Excellent ALD coating process
By adopting the ALD coating process of TMA+H2O+O3 on silicon-based solar cells, the problem of insufficient oxidation in the single oxygen source process is solved, low resistivity and efficient passivation effects are achieved, and the conversion efficiency of solar cells is improved.
Patent Information
- Application Number
- CN202411308090.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-08
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, when preparing alumina films, the single oxygen source process has problems such as insufficient oxidation, resulting in high resistivity and slow deposition rate, which is difficult to meet the needs of improving the efficiency of silicon-based solar cells.
The ALD coating process using TMA+H2O+O3 as the growth source is used to grow an alumina film layer on the substrate, and the gas flow sequence and flow rate are controlled through alternating pulses, and the film resistivity is reduced and the deposition rate is increased.
It achieves low resistivity and efficient passivation effects, improves the conversion efficiency of solar cells, and is simple to operate and low cost.
Abstract
Description
[0001] This application is a divisional application. The application number of the parent application is 202210363758.6, the application date is April 8, 2022, and the name of the invention is “An excellent ALD coating process”. Technical Field
[0002] The invention relates to the technical field of solar cells, and in particular to an excellent ALD coating process. Background Art
[0003] Improving the efficiency of silicon-based solar cells is the main problem people are facing now. Surface passivation is a method to improve the efficiency of silicon-based solar cells. Among the many passivation film materials, Al 2 O 3 Due to the large amount of fixed negative charge and low interface state density at its interface, it is considered to be a natural surface passivation material for solar cells. Obtaining more efficient cells places higher demands on the passivation effect.
[0004] However, the existing technology for preparing alumina uses a single oxygen source, such as TMA and H 2 O or TMA and O 3 However, there are many disadvantages of using a single oxygen source to prepare aluminum oxide films: for example, TMA and H 2 O prepared aluminum oxide film, due to the weak oxidizing property of water, the resistivity of aluminum oxide film is relatively low compared with TMA and O 3 The prepared oxide film is higher; while TMA and O 3 The deposition rate of the prepared aluminum oxide film is relatively high compared with that of TMA and H 2 O deposition rate is slow.
[0005] Therefore, it is necessary to provide a new technical solution to overcome the above-mentioned defects. Summary of the invention
[0006] The object of the present invention is to provide an excellent ALD coating process which can effectively solve the above-mentioned technical problems.
[0007] In order to achieve the purpose of the present invention, the following technical scheme is adopted:
[0008] An excellent ALD coating process, which uses TMA+H 2 O+O 3 As a growth source, an aluminum oxide film layer is grown on the substrate.
[0009] Preferably, the steps of growing an aluminum oxide film layer on a substrate using this process are:
[0010] (1) placing the growth substrate into the chamber of the deposition equipment and controlling the chamber temperature to 170-250° C.;
[0011] (2) Using alternating pulses to generate TMA+H 2 O is the growth source to grow aluminum oxide on the growth substrate surface; the order of gas introduction in each cycle is TMA gas, purge gas, H 2 OEvaporation gas, purge gas;
[0012] (3) After each cycle or after several cycles, the auxiliary gas O 3 Into the cavity, and finally into the purge gas to purge the TMA.
[0013] Preferably, in each cycle of step (2), the flow rate of TMA is 10-30 sccm, the pulse duration is 1-5 s, and the purge duration is 4-9 s.
[0014] Preferably, in each cycle of step (2), H 2 The O flow rate is 10-30 sccm, the pulse duration is 3-10 s, and the purge duration is 6-12 s.
[0015] Preferably, in step (3), the single auxiliary source O 3 The flow rate is 10-30sccm, the pulse duration is 3-20s, and the purge duration is 5-20s.
[0016] Preferably, the purge gas is an inert gas.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention uses ALD (atomic layer deposition) process to prepare Al on the surface of silicon wafer 2 O 3 Thin film, using TMA+H 2 O+O 3 As a growth source, an aluminum oxide film is grown on a substrate, which is different from the prior art method of using TMA+O 3 or TMA+H 2 Compared with the aluminum oxide film grown with O as the growth source, it not only retains TMA+H 2 O has a fast growth rate; and during the growth process, O 3 As an auxiliary source, O 3 Can react with -CH 3 The final reaction is H 2 O+CO 2 and is purged out by the purge gas, thereby effectively reducing the resistivity of the film layer, improving the passivation effect, and thus improving the conversion efficiency of the battery; at the same time, the process of the present invention can be realized in the same chamber, and has the advantages of simple operation and low cost. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are partial embodiments of the present invention, rather than all embodiments.
[0020] Example
[0021] The present invention provides an excellent ALD process, comprising the following steps:
[0022] (1) The growth substrate is sent into the cavity, and before the aluminum oxide growth process, the temperature is ensured to reach the set temperature requirement. The preferred temperature is 210°C, and the constant pressure and temperature are maintained for a certain period of time to ensure that the substrate to be grown and the entire process cavity are stable at this temperature. The constant temperature state is conducive to ensuring the uniformity of the subsequent aluminum oxide film growth.
[0023] (2) Preferential growth with TMA+H 2 O is the growth source to grow the aluminum oxide film, TMA and H 2 O is alternately introduced into the process chamber for deposition; the minimum cycle of the process gas alternately introduced is TMA gas, purge gas, H 2 O evaporation gas, purge gas; the single TMA flow rate is 18 sccm, the pulse duration is 2.5 s, N 2 The purge time is 7s, single H 2 The O flow rate is 18 sccm, the pulse duration is 6 s, and the N 2 The purge time is 8s.
[0024] Among them, TMA and H 2 The number of times O is alternately introduced directly determines the thickness of the aluminum oxide film layer, and can therefore be set according to the process and on-site matching requirements.
