Processing method for improving degreasing performance of titanium strip coil
Through the titanium tape roll degreasing method without unrolling, combined with high-pressure nozzles, electrolytic cells and special degreasing agents, the problems of complex and time-consuming degreasing process and difficult to remove oil stains in the prior art are solved, and efficient and thorough cleaning of the titanium tape roll surface is achieved. , ensuring product quality and stability.
Patent Information
- Application Number
- CN202410940143.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-15
AI Technical Summary
In the prior art, the degreasing process of titanium tape coils requires unrolling, which leads to complex operation, time-consuming and may damage or contaminate the titanium tape coils, and cannot effectively remove oil stains in complex structures, affecting product quality and performance.
The processing method without unrolling is adopted, including pre-degreasing, powder degreasing, electrolytic degreasing and annealing treatment, and the use of high-pressure nozzles, electrolytic cells and special degreasing agents combined with lye and microwave assisted treatment to ensure the surface of the titanium tape roll is thoroughly clean.
It has achieved efficient degreasing on the surface of titanium tape rolls that are up to thousands of meters long, with a wet water area ratio of 99.5-99.9%, avoiding local deformation after unrolling, improving the thoroughness and efficiency of degreasing, and maintaining the titanium tape rolls. Integrity and stability.
Smart Images

Figure CN118880348A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy strip coil surface grease removal, and in particular to a processing method for improving the degreasing performance of a titanium strip coil. Background Art
[0002] During the cold rolling process of titanium strip, lubricating oil needs to be sprayed on the surface to play a role in lubrication and cooling. Therefore, after rolling, a layer of rolling oil film remains on the surface of the titanium coil. In order to clean the titanium coil, the surface oil film must be quickly removed. In order to avoid lubricating oil contaminating the surface quality of the titanium strip, the surface needs to be cleaned and degreased before annealing; in the production process of titanium coil, surface grease removal is a very critical step. This step is mainly to ensure that the rolling oil and other grease substances on the surface of the titanium coil are completely removed before entering the vacuum furnace for heat treatment. If these greases remain on the surface of the titanium coil, even a small amount, it may cause oxidation pollution and discoloration on the surface of the titanium strip, thereby affecting the quality and performance of the product.
[0003] Moreover, most of the degreasing methods for the coils in the prior art require unwinding before operation. Although unwinding and degreasing can more directly degrease each part of the titanium coil, this process is usually more complicated and time-consuming. After unwinding, each layer or each section needs to be processed separately and then rewound, which not only increases the complexity and time cost of the operation, but may also cause damage or contamination to the surface of the titanium coil due to multiple treatments. In order to solve the above problems, the present invention decides to propose a processing method that does not require unwinding and has good degreasing performance. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a processing method for improving the degreasing performance of titanium strip coils.
[0005] The technical solution of the present invention is: a processing method for improving the degreasing performance of titanium strip coils, comprising the following steps:
[0006] S1. Pre-degreasing
[0007] The titanium strip coil is sequentially passed through the first alkali solution tank, the soaking tank, the second alkali solution tank, the rinsing tank, the third alkali solution tank, and the cleaning tank for ultrasonic treatment for 5-10 minutes to obtain a pre-degreased titanium strip coil; the alkali point of the first alkali solution tank is 3-5%, and then the alkali point of the alkali solution in each tank is increased by 2.5-5%; the rinsing tank contains a solution obtained by mixing nitric acid with a concentration of 15-20g / L and hydrofluoric acid with a concentration of 30-50g / L in a mass ratio of 2-2.5:1; the alkali solution temperature is 15-30°C;
[0008] The soaking tank contains water at a temperature of 40-50°C; a spray port is provided at the top of the cleaning tank for spraying a degreasing agent A at a temperature of 50-60°C, and a brush roller is provided above the cleaning tank for rotation; the brush roller brushes the upper surface of the titanium strip coil to clean the debris adhering to the surface of the titanium strip coil;
[0009] S2. Degreasing treatment
[0010] S2-1, powder degreasing:
