Process for preparing integrated shaft through cold metal transfer cladding
Through the cold metal transfer welding process, the transition layer alloy and wear-resistant layer alloy are clad on the wind power gear box shaft to form an integrated structure, solving the failure problem of traditional sliding bearings under extreme operating conditions, and improving reliability and cost-effectiveness , suitable for long-life wind power gearbox applications.
Patent Information
- Application Number
- CN202410940306.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The sliding bearings of traditional wind power gear boxes are prone to deform and displace under extreme operating conditions, and lack of binding force, resulting in high failure risk and long design life increase maintenance costs.
The integrated shaft is manufactured by cold metal transfer welding process. By clading the transition layer alloy and wear-resistant layer alloy on the shaft surface, combined with fine process parameters and detection measures, an integrated structure is formed to enhance the ductility, thermal stability and Abrasion resistance.
It significantly improves the reliability and service life of bearings, reduces material costs and maintenance frequency, and enhances environmental adaptability and operating efficiency.
Smart Images

Figure CN118880313A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of manufacturing wind power gearboxes and shafts thereof, and specifically relates to a process for preparing an integrated shaft by cold metal transfer cladding. Background Art
[0002] In recent years, as the world pays more and more attention to renewable energy, the development and utilization of wind energy as a clean and sustainable energy form has been rapidly developed. One of the core components of wind power equipment, the gearbox, plays a key role in converting the rotational motion generated by the wind wheel into the speed required by the generator. Among them, the sliding bearing is an important component inside the gearbox, and its performance directly affects the reliability and efficiency of the entire system.
[0003] In traditional sliding bearing design, Figure 1 The planetary axis shown is similar to Figure 2 The alloy sleeves shown are connected by interference fit and fixed with bolts or pins. Although this method is widely used, it exposes many problems in practical applications. First, the radial force, bending force and thermal expansion caused by temperature rise during operation can easily cause bearing deformation and displacement, especially under extreme working conditions. Secondly, the thick wall thickness of the alloy sleeve not only increases the material cost, but also affects the overall economy. In addition, the bonding force under the traditional connection method is often insufficient when facing complex working conditions, especially in the case of oil hole blockage, which can easily cause bearing slippage or displacement, thereby accelerating the failure process. In addition, the design life of wind turbine gearboxes is relatively long (20 years on land and 25 years at sea). The limitations of traditional sliding bearing design significantly increase the failure risk and maintenance costs throughout the life cycle.
[0004] In view of the above problems, developing a new type of bearing technology to overcome the limitations of traditional sliding bearings, achieve longer service life, lower maintenance frequency and higher operating efficiency, while having good economy and environmental adaptability will be of great practical significance to the development of the wind power industry. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a process for preparing an integrated shaft by cold metal transfer cladding.
[0006] The first aspect of the present invention is to provide a process for preparing an integrated shaft, comprising the following steps: Step S1: Clean the surface of the shaft to remove oxides and oil stains; Step S2: using a cold metal transfer cladding process to melt the transition layer alloy onto the surface of the shaft; Step S3: Processing and inspecting the transition layer to ensure that its surface meets the preset flatness and geometric accuracy and has no cracks, unfused or hole defects; Step S4: using a cold metal transfer cladding process to melt the wear-resistant layer alloy onto the transition layer; Step S5: Process and inspect the wear-resistant layer to ensure that the surface has no cracks, unfused or hole defects, and meets the designed roughness requirements.
[0007] As a further optimization solution for the preparation process of the above-mentioned integrated shaft, in step S2, a cold metal transfer cladding process is used to clad the transition layer alloy on the surface of the shaft with the following parameters: Current: 180-220A; Voltage: 22-26V; Surfacing speed: 15-25mm / s; Gas protection: He, flow rate 15-20L / min; or other single or mixed protective gases with the same flow rate; Preheat the shaft to 100-150℃ before surfacing welding, and control the temperature of the surfacing area not to exceed 400℃ during surfacing welding. Forced air cooling is performed after surfacing welding. The transition layer alloy includes but is not limited to the following components and mass ratio ranges: Co (cobalt): 50-60%; Cr (chromium): 20-30%; W (tungsten): 10-20%; C (carbon): 0.5-1.5%; Other elements: less than 2%.
