Hot-dip plated steel material
By controlling the crystal orientation of the MgZn2 phase and the α phase in the hot-dip plating layer of the hot-dip plating steel, the problem of insufficient corrosion resistance of the hot-dip plating steel in the prior art and after coating is solved, and better resistance is achieved Corrosive properties.
Patent Information
- Application Number
- CN202411003167.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-01
AI Technical Summary
There are shortcomings in the corrosion resistance of existing hot-dip plated steels in flat surfaces and after coating, especially few studies have taken into account the performance of both.
By controlling the crystal orientation of the MgZn2 phase and the α phase in the hot-dip plating layer, the dense surface is parallel to the surface of the plating layer, and the specific X-ray diffraction intensity ratio relationship is met, so as to improve the corrosion resistance of the flat surface of the plating layer and after coating.
The corrosion resistance of hot-dip plated steel is significantly improved and the after-coating corrosion resistance is achieved, achieving better performance between the two.
Smart Images

Figure BDA0004962204830000181 
Figure BDA0004962204830000191 
Figure BDA0004962204830000201
Abstract
Description
[0001] This application is a divisional application of the invention patent with an application date of March 23, 2023, Chinese patent application number 202380011420.7, and invention name “Hot-dip galvanized steel” (international application No. PCT / JP2023 / 011387 entered the Chinese national stage). Technical Field
[0002] The present invention relates to hot-dip galvanized steel products.
[0003] This application claims priority based on Japanese Patent Application No. 2022-046793 filed in Japan on March 23, 2022, the contents of which are incorporated herein by reference. Background Art
[0004] Steel materials with a hot-dip Zn-plated layer containing Al and Mg formed on the surface (hot-dip Zn-Al-Mg plated steel materials) have excellent corrosion resistance. Therefore, hot-dip Zn-Al-Mg plated steel materials have been widely used as materials for structural members that require corrosion resistance, such as building materials.
[0005] For example, Patent Document 1 describes a hot-dip plated steel sheet comprising a steel sheet and a hot-dip plated layer formed on the surface of the steel sheet, wherein the hot-dip plated layer contains, in average, 0 to 90% by mass of Al and 0 to 10% by mass of Mg, and the remainder contains Zn and impurities, and a pattern portion and a non-pattern portion arranged in a prescribed shape are formed in the hot-dip plated layer, the pattern portion and the non-pattern portion each contain one or two of a first region and a second region, the absolute value of the difference between the area ratio of the first region in the pattern portion and the area ratio of the first region in the non-pattern portion is greater than 30%, the first region is a region with an orientation ratio of greater than 3.5, and the second region is a region with an orientation ratio of less than 3.5.
[0006] Patent document 2 describes a Zn-Al-Mg hot-dip plated steel sheet comprising a steel sheet and a hot-dip plated layer, wherein the hot-dip plated layer contains 4 mass % or more and 22 mass % or less of Al and 1 mass % or more and 5 mass % or less of Mg, the remainder comprising Zn and unavoidable impurities, and the ratio of the X-ray diffraction intensity I(200) of the (200) plane of the Al phase to the X-ray diffraction intensity I(111) of the (111) plane of the Al phase at a cross section of the hot-dip plated layer parallel to the surface of the hot-dip plated layer, i.e., the diffraction intensity ratio I(200) / I(111) is greater than 0.8.
[0007] In recent years, hot-dip galvanized steel materials used for building materials such as roofs and wall materials have been required to have both the corrosion resistance of the coating itself in the uncoated state, i.e., the flat surface corrosion resistance, and the corrosion resistance when coated, i.e., the corrosion resistance after coating. In the prior art, there has been little research on both the flat surface corrosion resistance and the corrosion resistance after coating.
[0008] Patent Document 1 describes that the diffraction peak intensity I of the (0002) plane of the Zn phase is 0002 The diffraction peak intensity I 10-11 In the case where the area with an intensity ratio of 3.5 or more is used as the first area and the area with an intensity ratio of less than 3.5 is used as the second area, by making the difference between the area ratio of the first area in the pattern part and the area ratio of the first area in the non-pattern part be 30% or more, it is possible to intentionally show text, design, etc. on the surface of the coating, but there is no research on the corrosion resistance after painting.
[0009] In Patent Document 2, the orientation of the Al phase in the plating layer is controlled to make the appearance of the plating layer a pear-skin appearance with fine and smooth lines and many glossy portions, but no study is made on corrosion resistance after painting.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2021-85086
[0013] Patent Document 2: International Publication No. 2011 / 001662 Summary of the invention
[0014] Problems to be solved by the invention
[0015] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide a hot-dip plated steel material having both excellent flat surface corrosion resistance and post-painting corrosion resistance.
[0016] Means for solving problems
[0017] In order to solve the above-mentioned problems, the present invention adopts the following configuration.
[0018] [1] A hot-dip plated steel material comprising: a steel material; and a hot-dip plated layer disposed on a surface of the steel material, wherein the chemical composition of the hot-dip plated layer comprises, in terms of mass%, 10.0 to 30.0% Al, 3.0 to 15.0% Mg, 0.01 to 15.0% Fe, 0 to 10.0% Si, 0 to 1.0% Ni, and 0 to 4.0% Ca.