[0011] The suction powder and the binder are mixed with the degreasing agent A flowing out from the bottom of the titanium strip in a mass ratio of 0.3-0.5:0.05-0.1:1 to obtain the degreasing agent B, which is evenly divided into 2-3 portions; the pre-degreased titanium strip is then placed vertically, and one portion of the degreasing agent B is sprayed along the gaps between the layers of the top titanium strip using a high-pressure rotary spray nozzle for degreasing; the flow rate of the high-pressure nozzle is 1.5-2m 3 / h, nozzle pressure is 0.8-1.8MPa, and the spray angle is 45-65°; spraying the degreaser onto the surface of the coil at the above pressure can help the degreasing liquid penetrate the interlayer of the coil and reduce the residual impurities inside. This method can ensure the full contact between the degreaser and the oil stains better than traditional immersion or surface coating, thereby improving the degreasing effect; high-pressure airflow not only helps the degreaser to be evenly distributed on the surface of the titanium coil, but also may enhance its permeability, so that the degreaser can penetrate deeper into the oil stains, especially those attached to the inside of the titanium coil or in the complex structure. This helps to remove the oil stains more thoroughly and improve the degreasing quality; the role of the binder is to provide a carrier and mechanical support for the air-intake powder, so that it has good fluidity, thereby forming a degreaser B with a stable composition, which provides the necessary promotion effect for improving the electrolytic degreasing effect of the degreaser B on the surface of the titanium coil;
[0012] S2-2, Electrolytic degreasing
[0013] The titanium strip coil is placed in an electrolytic cell, with the titanium strip coil as the cathode and the electrode plate as the anode, and then powered on. The electrolyte in the electrolytic cell is a potassium hydroxide solution with a molar concentration of 0.15-0.2 mol / L. When the electrolyte temperature rises by 5-10°C, 1 / 8-1 / 4 of the remaining degreasing agent B and a low-foaming surfactant accounting for 0.5-0.7% of the mass percentage of the degreasing agent B are added, and the temperature is kept for 5-7 minutes. After the degreasing agent B is added, the titanium strip coil is taken out and rinsed with water spray at a pressure of 0.15-0.25 MPa and a water temperature of 40-50°C; wherein, the current in the electrolytic cell is 2400-2600A, and the current density is 5-10A / dm 2 ;
[0014] S3, annealing
[0015] The titanium strip coil after electrolytic degreasing is sent into a vacuum furnace at 750-800℃ for 25-45m 3 Helium is introduced at a flow rate of / h for annealing, and tension straightening is performed after annealing is completed;
[0016] S4, leveling treatment
[0017] The titanium strip coil that has undergone the tension and straightening treatment is subjected to surface flattening treatment to obtain a titanium strip coil that has undergone flattening treatment.
[0018] Description: The titanium strip degreasing process of this method can achieve the treatment of the surface of the titanium strip that has been opened up to a length of thousands of meters and wrapped into a ring shape. The wet water area ratio after degreasing can reach 99.5-99.9%, which is slightly different from the degreasing effect after unwinding by the traditional degreasing process. The vacuum powder degreasing is used as the preliminary treatment step to preliminarily remove most of the grease and dirt on the surface of the titanium strip. The subsequent electrolytic degreasing can further clean and remove more difficult-to-treat oil and residues. This combined degreasing method can improve the thoroughness and efficiency of degreasing. The surface of the titanium strip after vacuum powder degreasing is cleaner, which can reduce the content of impurities and pollutants in the electrolytic degreasing solution, thereby helping to maintain the stability and activity of the electrolytic degreasing solution and extend its service life.
[0019] As a strong electrolyte, potassium hydroxide solution can form ions in water, thereby enhancing the conductivity of the solution. This helps the electrolytic reaction to proceed more efficiently, improves the speed and effect of degreasing, and can also keep the pH value of the degreasing solution in the alkaline range. The alkaline environment helps the saponification and emulsification of oils and fats, thereby more effectively removing oil stains on the surface of the titanium strip coil; and adding degreasing agent B in the form of mass percentage can also play a positive role in supplementing the degreasing ability, thereby improving the degreasing effect and efficiency;
[0020] The getter powder can absorb the grease on the surface of the titanium coil, because the grease molecules tend to have strong lipophilicity, while the getter powder has the opposite hydrophilicity. Under the action of high-pressure airflow, the getter powder is sprayed onto the surface of the titanium coil. After contacting with the grease molecules, the grease molecules are firmly adsorbed through physical or chemical adsorption, thereby achieving the purpose of removing grease. The getter powder can not only absorb grease, but also form tiny bumps on the surface of the titanium coil through its own physical form (such as spherical or irregular shape), which can increase the mechanical force during the cleaning process and help to more thoroughly remove grease and other particles on the surface.
[0021] Further, in step S1, during the rinsing process, spherical cast steel sand with a particle size of 1-3 mm is used for shot blasting, the shot blasting speed is 40-200 m / min, the spraying angle is 30-50°C, the shot blasting sand amount is 600-800 kg / min, and the shot blasting time is 30-120 s;
[0022] Description: Shot blasting can remove residues, oil stains and other impurities on the surface of titanium coils through the high-speed impact of spherical cast steel sand, which helps to enhance the rinsing effect and make the rinsing process more thorough; and shot blasting can also improve the surface morphology of titanium coils and increase the surface roughness, which helps to improve the adhesion and permeability of subsequent degreasing agents on the surface; when performing shot blasting, the above-mentioned processing parameters can avoid excessive damage to the titanium coils.