[0025] TMA and H 2 The aluminum oxide generated by the reaction of O reduces the interface state density of the substrate, and H 2 The O pulse introduces hydroxyl groups during the reaction, which not only increases the reaction rate, but also improves the quality of the interfacial oxide layer during the annealing step, thereby enhancing the chemical passivation effect.
[0026] (3) After each minimum cycle or after multiple minimum cycles, the auxiliary gas O 3 into the process chamber, and then through N 2 Purge gas, O 3 The flow rate is 12sccm, the pulse duration is 6s, N 2 The purge time is 7s.
[0027] TMA and H 2O reaction generates alumina film with low interface state density and good chemical passivation, but due to H 2 O has no oxidizing property 3 Strong, TMA and H 2 The resistivity of the aluminum oxide film generated by the reaction of O is relatively high, the main reason being the high content of C in the film. 3 The strong oxidizing property can effectively oxidize -CH 3 ligands, thereby reducing the resistivity of the film.
[0028] (4) According to the thickness selection, steps (2) and (3) are cycled 8 times, and the aluminum oxide film layer of about 8 nm is obtained by testing;
[0029] (5) Perform N 2 Purge, break vacuum and exit the chamber.
[0030] Comparative Example 1
[0031] (1) The growth substrate is sent into the cavity, and before the aluminum oxide growth process, the temperature is ensured to reach the set temperature requirement. The preferred temperature is 210°C, and the constant pressure and temperature are maintained for a certain period of time to ensure that the substrate to be grown and the entire process cavity are stable at this temperature. The constant temperature state is conducive to ensuring the uniformity of the subsequent aluminum oxide film growth.
[0032] (2) Preferential growth with TMA+H 2 O is the growth source to grow the aluminum oxide film, TMA and H 2 O is alternately introduced into the process chamber for deposition; the minimum cycle of the process gas alternately introduced is TMA gas, purge gas, H 2 O evaporation gas, purge gas; the single TMA flow rate is 18 sccm, the pulse duration is 2.5 s, N 2 The purge time is 7s, single H 2 The O flow rate is 18 sccm, the pulse duration is 6 s, and the N 2 The purge time is 8s.
[0033] (3) According to the thickness selection, step (2) was repeated 8 times, and the aluminum oxide film layer of about 8 nm was obtained by testing.
[0034] Comparative Example 2
[0035] (1) The growth substrate is sent into the cavity, and before the aluminum oxide growth process, the temperature is ensured to reach the set temperature requirement. The preferred temperature is 210°C, and the constant pressure and temperature are maintained for a certain period of time to ensure that the substrate to be grown and the entire process cavity are stable at this temperature. The constant temperature state is conducive to ensuring the uniformity of the subsequent aluminum oxide film growth.
[0036] (2) Preferential growth with TMA+O 3As the growth source, aluminum oxide film is grown. TMA and O 3 The process gas is alternately introduced into the process chamber for deposition; the minimum cycle of the process gas alternately introduced is TMA gas, purge gas, O 3 gas, purge gas; the single TMA flow rate is 18sccm, the pulse duration is 2.5s, N 2 The purge time is 7s, single O 3 The flow rate is 18 sccm, the pulse duration is 6 s, N 2 The purge time is 8s.
[0037] (3) According to the thickness selection, step (2) was repeated 8 times, and the aluminum oxide film layer of about 8 nm was obtained by testing.
[0038] The performance of the aluminum oxide films of the above embodiments and comparative examples 1-2 were tested by a testing instrument, and the results are shown in Table 1 below, where the total number of negative charges Qtot (E12) and the interface state density Dit (E11) are shown.
[0039] Table 1
[0040] Qtot(E12) Yours(E11) <![CDATA[TMA+H 2 The]]> -2.41 10.8 <![CDATA[TMA+O 3 ]]> -2.63 12.1 <![CDATA[TMA+H 2 O+O 3 ]]> -2.97 8.4
[0041] It can be seen from the data in the table that the aluminum oxide film prepared by the ALD process of the present invention has a low film resistivity and a good passivation effect.
[0042] Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.
Claims
1. An excellent ALD coating process, characterized by: This process uses TMA+H2O+O3 as growth sources to grow an aluminum oxide film layer on a substrate; The steps of growing an aluminum oxide film layer on a substrate using this process are: (1) placing the growth substrate into the chamber of the deposition equipment and controlling the chamber temperature to 210° C. (2) growing aluminum oxide on the surface of a growth substrate using TMA+H2O as a growth source in an alternating pulse manner; the order of gas introduction in each cycle is TMA gas, purge gas, H2O evaporation gas, and purge gas; (3) After each cycle or after several cycles, the auxiliary gas O3 is introduced into the chamber, and finally the purge gas is introduced to purge the TMA; During the growth process, O3 is introduced into the cavity as an auxiliary source. O3 can react with -CH3 in the film, and the final reaction is H2O+CO2, which is purged out by the purge gas; In each cycle of step (2), the flow rate of TMA is 18 sccm, the pulse duration is 2.5 s, and the purge duration is 7 s; In each cycle of step (2), the flow rate of H2O is 18 sccm, the pulse duration is 6 s, and the purge duration is 8 s; In step (3), the O3 flow rate is 12 sccm and the pulse duration is 6 s.
2. An excellent ALD coating process according to claim 1, characterized in that: The purge time in step (3) is 7 seconds.
3. An excellent ALD coating process according to claim 1, characterized in that: The purge gas is nitrogen.
Citation Information
Cited By
Method for preparing aluminum oxide and aluminum nitride composite film through hot filament assisted atomic layer deposition
CN122327181A
Method for preparing aluminum oxide and aluminum nitride composite film by hot-wire assisted atomic layer deposition
CN122327181B