[0019] further containing one or more elements selected from the group consisting of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, and W: 0 to 0.5%, and the total amount of these elements is set to 5% or less,
[0020] The rest: contains Zn and impurities,
[0021] The diffraction intensity of the hot-dip galvanized layer obtained from the X-ray diffraction measurement results satisfies the relationship between the following formulas (1a) and (2a):
[0022] 0.3≤I(002) MgZn2 / {I(100) MgZn2 +I(101) MgZn2}≤3.0(1a)
[0023] 5.0<I(111) α / I(200) α ≤40.0(2a)
[0024] Wherein, I(002) in formula (1a) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(100) MgZn2 is the diffraction intensity of the MgZn2 phase (100), I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase, I(111) in formula (2a) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
[0025] [2] A hot-dip plated steel material comprising: a steel material; and a hot-dip plated layer disposed on a surface of the steel material, wherein the chemical composition of the hot-dip plated layer comprises, in terms of mass%, 15.0 to 30.0% Al, 5.0 to 10.0% Mg, 0.01 to 15.0% Fe, 0 to 10.0% Si, 0 to 1.0% Ni, and 0 to 4.0% Ca,
[0026] further containing one or more elements selected from the group consisting of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, and W: 0 to 0.5%, and the total amount of these elements is set to 5% or less,
[0027] The rest: contains Zn and impurities,
[0028] The diffraction intensity of the hot-dip galvanized layer obtained from the X-ray diffraction measurement results satisfies the relationship between the following formulas (1b) and (2b):
[0029] 0.6<I(002) MgZn2 / {I(100) MgZn2 +I(101) MgZn2}≤3.0(1b)
[0030] 5.0<I(111) α / I(200) α ≤40.0(2b)
[0031] Wherein, I(002) in formula (1b) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(100) MgZn2 is the diffraction intensity of the MgZn2 phase (100), I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase, I(111) in formula (2b) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
[0032] [3] The hot-dip coated steel material according to [1] or [2], wherein Sn in the chemical composition of the hot-dip coated layer is set to Sn: 0.05 to 0.5% by mass, and the Mg2Sn phase is detected by X-ray diffraction measurement results of the hot-dip coated layer.
[0033] Effects of the Invention
[0034] According to the present invention, it is possible to provide a hot-dip plated steel material having both excellent flat surface corrosion resistance and excellent post-painting corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic cross-sectional view of a hot-dip plated steel material as an embodiment of the present invention. DETAILED DESCRIPTION
[0036] Hot-dip plated steel with a coating formed on the surface of the coating sometimes corrodes along the interface between the coating and the coating, and then corrodes in the depth direction of the coating. Moreover, corrosion first occurs at the interface between the coating and the coating, so the coating sometimes expands before the coating is lost due to corrosion. Therefore, in order to improve the corrosion resistance of hot-dip plated steel after painting, it is necessary to suppress the corrosion at the interface between the coating and the coating. In addition, by improving the corrosion resistance after painting, it is expected that the corrosion of the coating itself is also suppressed, thereby improving the corrosion resistance of the flat part.
[0037] Therefore, the inventors of the present invention have conducted in-depth research to improve both the corrosion resistance of the planar portion of the hot-dip Zn-plated layer containing Al and Mg and the corrosion resistance after coating. There are dense planes in the MgZn2 phase and the α phase contained in the coating. The dense plane of the MgZn2 phase with a hexagonal crystal structure is set to the (002) plane. In addition, the dense plane of the α phase containing Al and a small amount of Zn and having a face-centered cubic crystal structure is the (111) plane. Moreover, the MgZn2 phase and the α phase each have the property that the corrosion resistance of the crystal orientation plane corresponding to their dense planes is higher than the corrosion resistance of other crystal orientation planes.
[0038] Therefore, in order to achieve the above-mentioned purpose, the inventors of the present invention have tried to orient the (002) plane as the dense plane of the MgZn2 phase and the (111) plane as the dense plane of the α phase in a manner parallel to the surface of the hot-dip coating. As a result, it was found that the corrosion resistance of such a hot-dip coating after coating is greatly improved, and the corrosion resistance of the flat portion of the hot-dip coating is further improved.
[0039] It was also found that when the X-ray diffraction intensity obtained from the X-ray diffraction measurement results for the surface of the coating satisfies the relationship between the following formula (1a) and the following formula (2), the crystal orientation of the MgZn2 phase and the α phase is oriented in a certain direction, and such a hot-dip coating can improve both the corrosion resistance of the planar portion and the corrosion resistance after painting, thereby completing the present invention.
[0040] Hereinafter, a hot-dip plated steel material which is an embodiment of the present invention will be described.
[0041] The hot-dip plated steel material of the present embodiment comprises: a steel material; and a hot-dip plating layer disposed on the surface of the steel material, wherein the chemical composition of the hot-dip plating layer contains, by mass%, 10.0-30.0% Al, 3.0-15.0% Mg, 0.01-15.0% Fe, 0-10.0% Si, 0-1.0% Ni, 0-1.0% Ca, and further contains 0-0.5% Sb, 0-0.5% Pb, 0-1.0% Cu, 0-2.0% Sn, 0-1.0% Ti, 0-1.0%, 0-1.0% Cr, 0-1.0% Nb, 0-1.0% Zr, 0-1.0% Mn, and 0-1.0% Mo. ~1.0%, Ag: 0~1.0%, Li: 0~1.0%, La: 0~0.5%, Ce: 0~0.5%, B: 0~0.5%, Y: 0~0.5%, P: 0~0.5%, Sr: 0~0.5%, Co: 0~0.5%, Bi: 0~0.5%, In: 0~0.5%, V: 0~0.5%, W: 0~0.5%, and the total amount of these elements is set to 5% or less, and the remainder: contains Zn and impurities, and the diffraction intensity of the hot-dip galvanized layer obtained by the X-ray diffraction measurement result satisfies the relationship between the following formulas (1a) and (2).
[0042] 0.3≤I(002) MgZn2 / {I(100) MgZn2 +I(101) MgZn2}≤3.0(1a)
[0043] 5.0<I(111) α / I(200) α ≤40.0 (2)
[0044] Wherein, I(002) in formula (1a) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(100) MgZn2 is the diffraction intensity of the MgZn2 phase (100), I(101) MgZn2 is the diffraction intensity of (101) of MgZn2 phase, I(111) in formula (2) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
[0045] In addition, when the Al concentration and the Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 15.0 to 30.0% and Mg: 5.0 to 10.0%, respectively, it is preferred that the above formula (2) is satisfied and the following formula (1b) is satisfied instead of satisfying the above formula (1a). Furthermore, when the Al concentration and the Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 10.0 to 30.0% and Mg: 3.0 to 15.0%, respectively, and the range of Al: 15.0 to 30.0% and Mg: 5.0 to 10.0%, it is sufficient to satisfy the above formula (1a). When the Al concentration and the Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 10.0 to 30.0% and Mg: 3.0 to 15.0%, respectively, and the range of Al: 15.0 to 30.0% and Mg: 5.0 to 10.0%, respectively, it is preferred that the above formula (1a) is satisfied and the following formula (1b) is satisfied.