[0023] Further, in step S1, the alkali solution in the first alkali solution tank, the second alkali solution tank, and the third alkali solution tank is a sodium hydroxide solution, and microwave-assisted heating is performed while immersing in each alkali solution tank; wherein the microwave power is 18-20kW, the heating temperature is 25-40°C, and the microwave time is 5-25min;
[0024] Note: Microwave-assisted treatment can also promote the cleanliness of the titanium coil surface by alkali solution, and because the titanium coil is not unwound, the microwave can accelerate the decomposition and removal of grease and impurities in the gaps on the surface of the titanium coil, thereby improving the treatment effect of the alkali solution on the surface of the titanium coil.
[0025] Further, in step S1, the brush roller is one of a nylon brush roller, a non-woven fabric brush roller, and a ceramic brush roller;
[0026] Description: Nylon bristles and non-woven brush rollers have small capillary counts and are usually soft, which can effectively clean dirt and oil stains on the end surface of the titanium strip roll. In addition, it can gently clean without damaging the surface of the titanium strip roll; ceramic brush rollers can significantly improve the surface finish of the end surface of the titanium strip roll and remove poor surface conditions through the slight friction and passivation of the bristles.
[0027] Furthermore, in step S1, the degreasing agent A comprises, by weight: 2-5 parts of acetone, 0.5-3 parts of sodium carbonate, 8-12 parts of benzotriazole, 3-4 parts of emulsifying microcapsules, 4-6 parts of penetrant JFC, and 35-65 parts of deionized water;
[0028] The emulsified microcapsule comprises, by mass percentage, 25-40% of resin microspheres, 2-8% of a sodium silicate solution with a concentration of 25-35 g / L, 10-20% of a white carbon black dispersant, 1-5% of dextrin, 1.5-2% of silica sol, 0.8-1.2% of a curing agent, and the balance of water;
[0029] Description: By adding emulsified microcapsules to the degreasing agent A, a variety of water-soluble emulsifiers can be spontaneously embedded in the microcapsules and controlled to be released at a controllable rate, which means that the emulsified components can act on the grease more evenly and continuously, thereby further enhancing the degreasing efficiency of the degreasing agent on the surface of the titanium strip, thereby improving the degreasing effect; when preparing emulsified microcapsules, resin microspheres can be used as the wall material of the microcapsules to provide structural support and protection. The addition of sodium silicate solution can improve the stability of the emulsified microcapsules and prevent the microcapsules from rupturing or agglomerating during the preparation and storage process. The penetrant JFC can be used as an auxiliary agent in the preparation process to improve the reaction efficiency and improve the degreasing effect. It has a high degree of permeability and can promote the degreasing components to diffuse and penetrate into the interior of the titanium strip more quickly.
[0030] Furthermore, the preparation method of the emulsified microcapsule is:
[0031] The sodium silicate solution is divided into 2-3 parts, and the silica sol, water and one of the sodium silicate solutions are mixed to obtain a composite solution A, and then resin microspheres are added to the composite solution A at a solid-liquid ratio of 1:2.5-3 and ultrasonically dispersed for 15-20 minutes to obtain a suspension C;
[0032] Sequentially add white carbon black dispersant and dextrin to the remaining sodium silicate solution, stir and mix at 80-90° C. to obtain a composite solution B;
[0033] The composite solution B is homogenized and emulsified by a homogenizer at a speed of 8000-9000 rpm for 1-1.5 min, and then centrifuged at 1000-1500 rpm for 18-20 min to obtain an emulsion, and finally the suspension C and the curing agent are mixed and added to the emulsion, and finally centrifugally spray-dried at a speed of 16000-18000 rpm for 10-20 min to obtain emulsified microcapsules;
[0034] Description: Sodium silicate solution mixed with silica sol and water can generate a colloidal solution with good suspension and dispersibility, which can be used to make coatings and adhesives; the concentration of sodium silicate solution will affect the dispersibility and stability of microcapsules, while the addition of white carbon black dispersant and dextrin may improve the morphology and size distribution of microcapsules; the addition of curing agent will cause the resin microspheres in the resin microsphere composite solution to undergo a curing reaction to form a stable structure. Adding the cured resin microsphere mixture to the emulsion can help the resin microspheres to be evenly dispersed in the liquid, thereby obtaining emulsified microcapsules.