[0008] As a further optimization scheme for the preparation process of the above-mentioned integrated shaft, in step S4, a cold metal transfer cladding process is used to clad the wear-resistant layer alloy on the transition layer with the following parameters: Current: 220-260A; Voltage: 22-26V; Surfacing speed: 15-25mm / s; Gas protection: He, flow rate 15-20L / min; or other single or mixed protective gases with the same flow rate; Preheat the shaft to 100-150℃ before surfacing welding, and control the temperature of the surfacing area not to exceed 400℃ during surfacing welding. Forced air cooling is performed after surfacing welding. The wear-resistant layer alloy includes but is not limited to the following components and mass ratio ranges: Cu (copper): 80-85% Sn (Tin): 10-13% Ni (nickel): 0.5-3% Other elements: less than 2%.
[0009] As a further optimization solution for the preparation process of the above-mentioned integrated shaft, the material of the shaft is selected from steel or cast iron.
[0010] As a further optimization solution for the preparation process of the above-mentioned integrated shaft, the shaft is a planetary shaft of a wind power gearbox.
[0011] As a further optimization scheme for the preparation process of the above-mentioned integrated shaft, the total thickness of the transition layer alloy and the wear-resistant layer alloy is 1 to 3 mm.
[0012] As a further optimization scheme for the preparation process of the above-mentioned integrated shaft, the thickness ratio of the transition layer alloy to the wear-resistant layer alloy is 3:7~7:3.
[0013] As a further optimization scheme for the preparation process of the above-mentioned integrated shaft, in step S2, the uneven parts of the transition layer surface are removed by mechanical processing such as turning or grinding; and magnetic particle testing or penetration testing is used to ensure that the transition layer has no cracks, unfused or hole defects.
[0014] As a further optimization scheme for the preparation process of the above-mentioned integrated shaft, in step S5, the uneven parts of the surface are removed by mechanical processing such as turning or grinding; the wear-resistant layer is ultrasonically tested to ensure that there are no delamination, voids or crack defects inside; and the surface quality of the wear-resistant layer is checked using a surface roughness meter to ensure that it meets the designed roughness requirements.
[0015] A second aspect of the present invention is to provide a wind turbine gearbox, in which a planetary shaft is rotatably installed, and the planetary shaft is manufactured according to the manufacturing process of the above-mentioned integrated shaft.
[0016] Beneficial Effects The integrated shaft cold metal transfer cladding manufacturing process proposed in the invention not only significantly improves the performance of the shaft, but also effectively reduces costs, enhances environmental adaptability and operating efficiency, and plays an important role in promoting the sustainable development of the wind power industry. The present invention provides excellent ductility, thermal stability, corrosion resistance and high hardness through the refined selection of transition layer alloys and wear-resistant layer alloys, especially the combined use of nickel-based alloys and cobalt-based alloys, and enhances the ability of the shaft to resist thermal expansion, mechanical stress and wear. The present invention ensures the uniformity and density of the alloy layer by finely controlling parameters such as current, voltage, speed and gas protection, reduces defects such as cracks, unfused or holes, and further improves the overall performance and reliability of the shaft. The present invention reduces the influence of thermal stress through effective control of the preheating and cooling processes. Compared with traditional sliding bearings and shafts, this integrated shaft reduces the wall thickness of the alloy sleeve, reduces material costs, simplifies the assembly process, and reduces manufacturing and maintenance costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1Schematic diagram of the structure of a traditional planetary shaft.
[0018] Figure 2 It is a schematic diagram of the structure of a traditional alloy sleeve.
[0019] Figure 3 A schematic diagram of the structure of the shaft manufactured by the present invention. DETAILED DESCRIPTION
[0020] The present invention is further illustrated by specific examples below. These examples are exemplary and are intended to illustrate the problem and explain the present invention, but are not intended to be limiting.
[0021] The present invention provides a manufacturing process for an integrated shaft, that is, a manufacturing process for an integrated shaft by cold metal transfer cladding. A transition layer alloy and another wear-resistant layer alloy are sequentially clad on the surface of the shaft by cold metal transfer cladding, and the total thickness of the alloy layer in the radial direction is 1-3 mm. The shaft manufactured by this technology is as follows Figure 3 As shown, it is a composite of a shaft and a bearing, which is essentially different from the traditional sliding bearing and the shaft being separated into two parts.