[0046] 0.6<I(002) MgZn2 / {I(100) MgZn2 +I(101) MgZn2}≤3.0(1b)
[0047] In the following description, the "%" of the content of each element in the chemical composition means "mass %". The content of the elements in the chemical composition is sometimes expressed as element concentration (for example, Zn concentration, Mg concentration, etc.). The so-called "flat portion corrosion resistance" refers to the property of the hot-dip coating (specifically, the Zn-Al-Mg alloy layer) itself that is difficult to corrode. The so-called "corrosion resistance after painting" refers to the property of the hot-dip coating itself that is difficult to corrode when a coating is applied to the coating surface. The so-called "hot-dip coating" means a coating film produced by the so-called hot-dip galvanizing process.
[0048] like Figure 1 As shown, the hot-dip galvanized steel material 1 involved in this embodiment has a steel material 11. There is no particular limitation on the shape of the steel material 11, and an example of the steel material 11 is a steel plate. In addition, the steel material 11 may be, for example, a steel pipe, civil engineering materials (fence ditch, corrugated pipe, drainage trough cover, flying sand prevention plate, bolt, wire mesh, guardrail, waterproof wall, etc.), home appliance components (shell of outdoor unit of air conditioner, etc.), automobile parts (travel components, etc.) and other formed base steel materials. Forming processing may be, for example, various plastic processing methods such as pressing, rolling, and bending.
[0049] The material of the steel material 11 is not particularly limited. The steel material 11 may be, for example, general steel, Al-killed steel, ultra-low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steel containing reinforcing elements such as Ni and Cr). The steel material 11 may be a hot-rolled steel sheet, hot-rolled steel strip, cold-rolled steel sheet, and cold-rolled steel strip as described in JIS G 3302:2010. There is no particular limitation on the manufacturing method of the steel sheet (hot rolling method, pickling method, cold rolling method, etc.) and its specific manufacturing conditions.
[0050] In this embodiment, the use of pre-plated steel is not excluded as the steel 11, but it is preferred to use a non-pre-plated steel. As described later, by hot-dip plating on the non-pre-plated steel and controlling the subsequent cooling conditions, it is easy to orient the crystal orientation of the MgZn2 phase and the α phase in a certain direction.
[0051] The hot-dip plated steel material 1 according to the present embodiment has a hot-dip plated layer 12 disposed on the surface of a steel material 11. The hot-dip plated layer 12 of the hot-dip plated steel material 1 according to the present embodiment is mainly composed of a Zn-Al-Mg alloy layer due to the chemical composition described later. In addition, the hot-dip plated layer 12 of the hot-dip plated steel material 1 according to the present embodiment may include an Al-Fe alloy layer between the steel material 11 and the Zn-Al-Mg alloy layer. That is, the hot-dip plated layer 12 may be a single-layer structure of a Zn-Al-Mg alloy layer, or may be a laminated structure including a Zn-Al-Mg alloy layer and an Al-Fe alloy layer.
[0052] The chemical composition of the hot-dip coating involved in this embodiment is composed of Zn and other alloying elements. The chemical composition of the hot-dip coating will be described in detail below. It should be noted that the elements described as having a lower limit of 0% in concentration are not necessary to solve the problem of the hot-dip coated steel material involved in this embodiment, but are optional elements allowed to be contained in the hot-dip coating for the purpose of improving properties.
[0053] <Al: 10.0~30.0%>
[0054] Al forms an α phase as a solid solution with Zn, which helps to improve the corrosion resistance of the flat part, the corrosion resistance after painting, and the processability. Therefore, the Al concentration is set to 10.0% or more. The Al concentration can be set to 11.0% or more, 12.0% or more, or 15.0% or more. On the other hand, in the case of excess Al, the Mg concentration and the Zn concentration are relatively reduced, and the corrosion resistance of the flat part and the corrosion resistance after painting are deteriorated. Therefore, the Al concentration is set to 30.0% or less. The Al concentration can be set to 28.0% or less, 25.0% or less, or 20.0% or less.
[0055] <Mg: 3.0~15.0%>
[0056] Mg is an element required to ensure the corrosion resistance of the flat part and the corrosion resistance after painting. Therefore, the Mg concentration is set to 3.0% or more. The Mg concentration can be set to 4.0% or more, 5.0% or more, or 6.0% or more. On the other hand, if the Mg concentration is excessive, the processability, especially the crushing property, deteriorates, and sometimes the corrosion resistance of the flat part and the corrosion resistance after painting deteriorate. Therefore, the Mg concentration is set to 15.0% or less. The Mg concentration can be set to 12.0% or less, 10.0% or less, or 8.0% or less.
[0057] <Fe: 0.01%~15.0%>
[0058] The concentration of Fe may be 0%. On the other hand, the hot-dip coating may contain 0.01% or more of Fe. It has been confirmed that if the Fe concentration is 15.0% or less, there is no adverse effect on the performance of the hot-dip coating. The Fe concentration may be, for example, 0.05% or more, 0.10% or more, 0.5% or more, or 1.0% or more. The Fe concentration may be, for example, 10.0% or less, 8.0% or less, or 6.0% or less. Fe is sometimes mixed in from the base steel plate, so the Fe concentration may be 0.05% or more.
[0059] <Si: 0%~10.0%>
[0060] The Si concentration may be 0%. On the other hand, Si contributes to the improvement of the corrosion resistance of the planar portion. Therefore, the Si concentration may be 0.05% or more, 0.1% or more, 0.2% or more, or 0.5% or more. On the other hand, if the Si concentration is excessive, the corrosion resistance of the planar portion and the corrosion resistance after painting deteriorate. Therefore, the Si concentration is set to 10.0% or less. The Si concentration may be 8.0% or less, 7.0% or less, or 6.0% or less.
[0061] <Ni: 0~1.0%>
[0062] The concentration of Ni may be 0%. On the other hand, Ni contributes to the improvement of the corrosion resistance of the flat part and the corrosion resistance after painting. Therefore, the Ni concentration may be 0.05% or more, 0.08% or more, or 0.1% or more. On the other hand, if the Ni concentration is excessive, the corrosion resistance of the flat part and the corrosion resistance after painting deteriorate. Therefore, the Ni concentration is set to 1.0% or less. The Ni concentration may be 0.8% or less, 0.6% or less, or 0.5% or less.