[0035] Further, in step S2-1, the getter powder is one of titanium powder or zirconium powder, and the binder is polyoxymethylene;
[0036] Description: Titanium powder and zirconium powder, as getters, have the ability to react with gases such as carbon, hydrogen, nitrogen, and oxygen at high temperatures. This means that during the degreasing process, these powders can effectively absorb and remove residual gases in the powder, which helps to reduce the adverse effects of gases on the degreasing effect and powder quality; titanium powder and zirconium powder, as metal powders, also have good thermal conductivity, which helps to transfer heat more evenly during the degreasing process and improve the degreasing speed and effect; polyformaldehyde, as a multi-component binder, can effectively fix the powder particles of the titanium strip coil and prevent the powder from falling off or deforming during the degreasing process, thereby ensuring the smooth progress of the degreasing process and effectively improving the degreasing performance of the titanium strip coil.
[0037] Further, in step S3, the elongation during the straightening treatment is 0.2-0.5%;
[0038] Description: Appropriate elongation helps to eliminate the shape defects of titanium strip, such as wave shape and buckling, thereby significantly improving the shape quality of the strip. The control of elongation can make the strip get appropriate deformation during the stretching, bending and straightening process to achieve the ideal straightness requirements.
[0039] Further, in step S4, the surface smoothing treatment adopts a continuous grinding and polishing machine group, and the process parameters are as follows: the running speed of the continuous grinding and polishing machine group is 5-7m / min, and the mesh number of the grinding head abrasive belt is 200-300 mesh;
[0040] Note: Appropriate running speed and abrasive belt mesh can ensure high production efficiency while ensuring the quality of grinding and polishing.
[0041] The beneficial effects of the present invention are:
[0042] (1) The present invention has effectively optimized the degreasing process of the titanium strip coil when it is not unrolled, and can achieve the surface treatment of the titanium strip coil with an unrolled length of thousands of meters and wrapped into a ring shape. The wet water area ratio after degreasing can reach 99.5-100%, which is slightly different from the degreasing effect after unrolling by the traditional degreasing process. At the same time, the degreasing process using this process can also help maintain the integrity and stability of the titanium strip coil. During the degreasing process, both the inside and the outside of the titanium strip coil can be effectively treated, avoiding problems such as local deformation that may occur after unrolling.
[0043] (2) The present invention firstly uses alkaline solution with increasing alkaline points to pretreat the titanium coil. The alkaline solution treatment can increase the surface roughness of the titanium substrate and produce nano-scale micropores on its surface. This microstructure can usually better adsorb and remove pollutants such as grease due to its rougher surface. At the same time, a porous sodium titanate structure will be formed on the surface of the titanium substrate after the alkali treatment. Then, the titanium coil is further treated locally by powder degreasing and electrolytic degreasing processes. For the local area of the titanium coil, the surface of the titanium coil after the alkali solution treatment contains negatively charged Ti-OH groups, which can serve as active sites for electrochemical reactions and promote the precipitation of hydrogen and oxygen during the electrolysis process. The precipitation of these gases will produce a strong stirring effect, which helps to peel off the oil and impurities on the surface of the titanium coil and bring them into the solution, further promoting the electrolytic degreasing treatment effect. The synergistic effect of the two degreasing processes of powder degreasing and electrolytic degreasing can achieve deep cleaning of the surface of the titanium coil and remove stubborn grease and pollutants that are difficult to remove by conventional methods.
[0044] (3) The present invention further promotes the degreasing effect of the degreasing agent on the surface of the titanium strip coil by preparing a specific degreasing agent A containing emulsified microcapsules, and realizes effective control of the emulsifier release rate by embedding the emulsifier in the emulsified microcapsules. When the emulsifier is embedded in the emulsified microcapsules, its dispersibility and stability are enhanced, which helps to more effectively interact with oils and fats during the degreasing process, thereby improving the separation efficiency of the degreasing agent. By first preparing the resin microspheres into a suspension, it can be ensured that the microspheres are evenly dispersed in the system to avoid agglomeration or sedimentation. The suspension is then mixed with a curing agent and then combined with an emulsion to form a more stable emulsified microcapsule system. Through the preparation of the emulsified microcapsules, the resin microsphere suspension and the curing agent can be more evenly coated in the emulsion, thereby further improving the emulsification effect of the emulsified microcapsules on oils and fats. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 It is a process flow chart of the present invention;
[0046] Figure 2 This is a graph showing the degreasing performance changes of titanium strip coils of Examples 1 to 12 of the present invention and Control Groups 1 to 3;
[0047] Figure 3 It is a graph showing the degreasing performance changes of titanium strip coils of Example 1, Example 12-Example 21, and Control Group 4-Control Group 5 of the present invention;
[0048] Figure 4 It is a graph showing the change in degreasing performance of the titanium strip coils of Example 1, Example 22-Example 30, and Control Group 6-Control Group 7 of the present invention. DETAILED DESCRIPTION
[0049] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.