[0022] As described above, the present invention clads a transition layer alloy and a wear-resistant layer alloy on the shaft surface through a cold metal transfer cladding process. In a specific embodiment, the planetary shaft is clamped on a cladding device, and the material of the planetary shaft can be steel or cast iron, and cold metal transfer cladding is performed according to set parameters. After the first transition layer is clad, processing and testing are performed, and after ensuring the quality, the second wear-resistant layer is clad, and then processing and testing are performed.
[0023] Axis preprocessing Clean the surface of the shaft by grinding and chemically cleaning to remove any remaining oxides and oils.
[0024] Selection of transition layer alloy materials A chromium-based alloy, a nickel-based alloy or other nonferrous metal alloy is selected. Preferably, the composition and mass ratio of the transition layer alloy are as follows: Co (cobalt): 50-60%; Cr (chromium): 20-30%; W (tungsten): 10-20%; C (carbon): 0.5-1.5%; Other elements are less than 2%.
[0025] The alloy has good ductility, thermal stability and corrosion resistance, and can effectively cope with thermal expansion and mechanical stress, ensuring a tight bond with the planetary shaft.
[0026] Transition layer cladding parameter setting Current: 180-220A, suitable for transition layer alloy.
[0027] Voltage: 22-26V, keep the arc stable.
[0028] Speed: 15-25mm / s, ensuring the uniformity and density of the alloy layer.
[0029] Gas protection: Use He gas (or other single or mixed protective gases with equivalent flow rate), and control the flow rate at 15-20L / min to prevent oxidation and splashing.
[0030] Before surfacing the transition layer, the planetary shaft is preheated to 100-150°C to reduce thermal stress.
[0031] During the surfacing process, the temperature of the surfacing area is controlled not to exceed 400℃ to avoid degradation of material properties. After surfacing, insulation is performed and then forced air cooling is performed.
[0032] Transition layer processing and testing Rough machining: Use turning or grinding to remove the uneven parts of the transition layer surface to ensure the flatness and geometric accuracy of the transition layer surface.
[0033] Non-destructive testing: Magnetic particle testing (MT) or penetrant testing (PT) is used to ensure that the transition layer has no cracks, unfused or hole defects.
[0034] Selection of wear-resistant layer alloy materials A copper-based alloy, an aluminum-based alloy or other nonferrous metal alloy wear-resistant layer alloy is selected. Preferably, the alloy composition and mass ratio range are as follows: Cu (copper): 80-85% Sn (Tin): 10-13% Ni (nickel): 0.5-3% Other elements are less than 2%.
[0035] This alloy has extremely high hardness and wear resistance, and can significantly increase the service life of the bearing.
[0036] Wear-resistant layer surfacing parameter setting Current: 220-260A, suitable for wear-resistant layer alloy.
[0037] Voltage: 22-26V, keep the arc stable.
[0038] Speed: 15-25mm / s, ensuring the uniformity and density of the alloy layer.
[0039] Gas protection: Use He gas (or other single or mixed protective gases with equivalent flow rate), and control the flow rate at 15-20L / min to prevent oxidation and splashing.
[0040] Before surfacing the wear-resistant layer, the planetary shaft is preheated to 100-150°C to reduce thermal stress.
[0041] During the surfacing process, the temperature of the surfacing area is controlled not to exceed 400℃ to avoid degradation of material properties. After surfacing, insulation is performed and then forced air cooling is performed.
[0042] Wear-resistant layer processing and testing Finishing: After the wear-resistant layer is clad, use turning or grinding to remove the uneven surface.
[0043] Ultrasonic Testing (UT): Ultrasonic testing of the wear-resistant layer ensures that there are no obvious internal defects such as delamination, voids or cracks.
[0044] Surface roughness detection: Use a surface roughness tester to check the surface quality of the wear-resistant layer to ensure that it meets the designed roughness requirements. Low surface roughness helps reduce friction and wear.
[0045] In summary, the embodiment of the present invention uses cold metal transfer cladding to melt the transition layer alloy and the wear-resistant layer alloy onto the planetary shaft to form an integrated structure, which effectively solves the failure problem of traditional sliding bearings and improves the reliability and cost-effectiveness of the bearings. Through precise process parameter control and quality inspection, the alloy layer is ensured to be firm and reliable, meeting the long-term operation requirements of the wind power gearbox.