[0063] <Ca: 0%~4.0%>
[0064] The Ca concentration may be 0%. On the other hand, Ca is an element that can adjust the amount of Mg dissolved that is most suitable for imparting corrosion resistance to the planar portion. Therefore, the Ca concentration may be 0.05% or more, 0.1% or more, or 0.5% or more. On the other hand, if the Ca concentration is excessive, the corrosion resistance and workability of the planar portion deteriorate. Therefore, the Ca concentration is set to 4.0% or less. The Ca concentration may be set to 3.5% or less, 3.0% or less, or 2.8% or less.
[0065] Furthermore, the hot-dip galvanized layer involved in the present embodiment may contain one or more elements selected from the group consisting of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, and W: 0 to 0.5%. The total amount of these elements is set to be 0% or more and 5% or less. If the total amount exceeds 5%, the flat surface corrosion resistance or the corrosion resistance after painting may be reduced.
[0066] <Sb, Pb: 0 to 0.5% each>
[0067] The concentration of Sb and Pb may be 0%. On the other hand, Sb and Pb contribute to the improvement of corrosion resistance after coating. Therefore, the concentration of each of Sb and Pb may be 0.05% or more, 0.10% or more, or 0.15% or more. On the other hand, if the concentration of Sb and Pb is excessive, the corrosion resistance of the flat portion deteriorates. Therefore, the concentration of each of Sb and Pb is 0.5% or less. The concentration of each of Sb and Pb may be 0.4% or less, 0.3% or less, or 0.25% or less.
[0068] <Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li: 0 to 1.0% each>
[0069] The concentration of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li may be 0% each. On the other hand, these elements contribute to the improvement of corrosion resistance after painting. Therefore, the concentration of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li may be 0.05% or more, 0.08% or more or 0.10% or more. On the other hand, if the concentration of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li is excessive, the corrosion resistance of the plane portion deteriorates. Therefore, the concentration of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li may be 1.0% or less. The concentration of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li may be 0.8% or less, 0.7% or less or 0.6% or less.
[0070] <Sn: 0~2.0%>
[0071] The Sn concentration may be 0%. On the other hand, Sn is an element that forms an intermetallic compound with Mg and improves the corrosion resistance of the hot-dip coating after coating. Therefore, the Sn concentration may be 0.05% or more, 0.10% or more, 0.20% or more, or 0.30% or more. However, if the Sn concentration is excessive, the corrosion resistance of the flat portion deteriorates. Therefore, the Sn concentration is set to 2.0% or less. The Sn concentration may be set to 0.8% or less, 0.7% or less, 0.6% or less, or 0.5% or less.
[0072] <La, Ce, B, Y, P and Sr: 0 to 0.5% each>
[0073] The concentration of each of La, Ce, B, Y, P and Sr may be 0%. On the other hand, La, Ce, B, Y, P and Sr contribute to the improvement of corrosion resistance after painting. Therefore, the concentration of each of La, Ce, B, Y, P and Sr may be 0.10% or more, 0.15% or more or 0.20% or more. On the other hand, if the concentration of La, Ce, B, Y, P and Sr is excessive, the corrosion resistance of the plane portion deteriorates. Therefore, the concentration of each of La, Ce, B, Y, P and Sr is 0.5% or less. The concentration of each of La, Ce, B, Y, P and Sr may be 0.4% or less, 0.3% or less.
[0074] <Co, Bi, In, V, W: 0 to 0.5% each>
[0075] The concentration of each of Co, Bi, In, V, and W may be 0%. On the other hand, Co, Bi, In, V, and W contribute to the improvement of corrosion resistance after painting. Therefore, the concentration of each of Co, Bi, In, V, and W may be 0.10% or more, 0.15% or more, or 0.20% or more. On the other hand, if the concentration of Co, Bi, In, V, and W is excessive, the corrosion resistance of the planar portion deteriorates. Therefore, the concentration of each of Co, Bi, In, V, and W is 0.5% or less. The concentration of each of Co, Bi, In, V, and W may be 0.4% or less, or 0.3% or less.
[0076] <Remainder: Zn and impurities>
[0077] The remainder of the components of the hot-dip coating involved in this embodiment is Zn and impurities. Zn is an element that brings corrosion resistance to the flat surface and corrosion resistance after coating to the hot-dip coating. Impurities are components contained in the raw materials or components mixed in the manufacturing process, and refer to components that are not intentionally contained. For example, in the hot-dip coating, due to the mutual atomic diffusion between the steel material and the coating bath, components other than Fe are sometimes mixed in trace amounts as impurities.
[0078] The chemical composition of the hot-dip coating is determined by the following method. First, an acid containing an inhibitor that inhibits the corrosion of steel is used to obtain an acid solution that can strip and dissolve the hot-dip coating. Secondly, the obtained acid solution is subjected to inductively coupled plasma (ICP) analysis. In this way, the chemical composition of the hot-dip coating can be obtained. There is no particular restriction on the acid type as long as it is an acid that can dissolve the hot-dip coating. In addition, the chemical composition determined by the above-mentioned means is the average chemical composition of the entire hot-dip coating.
[0079] Next, the metal structure of the hot-dip galvanized layer will be described.
[0080] The metal structure of the hot-dip coating contains an α phase and a MgZn2 phase. The α phase and the MgZn2 phase improve the corrosion resistance of the flat portion of the hot-dip coating. In addition, as described later, the corrosion resistance of the hot-dip coated steel material after coating is improved by orienting the α phase and the MgZn2 phase in a certain direction, and the corrosion resistance of the flat portion is also improved.
[0081] The area ratio of the α phase in the hot-dip galvanized layer is preferably 15 to 80%. In addition, the area ratio of the MgZn2 phase is preferably 5 to 60%. The combined area ratio of the α phase and the MgZn2 phase is preferably 20% or more and 100% or less. However, the range of the area ratio is an example, and the area ratio of the structure of the hot-dip galvanized layer of the present invention is not limited to any of the ranges, as long as the hot-dip galvanized layer satisfies at least one of the formulas (1a) and (1b) described below and formula (2).
[0082] In addition, when the hot-dip coating contains 0.05 to 0.5% Sn, the hot-dip coating will reliably contain the Mg2Sn phase. Since the Mg2Sn phase is a small amount, its presence is confirmed by X-ray diffraction measurement. By containing the Mg2Sn phase in the hot-dip coating, the corrosion resistance of the hot-dip coating after coating is further improved.
