of the cross-sectional area of ​​the original cast billet to the cross-sectional area of ​​the final plate / bar are shown in Table 2. The hot-worked bars or plates are further treated by the heat treatment process shown in Table 2 to obtain the final bars or plates. The matrix structure of all the steel grades in the embodiments is a single austenite structure. The steel grade of comparative example 2 contains a partial ferrite structure.

[0106] Table 2

[0107]

[0108] Room temperature hardness, room temperature hardness after 24h of 700℃ heat preservation and average linear expansion coefficient α of Examples 1-11 of the present invention and Comparative Examples 1-2 m(25,400) See Table 3.

[0109] Table 3

[0110]

[0111] It can be seen from the steel grades in the embodiment in Table 3 that the present invention can obtain low-cost, high-strength and heat-resistant austenitic alloy steel through reasonable composition and process design. The room temperature hardness of the alloy steel is ≥38HRC, and the room temperature hardness is ≥36HRC after being kept at 700℃ for 24h. The average linear expansion coefficient α of the alloy steel is m(25,400) >17.5×10 -6 / ℃. In the steel of comparative example 1, V+0.7Nb<0.8%, and accordingly, the room temperature hardness is low (less than 38HRC). The steel of comparative example 2 contains part of ferrite in its matrix structure, and the average linear expansion coefficient of the steel is α m(25,400) <17.5×10 -6 / ℃; in addition, due to the rich Cr, the notch impact energy of the comparative example 2 steel is significantly lower than that of the example steel.

[0112] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A low-cost, high-strength, and heat-resistant austenitic alloy steel, characterized in that: The chemical composition mass percentage of the low-cost, high-strength and tough heat-resistant austenitic alloy steel is as follows: 0.45%≤C≤0.75%, 10.0%≤Mn≤16.0%, 3.0%≤Cr≤6.5%, 1.5%≤Al≤4.0%, 1.0%≤Ni≤5.0%, Si≤1.5%, 0.6%≤V≤1.4%, Mo≤3.0%, Cu≤4.0%, Nb≤1.0%, N≤0.03%, P≤0.03%, S≤0.10%, and the rest are Fe and unavoidable impurity elements; wherein the element mass percentages of Ni, Mn, C, Cr and Al, V and Nb elements must also satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%; The matrix structure of the low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel is a single austenite structure and second phase particles dispersed in the austenite matrix; The second phase particles include two or more of MX-type carbides and carbonitrides formed between C and V and Nb elements, carbides formed between C and Cr elements, Cu particles, and intermediate compounds formed between Ni and Al elements.

2. The low-cost, high-strength, and high-toughness heat-resistant austenitic alloy steel according to claim 1, characterized in that: The properties of the low-cost, high-strength, and heat-resistant austenitic alloy steel meet the following requirements: room temperature hardness ≥ 38HRC, room temperature hardness ≥ 36HRC after being kept at 700°C for 24 hours; average linear expansion coefficient α m(25,400) >17.5×10 -6 / ℃.

3. The method for producing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel according to claim 1 or 2, characterized in that: The following steps are involved: 1) Smelt and cast according to the following composition ratio to obtain a casting The mass percentage of chemical composition is: 0.45%≤C≤0.75%, 10.0%≤Mn≤16.0%, 3.0%≤Cr≤6.5%, 1.5%≤Al≤4.0%, 1.0%≤Ni≤5.0%, Si≤1.5%, 0.6%≤V≤1.4%, Mo≤3.0%, Cu≤4.0%, Nb≤1.0%, N≤0.03%, P≤0.03%, S≤0.10%, and the rest are Fe and unavoidable impurity elements; among which, the mass percentage of Ni, Mn, C, Cr and Al, V and Nb elements must also satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%; 2) Thermal deformation processing The ingot is heated within a temperature range of 1050 to 1230°C, kept at this temperature for 1 to 6 hours, and then processed into bars or plates by hot rolling or forging; 3) Heat treatment after deformation Post-deformation heat treatment includes two processes: solution treatment and aging treatment. First, the bars or plates deformed by hot working are subjected to solution treatment, and then the bars or plates after solution treatment are subjected to aging treatment.