[0046] The above embodiments are exemplary, and their purpose is to illustrate the technical concept and features of the present invention so that people familiar with the technology in this field can understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A process for preparing an integrated shaft by cold metal transfer cladding, characterized in that: The following steps are involved: Step S1: Clean the surface of the shaft to remove oxides and oil stains; Step S2: using a cold metal transfer cladding process to melt the transition layer alloy onto the surface of the shaft; Step S3: Processing and inspecting the transition layer to ensure that its surface meets the preset flatness and geometric accuracy and has no cracks, unfused or hole defects; Step S4: using a cold metal transfer cladding process to melt the wear-resistant layer alloy onto the transition layer; Step S5: Process and inspect the wear-resistant layer to ensure that the surface has no cracks, unfused or hole defects and meets the designed roughness requirements.
2. The process for preparing an integrated shaft by cold metal transfer cladding according to claim 1, characterized in that: In step S2, a cold metal transfer cladding process is used to clad the transition layer alloy on the surface of the shaft with the following parameters: Current: 180-220A; Voltage: 22-26V; Surfacing speed: 15-25mm / s; Gas protection: He, flow rate 15-20L / min; or other single or mixed protective gases with the same flow rate; Preheat the shaft to 100-150℃ before surfacing, and control the temperature of the surfacing area not to exceed 400℃ during surfacing, and keep it warm and then cool after surfacing; The transition layer alloy comprises the following components and mass ratios: Co (cobalt): 50-60%; Cr (chromium): 20-30%; W (tungsten): 10-20%; C (carbon): 0.5-1.5%; Other elements: less than 2%.
3. The process for preparing an integrated shaft by cold metal transfer cladding according to claim 1, characterized in that: In step S4, the wear-resistant layer alloy is clad on the transition layer using a cold metal transfer cladding process with the following parameters: Current: 220-260A; Voltage: 22-26V; Surfacing speed: 15-25mm / s; Gas protection: He, flow rate 15-20L / min; or other single or mixed protective gases with the same flow rate; Preheat the shaft to 100-150℃ before surfacing welding, and control the temperature of the surfacing area not to exceed 400℃ during surfacing welding. Forced air cooling is performed after surfacing welding. The wear-resistant layer alloy comprises the following components and mass ratio ranges: Cu (copper): 80-85% Sn (Tin): 10-13% Ni (nickel): 0.5-3% Other elements: less than 2%.
4. The process for preparing an integrated shaft by cold metal transfer cladding according to claim 1, characterized in that: The material of the shaft is selected from steel or cast iron.
5. The process for preparing an integrated shaft by cold metal transfer cladding according to claim 4, characterized in that: The shaft is a planetary shaft of a wind power gearbox.
6. The process for preparing an integrated shaft by cold metal transfer cladding according to claim 1, characterized in that: The total thickness of the transition layer alloy and the wear-resistant layer alloy is 1~3 mm.
7. The process for preparing an integrated shaft by cold metal transfer cladding according to claim 6, characterized in that: The thickness ratio of the transition layer alloy to the wear-resistant layer alloy is 3:7~7:
3.
8. The process for preparing an integrated shaft by cold metal transfer cladding according to claim 1, characterized in that: In step S2, the uneven parts on the surface of the transition layer are removed by mechanical processing such as turning or grinding; and magnetic particle testing or penetration testing is used to ensure that the transition layer has no cracks, unfused or hole defects.
9. The process for preparing an integrated shaft by cold metal transfer cladding according to claim 1, characterized in that: In step S5, the uneven parts of the surface are removed by mechanical processing such as turning or grinding; the wear-resistant layer is ultrasonically tested to ensure that there are no delamination, voids or cracks inside; and the surface quality of the wear-resistant layer is checked using a surface roughness meter to ensure that it meets the designed roughness requirements.
Citation Information
Patent Citations
Wear resistant shaft
CN103089794A
Overlaying welding method of metal-based composite-type hard-surface material layer of TC (Tungsten Carbide) bearing
CN103388145A
Laser cladding process for wind power sliding shaft
CN115772668A