[0083] The hot-dip coating may contain phases other than the α phase and the MgZn2 phase as the remainder. For example, the hot-dip coating of the above chemical composition may contain η-Zn phase, Al-Ca-Si phase, etc. If the content of the α phase and the MgZn2 phase is within the above range, the corrosion resistance of the plane part and the corrosion resistance after coating can be ensured, so there is no particular limitation on the composition of the phases or structures other than the α phase and the MgZn2 phase.
[0084] Next, the crystal orientations of the α phase and the MgZn2 phase are described.
[0085] In the hot-dip coating of the present embodiment, when the X-ray diffraction intensity of the hot-dip coating obtained from the X-ray diffraction measurement results satisfies the relationship between the following formulas (1a) and (2), as described later, the crystal orientation of the MgZn2 phase and the α phase will be oriented in a certain direction, and the corrosion resistance and flat surface corrosion resistance after coating will be improved.
[0086] 0.3≤I(002) MgZn2 / {I(100) MgZn2 +I(101) MgZn2}≤3.0(1a)
[0087] 5.0<I(111) α / I(200) α ≤40.0 (2)
[0088] In addition, when the Al concentration and the Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 15.00-30.00% and Mg: 5.00-10.00%, respectively, it is preferred that the following formula (1b) is satisfied in addition to the above formula (2) instead of satisfying the above formula (1a). Furthermore, when the Al concentration and the Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 10.0-30.0% and Mg: 3.0-15.0%, respectively, and when the Al concentration and the Mg concentration are in the range of Al: 15.0-30.0% and Mg: 5.0-10.0%, respectively, it is sufficient to satisfy the above formula (1a). In the chemical composition of the hot-dip galvanized layer, when the Al concentration and the Mg concentration satisfy the ranges of Al: 10.0-30.0% and Mg: 3.0-15.0%, respectively, and satisfy the ranges of Al: 15.0-30.0% and Mg: 5.0-10.0%, it is preferred to satisfy the above formula (1a), and it is further preferred to satisfy the following formula (1b).
[0089] 0.6<I(002) MgZn2 / {I(100) MgZn2 +I(101) MgZn2}≤3.0(1b)
[0090] Among them, I(002) in formula (1a) and formula (1b) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(100) MgZn2 is the diffraction intensity of the MgZn2 phase (100), I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase. In addition, I(111) in formula (2) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
[0091] As shown in formula (1a), through I (100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2} becomes 0.3 or more, so that the dense surface of the MgZn2 phase, that is, the (002) plane, is oriented parallel to the surface of the hot-dip galvanized layer. Preferably, when the Al concentration is 15.0 to 30.0% and the Mg concentration is 5.0 to 10.0%, it is preferably greater than 0.6 as shown in formula (1b). I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2 The higher the value of MgZn2, the more the dense plane of the MgZn2 phase, i.e., the (002) plane, is parallel to the surface of the hot-dip galvanized layer.
[0092] On the other hand, I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2 The upper limit of} is set to be 3.0 or less. Even if the orientation of the dense plane of the MgZn2 phase is increased to the maximum, the upper limit is 3.0.
[0093] In addition, through I(111) in formula (2) α / I(200) α When the ratio is greater than 5.0, the (111) plane, which is the dense plane of the α phase, is oriented parallel to the surface of the hot-dip galvanized layer. α / I(200) α The higher the value, the more the dense plane of the α phase, that is, the (111) plane, is parallel to the surface of the hot-dip galvanized layer.
[0094] On the other hand, I(111) α / I(200) α The upper limit is set to 40.0 or less. Even if the orientation of the dense plane of the α phase is increased to the maximum, the upper limit is 40.0.
[0095] It is presumed that the reason why the corrosion resistance after coating and the corrosion resistance of the flat surface of the hot-dip coating layer satisfying the above formula (1a) or (1b) and (2) are improved is due to the following reasons.
[0096] The dense plane of the MgZn2 phase having a hexagonal crystal structure is set to the (002) plane. In addition, the dense plane of the α phase containing Al and a small amount of Zn and having a face-centered cubic crystal structure is set to the (111) plane. The MgZn2 phase and the α phase each have the property of high corrosion resistance of the crystal orientation plane corresponding to their dense planes and high corrosion resistance of other crystal orientation planes. The dense planes of the MgZn2 phase and the α phase of the hot-dip galvanized layer that satisfies at least one of the above-mentioned formulas (1a) and (1b) and (2) are oriented parallel to the surface of the hot-dip galvanized layer.
[0097] In hot-dip coated steel materials in which a coating is formed on the surface of the hot-dip coating, corrosion sometimes proceeds along the interface between the coating and the coating. It is believed that the respective dense planes of the MgZn2 phase and the α phase in the hot-dip coating are oriented in parallel with the surface of the hot-dip coating, thereby significantly improving the corrosion resistance of the interface between the hot-dip coating and the coating, and greatly improving the corrosion resistance after coating.
[0098] In addition, in hot-dip coated steel, corrosion sometimes proceeds from the surface of the hot-dip coating. It is believed that the corrosion resistance of the surface of the hot-dip coating is significantly improved by orienting the respective dense surfaces of the MgZn2 phase and the α phase parallel to the surface of the hot-dip coating as described above, and the corrosion resistance of the flat portion is also greatly improved.
[0099] The method for determining the area ratio of the MgZn2 phase is as follows. The surface of the hot-dip coating of a sample cut into 30 mm × 30 mm is adjusted to be flat by mechanical grinding (for example, grinding with sandpaper #2000). Secondly, the surface of the coating is chemically polished by colloidal grinding until the surface becomes a mirror surface. The surface of the polished coating is observed with a scanning electron microscope (SEM). Specifically, an element distribution image is taken using a scanning electron microscope-energy dispersive spectrometer (SEM-EDS) at a magnification of 5000 times. In this element distribution image, the phase in which Mg and Zn coexist is determined to be the MgZn2 phase. Furthermore, in this specification, the area of Mg: 20 to 40 atomic % and Zn: 50 to 80 atomic % is judged as the phase in which Mg and Zn coexist (MgZn2 phase). After the MgZn2 phase is determined, the area ratios of the α phase and the MgZn2 phase contained in the field of view are calculated by binarization using image analysis software.