4. The method for manufacturing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel according to claim 3, characterized in that: In step 2), the deformation pass temperature during hot rolling or forging is ≥850°C, and the ratio of the cross-sectional area of ​​the ingot before and after hot deformation is ≥2.

0.

5. The method for manufacturing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel according to claim 3, characterized in that: In step 3), The conditions for the solution treatment are: the solution temperature is 1100-1230°C, the temperature is kept for 1-5 hours, and then cooled to room temperature at a cooling rate of not less than 300°C / min; The conditions for aging treatment are: aging temperature is 600-750°C, keeping warm for 2-50 hours, and then air cooling to room temperature.

6. The method for producing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel according to claim 1 or 2, characterized in that: The following steps are involved: 1) Smelt and cast according to the following composition ratio to obtain a casting The mass percentage of chemical composition is: 0.45%≤C≤0.75%, 10.0%≤Mn≤16.0%, 3.0%≤Cr≤6.5%, 1.5%≤Al≤4.0%, 1.0%≤Ni≤5.0%, Si≤1.5%, 0.6%≤V≤1.4%, Mo≤3.0%, Cu≤4.0%, Nb≤1.0%, N≤0.03%, P≤0.03%, S≤0.10%, and the rest are Fe and unavoidable impurity elements; among which, the mass percentage of Ni, Mn, C, Cr and Al, V and Nb elements must also satisfy the following relationship: Ni+0.5Mn+30C≥1.1Cr+6Al-2.0%, Cr+Al≥6.0%, 0.8%≤V+0.7Nb≤1.8%; 2) Thermal deformation processing The hot deformation processing method includes forging and hot rolling. The ingot is first forged to form an intermediate slab or billet, and then the intermediate slab or billet is hot rolled into a plate or bar of the required size. 3) Heat treatment after deformation Post-deformation heat treatment includes two processes: solution treatment and aging treatment. First, the bars or plates deformed by hot working are subjected to solution treatment, and then the bars or plates after solution treatment are subjected to aging treatment.

7. The method for manufacturing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel according to claim 6, characterized in that: In step 2), the process conditions for forging are: heating the ingot at 1050-1230°C, keeping it warm for 1-6 hours, and then forging the ingot into an intermediate slab or billet, the forging deformation pass temperature is ≥850°C, and the ratio of the cross-sectional area of ​​the ingot before and after forging is ≥1.

5.

8. The method for manufacturing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel according to claim 6, characterized in that: In step 2), the process conditions for hot rolling are: heating the intermediate slab or billet at 1050-1230°C, keeping it warm for 1-6 hours, and then hot-rolling the intermediate slab or billet into plates or bars of required size specifications, the hot rolling deformation pass temperature is ≥850°C, and the ratio of the cross-sectional area of ​​the original ingot to the cross-sectional area of ​​the plate or bar after hot rolling is ≥2.

0.

9. The method for manufacturing low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel according to claim 6, characterized in that: In step 3), The conditions for the solution treatment are: the solution temperature is 1100-1230°C, the temperature is kept for 1-5 hours, and then cooled to room temperature at a cooling rate of not less than 300°C / min; The conditions for aging treatment are: aging temperature is 600-750°C, keeping warm for 2-50 hours, and then air cooling to room temperature.

10. Application of the low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel according to claim 1 or 2, characterized in that: The low-cost, high-strength and high-toughness heat-resistant austenitic alloy steel is used to manufacture containing parts for heat assembly.

Citation Information

Cited By

  • High-toughness large-expansion austenitic stainless steel and preparation method thereof

    CN119800250A

  • Steel with light weight, high heat resistance and good fatigue life as well as preparation method and application of steel