[0100] The method for determining the area ratio of the α phase is as follows. The surface of the hot-dip coating of a sample cut into 30 mm × 30 mm is adjusted to be flat by mechanical grinding. Secondly, the surface of the coating is chemically polished by colloidal polishing until the surface becomes a mirror surface. The surface of the polished coating is observed by SEM. Specifically, the element distribution image is photographed using SEM-EDS at a magnification of 5000 times. In this element distribution image, the phase in which Al and Zn coexist is determined to be the α phase. Furthermore, in this specification, the area of Al: 40 to 95 atomic % and Zn: 0.5 to 50 atomic % will be judged as the phase in which Al and Zn coexist (α phase). After the α phase is determined, the area ratio of the α phase contained in the field of view is calculated by binarization using image analysis software.
[0101] I(002) in formula (1a) and formula (1b) MgZn2 / {I(100) MgZn2 +I(101) MgZn2 The method for determining the} is as follows. First, the surface of the hot-dip galvanized layer is mirror-polished and chemically polished as needed. Next, for example, an X-ray diffraction device (Rigaku Corporation (model RINT-TTR III), set to X-ray output 50kV, 300mA, copper target, goniometer TTR (horizontal goniometer), Kβ filter slit width 0.05mm, longitudinal limiting slit width 2mm, light receiving slit width 8mm, light receiving slit 2 open, as measurement conditions, at a scanning speed of 5 degrees / minute, a step width of 0.01 degrees, and a scanning axis of 2θ (5~90°), perform X-ray diffraction measurement. Then, the diffraction intensity of the (100) plane of the MgZn2 phase (maximum intensity in the range of 19.67±0.2°), the diffraction intensity of the (002) plane (maximum intensity in the range of 20.78±0.2°), and the diffraction intensity of the (101) plane (maximum intensity in the range of 22.26±0.2°) are measured respectively. The diffraction intensity is set to the intensity excluding the background intensity. I(002) is calculated from the obtained diffraction intensity. MgZn2 / {I(100) MgZn2 +I(101) MgZn2}.
[0102] I(111) in formula (2) α / I(200) αThe measurement method is as follows. First, the surface of the hot-dip galvanized layer is mirror-polished and, if necessary, chemically polished. Next, for example, an X-ray diffraction device and measurement conditions are the same as those described above, and an X-ray diffraction measurement is performed. Then, the diffraction intensity of the (111) plane of the α phase (maximum intensity in the range of 38.47±0.2°) and the diffraction intensity of the (200) plane (maximum intensity in the range of 44.74±0.2°) are measured respectively. The diffraction intensity is set to the intensity excluding the background intensity. I(111) is calculated from the obtained diffraction intensity. α / I(200) α .
[0103] In addition, whether the hot-dip galvanized layer contains a Mg2Sn phase is determined by whether a diffraction peak specific to Mg2Sn appears during the above-mentioned X-ray diffraction measurement.
[0104] The coating weight per single side of the hot-dip coating layer can be set to, for example, 20 to 150 g / m 2 By setting the adhesion amount per single side to 20g / m 2 On the other hand, by setting the coating weight per single surface to 150 g / m 2 As a result, the workability of the hot-dip plated steel material can be further improved.
[0105] Next, a method for producing the hot-dip plated steel material according to the present embodiment will be described. The method for producing the hot-dip plated steel material according to the present embodiment is not particularly limited. For example, the hot-dip plated steel material according to the present embodiment can be obtained according to the production conditions described below.
[0106] The method for manufacturing hot-dip plated steel of the present embodiment forms a hot-dip coating on the surface of the steel by annealing the steel in a reducing atmosphere, immersing the annealed steel in a hot-dip coating bath, and then pulling it out. Next, cooling gas is sprayed while the temperature of the hot-dip coating decreases from the bath temperature to 300° C. or less to cool the hot-dip coating.
[0107] Specifically, the steel material to be plated is annealed in a reducing atmosphere. The reducing atmosphere and annealing conditions are not particularly limited. Through this annealing, oxides existing on the surface of the steel material are removed as much as possible.
[0108] Next, the steel material immediately after annealing is immersed in a hot dip coating bath. The chemical composition of the hot dip coating bath can be appropriately adjusted so as to obtain the chemical composition of the hot dip coating layer described above. In addition, the temperature of the hot dip coating bath is not particularly limited, and a temperature that can perform hot dip coating can be appropriately selected. For example, the coating bath temperature can be set to a value that is about 20°C higher than the melting point of the coating bath.
[0109] Next, the steel material is lifted from the hot dip coating bath. By controlling the lifting speed of the steel material, the amount of hot dip coating can be controlled. If necessary, the steel material to which the hot dip coating is attached can be wiped to control the amount of hot dip coating. There is no particular limitation on the amount of hot dip coating, and for example, it can be within the above range.
[0110] Next, the hot dip coating is cooled. For cooling, the steel material is cooled by spraying cooling gas just after being pulled out of the hot dip coating bath. Cooling by spraying cooling gas is continuously performed while the temperature of the hot dip coating layer increases from the bath temperature to 300°C. There is no particular limitation on the cooling conditions below 300°C, and cooling by spraying cooling gas may be performed subsequently, or cooling may be performed naturally.
[0111] The cooling start temperature is above -40°C and below the temperature of the hot dip coating bath. If the cooling start temperature is lower than -40°C, the coating is cooled (for example, the cooling rate is 2°C / s) until the cooling starts. Therefore, a large number of nuclei are formed in the hot dip coating before the hot dip coating is cooled. Therefore, it becomes difficult to control the orientation of the α phase and the MgZn2 phase in the hot dip coating in the subsequent steps.
[0112] For cooling by spraying cooling gas, a cooling belt is arranged along the conveying path of the steel material. The cooling belt is equipped with a plurality of spray nozzles for cooling gas. By setting the flux to 5000 L / min / m 2 Above, the hot dip coating can be cooled to below 300°C in a relatively short time. 2 In the case of , the cooling gas flow rate is reduced while maintaining the cooling rate of the entire steel material, thereby reducing the cooling gas temperature. As a result, the liquid phase on the surface of the coating is overcooled and becomes a solidification nucleus, the crystallization increases, and the orientation control becomes impossible. In addition, by setting the flux to 25000L / min / m 2 Hereinafter, the steel material can be cooled without applying vibration.
[0113] The cooling gas to be sprayed is not particularly limited, and may be a non-oxidizing gas such as nitrogen, an inert gas such as argon, or air, or a mixed gas thereof.
[0114] When the flux of the cooling gas is controlled, the shape of the gas nozzle from which the cooling gas is ejected is set, for example, to a range of 1 to 50 mm in diameter. The angle between the tip of the gas nozzle and the surface of the steel plate is, for example, in the range of 70 to 110°, and is more preferably set to 90° (right angle). The distance between the tip of the gas nozzle and the steel plate is set to a range of 30 to 1000 mm. The shape, angle, and distance of the gas nozzle are merely examples and are not limited to the above ranges.
[0115] By cooling the hot-dip coating layer so as to satisfy the above conditions, a hot-dip coating layer satisfying at least one of the above formulas (1a) and (1b) and formula (2) can be formed. The reason for this is presumably as follows.
[0116] In the above-mentioned manufacturing method, the steel material is annealed in a reducing atmosphere just before being immersed in the hot dip bath to remove oxides on the surface of the steel material, thereby reducing the number of nucleation sites. When such a steel material is hot dipped, Fe in the steel material reacts with Al in the hot dip bath to form an Al-Fe alloy layer on the surface of the steel material. The Al-Fe alloy layer has fewer nucleation sites. Furthermore, after hot dip galvanizing, the steel material is heated at 5000 L / min / m 2 Above and 25000L / min / m 2 The cooling gas is sprayed at the following fluxes to cool the steel material, and the generation of nucleation sites is further suppressed by minimizing vibrations to the steel material. It is thus inferred that the α phase and MgZn2 phase in the hot-dip coating are oriented in a certain direction to satisfy the above formula (1a) or (1b), and formula (2).
[0117] Example
[0118] The following is an explanation of the embodiments of the present invention. However, the conditions in the embodiments are only a conditional example adopted to confirm the feasibility and effect of the present invention. The present invention is not limited to this conditional example. As long as the purpose of the present invention is achieved without departing from the gist of the present invention, various conditions can be adopted.
[0119] The steel material annealed under the conditions of N2-4% H2 atmosphere, soaking temperature of 800°C, soaking time of 2 minutes was immersed in various hot dip coating baths and pulled up, so that the hot dip coating layer was attached to the surface of the steel material. Then, from just after being pulled up from the hot dip coating bath until the hot dip coating layer reached 300°C, it was cooled by spraying cooling gas, thereby manufacturing various hot dip coated steel materials. When the cooling gas was sprayed, the gas flux was controlled as shown in Table 2. The shape of the gas nozzle for spraying the cooling gas was: the diameter was 6 mm, the angle between the tip of the gas nozzle and the steel plate was a right angle, and the distance between the tip of the gas nozzle and the steel plate was set to 35 mm.
[0120] The chemical composition of the hot-dip plated layer is shown in Table 1. The manufacturing conditions are shown in Table 2. In addition, the metal structure of the plated layer was evaluated, and the results are shown in Table 2. Furthermore, the surface corrosion resistance and post-painting corrosion resistance of the hot-dip plated steel material were evaluated, and the results are shown in Table 3.
[0121] The chemical composition of the hot-dip coating and the metal structure of the hot-dip coating were evaluated by the above-mentioned means.
[0122] The evaluation of the flat part corrosion resistance is as follows. The obtained hot-dip galvanized steel material is cut into 100 mm × 50 mm and provided for the flat part corrosion resistance evaluation test. The evaluation of the flat part corrosion resistance is carried out by the corrosion promotion test specified in JASO-CCT-M609, and is carried out by comparing the corrosion loss after 120 cycles. The evaluation criteria are as follows, and "AAA", "AA" and "A" are set as qualified.
[0123] AAA: Corrosion loss is less than 40g / m 2
[0124] AA: Corrosion loss is 40g / m 2 Above and less than 60g / m 2
[0125] A: Corrosion loss is 60g / m 2 Above and less than 80g / m 2
[0126] B: Corrosion loss is 80g / m 2 above
[0127] The evaluation of corrosion resistance after painting (peeling of coating after painting) is as follows. The obtained hot-dip galvanized steel material was cut into 100mm×50mm and provided for corrosion resistance test after painting. For the test piece, a chemical conversion treatment layer with a film thickness of 1.2μm and a coating layer with a film thickness of 20μm were formed. Then, a cut reaching the base metal was applied to the front side with a cutting knife, and CCT with SST 4 hours → drying 2 hours → wetting 2 hours as one cycle was performed for 120 cycles and evaluated. The maximum expansion width on one side of the cut after the test was used for judgment. The details of the chemical conversion treatment layer and the coating layer are as follows.
[0128] <Chemical treatment layer>
[0129] A chemical conversion treatment film is formed by applying a chromate-free chemical conversion treatment solution prepared by mixing a silane coupling agent, tannic acid, silica, and a polyester resin to the plated layer and drying the solution.
[0130] <Coating layer>
[0131] The primer resin and topcoat resin described below were applied on the chemical conversion film to form coating layers. The thickness of the layer formed by the primer resin was 5 μm, and the thickness of the layer formed by the topcoat resin was 15 μm, for a total of 20 μm.
[0132] <Film-forming components of the coating layer>
[0133] (1) Primer coating resin for front and back surfaces
[0134] Polyester / melamine + isocyanate combined curing type (FLC687 coating resin manufactured by Japan Fine Coatings Co., Ltd.)
[0135] (2) Front surface paint resin
[0136] High molecular weight polyester / melamine curing type (FLC7000 coating resin manufactured by Japan Fine Coatings Co., Ltd.)
[0137] (3) Back side topcoat resin
[0138] Polyester / melamine curing type (FLC100HQ coating resin manufactured by Japan Fine Coatings Co., Ltd.)
[0139] The evaluation criteria for corrosion resistance after painting are shown below. Judgment is made by the following scoring. "AAA", "AA" and "A" are set as pass.
[0140] AAA: Maximum expansion width is less than 5mm
[0141] AA: Maximum expansion width is 5 mm or more and less than 8 mm
[0142] A: The maximum expansion width is more than 8mm and less than 10mm
[0143] B: Maximum expansion width is more than 10mm
[0144] The chemical composition and metal structure of the hot-dip coating layer are appropriately controlled. The No. 1 to 25 (Examples) of the present invention are excellent in both flat surface corrosion resistance and post-coating corrosion resistance. It should be noted that the adhesion amount of the hot-dip coating layer of the Examples is 20 to 150 g / m 2 range.
[0145] In No. 26 of the comparative example, the Al content of the hot-dip coating layer was insufficient. Therefore, in No. 26, the flat surface corrosion resistance was insufficient.
[0146] In No. 27 of the comparative example, the amount of Al in the hot-dip coating was excessive, so that in No. 27, the corrosion resistance after painting was insufficient.
[0147] In No. 28 of the comparative example, the amount of Mg in the hot-dip coating was insufficient. Therefore, in No. 28, both the flat surface corrosion resistance and the post-painting corrosion resistance were insufficient.
[0148] In No. 29 of the comparative example, the amount of Mg in the hot-dip coating was excessive, so the corrosion resistance of the flat surface portion of No. 29 was insufficient.
[0149] In No. 30 of the comparative example, the amount of Si in the hot-dip coating layer was excessive, so that in No. 30, both the flat surface corrosion resistance and the post-painting corrosion resistance were insufficient.
[0150] In No. 31 of the comparative example, the amount of Sn in the hot-dip coating layer was excessive, so that in No. 31, both the flat surface corrosion resistance and the post-painting corrosion resistance were insufficient.
[0151] In No. 32 of the comparative example, the Ca content of the hot-dip coating layer was excessive. Therefore, in No. 30, both the flat surface corrosion resistance and the post-painting corrosion resistance were insufficient.
[0152] In the comparative example No. 33, the gas flux of the cooling gas was insufficient. Therefore, in No. 33, the α phase and the MgZn2 phase were not oriented in a certain direction. Therefore, in No. 33, both the flat surface corrosion resistance and the corrosion resistance after painting were insufficient.
[0153] In the comparative example No. 34, the gas flux of the cooling gas is excessive. Therefore, in No. 34, the α phase and the MgZn2 phase are not oriented in a certain direction. Therefore, in No. 34, both the flat part corrosion resistance and the corrosion resistance after coating are insufficient. If the comparative example No. 34 is compared with the examples No. 12, 22, and 23, although the cooling rates of the two are relatively close, the gas flux of No. 34 is excessive, so it fails to meet the scope of the invention.
[0154] In the comparative examples No. 35 and No. 36, the gas flux of the cooling gas was insufficient and the cooling gas temperature was too low, so that the liquid phase on the surface of the coating was overcooled, forming a large number of solidification nuclei. Therefore, in No. 35 and No. 36, the α phase and the MgZn2 phase were not oriented in a certain direction. As a result, in No. 35 and No. 36, both the corrosion resistance of the flat part and the corrosion resistance after coating were insufficient.
[0155] In the comparative example No. 37, the cooling start temperature was too low, and a large number of nuclei were generated. Therefore, in No. 37, the α phase and the MgZn2 phase were not oriented in a certain direction. Therefore, in No. 37, both the flat part corrosion resistance and the corrosion resistance after painting were insufficient.
[0156] Table 1
[0157]
[0158] The underlined part indicates that it is outside the scope of the present invention.
[0159] Table 2
[0160]
[0161] The underlined part indicates that it is outside the scope of the present invention.
[0162] Table 3
[0163]
[0164] The underlined part indicates that it is outside the scope of the present invention.
[0165] Industrial Applicability
[0166] According to the above aspect of the present invention, both the plane corrosion resistance and the sacrificial corrosion resistance are excellent, and therefore the industrial applicability is high.
Claims
1. A hot-dip plated steel material, comprising: a steel material; and a hot-dip plated layer disposed on a surface of the steel material, wherein the chemical composition of the hot-dip plated layer comprises, in mass%, 10.0 to 30.0% Al, 4.0 to 15.0% Mg, 0.01 to 15.0% Fe, 0 to 10.0% Si, 0 to 1.0% Ni, and 0 to 4.0% Ca, further containing one or more elements selected from the group consisting of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, and W: 0 to 0.5%, and the total amount of these elements is set to 5% or less, The rest: contains Zn and impurities, The diffraction intensity of the hot-dip galvanized layer obtained from the X-ray diffraction measurement results satisfies the relationship between the following formulas (1a) and (2a): 0.3≤I(002) MgZn2 / {I(100) MgZn2 +I(101) MgZn2 }≤3.0(1a) 5.0<I(111) α / I(200) α ≤40.0(2a) in, I(002) in formula (1a) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(100) MgZn2 is the diffraction intensity of the MgZn2 phase (100), I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase, I(111) in formula (2a) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
2. The hot-dip galvanized steel material according to claim 1, wherein: The Mg content in the chemical composition of the hot-dip coating layer is set to Mg: 5.0 to 15.0% by mass.
3. The hot-dip galvanized steel material according to claim 1, wherein: The Mg content in the chemical composition of the hot-dip coating layer is set to Mg: 6.0 to 15.0% by mass%.
4. A hot-dip plated steel material, comprising: a steel material; and a hot-dip plated layer disposed on a surface of the steel material, wherein the chemical composition of the hot-dip plated layer comprises, by mass%, 12.0 to 30.0% Al, 3.0 to 15.0% Mg, 0.01 to 15.0% Fe, 0 to 10.0% Si, 0 to 1.0% Ni, and 0 to 4.0% Ca, further containing one or more elements selected from the group consisting of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, and W: 0 to 0.5%, and the total amount of these elements is set to 5% or less, The rest: contains Zn and impurities, The diffraction intensity of the hot-dip galvanized layer obtained from the X-ray diffraction measurement results satisfies the relationship between the following formulas (1a) and (2a): 0.3≤I(002) MgZn2 / {I(100) MgZn2 +I(101) MgZn2 }≤3.0(1a) 5.0<I(111) α / I(200) α ≤40.0(2a) in, I(002) in formula (1a) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(100) MgZn2 is the diffraction intensity of the MgZn2 phase (100), I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase, I(111) in formula (2a) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
5. The hot-dip galvanized steel material according to claim 4, wherein: The Al content in the chemical composition of the hot-dip coating layer is set to be 15.0 to 30.0% by mass.