[0050] Embodiment 1: A processing method for improving the degreasing performance of a titanium strip coil, comprising the following steps:
[0051] S1. Pre-degreasing
[0052] The titanium strip coil is sequentially passed through the first alkali solution tank, the soaking tank, the second alkali solution tank, the rinsing tank, the third alkali solution tank, and the cleaning tank for ultrasonic treatment for 8 minutes to obtain a pre-degreased titanium strip coil; the alkali point of the first alkali solution tank is 4%, and then the alkali point of the alkali solution in each tank is increased by 4%, the alkali solution is a sodium hydroxide solution, and the temperature is 22°C; the rinsing tank is a solution obtained by mixing nitric acid with a concentration of 18g / L and hydrofluoric acid with a concentration of 40g / L in a mass ratio of 2.3:1;
[0053] In step S1, during the rinsing process, spherical cast steel sand with a particle size of 1-3 mm is used for shot blasting, the shot blasting speed is 120 m / min, the spray angle is 40°, the shot blasting sand amount is 700 kg / min, and the shot blasting time is 75 s;
[0054] In step S1, microwave-assisted heating is performed while soaking in each alkali solution tank; wherein the microwave power is 19 kW, the heating temperature is 32° C., and the microwave time is 15 min;
[0055] The soaking tank contains water at a temperature of 45°C; a spray port is provided on the top of the cleaning tank for spraying a degreasing agent A at a temperature of 55°C, and a brush roller is provided above the cleaning tank for rotation; the brush roller is a nylon brush roller; the degreasing agent A is a commercially available degreasing agent;
[0056] S2. Degreasing treatment
[0057] S2-1, powder degreasing:
[0058] The suction powder and the binder and the degreasing agent A flowing out from the bottom of the titanium strip are mixed in a mass ratio of 0.4:0.08:1 to obtain the degreasing agent B, which is evenly divided into two parts; the pre-degreased titanium strip is then placed vertically, and one portion of the degreasing agent B is sprayed along the gap between the layers of the top titanium strip using a high-pressure rotary spray nozzle for degreasing; the flow rate of the high-pressure nozzle is 1.8m 3 / h, nozzle pressure is 1.3MPa, spray angle is 55°;
[0059] In step S2-1, the getter powder is titanium powder and the binder is polyoxymethylene;
[0060] S2-2, Electrolytic degreasing
[0061] The titanium strip coil is placed in an electrolytic cell, with the titanium strip coil as the cathode and the electrode plate as the anode, and then the power is turned on. The electrolyte in the electrolytic cell is a potassium hydroxide solution with a molar concentration of 0.18 mol / L. For every 8°C increase in the electrolyte temperature, 1 / 6 of the remaining degreasing agent B and a low-foaming surfactant accounting for 0.6% of the mass percentage of the degreasing agent B are added, and the temperature is kept for 6 minutes; after the degreasing agent B is added (that is, the degreasing agent B is added 6 times, and the amount added each time is 1 / 6 of the remaining degreasing agent B), the titanium strip coil is taken out and rinsed with water spray at a pressure of 0.2 MPa and a water temperature of 45°C; wherein, the current in the electrolytic cell is 2500A, and the current density is 8A / dm 2 ; Wherein, the low foaming surfactant is trisodium phosphate solid;
[0062] S3, annealing
[0063] The titanium strip coil after electrolytic degreasing is sent into a vacuum furnace at 775℃ for 35min. 3 Helium is introduced at a flow rate of / h for annealing treatment, and tension straightening is performed after annealing is completed; wherein, the elongation during the tension straightening treatment is 0.3%;
[0064] S4, leveling treatment
[0065] The titanium strip coil after the tension and straightening treatment is subjected to surface flattening treatment to obtain a flattened titanium strip coil; the surface flattening treatment adopts a continuous grinding and polishing unit, and the process parameters are as follows: the running speed of the continuous grinding and polishing unit is 6m / min, and the mesh number of the grinding head sand belt is 250 meshes.
[0066] Embodiment 2: Different from Embodiment 1, in step S1, the alkaline point of the first alkali solution tank is 3%, and then the alkaline point of the alkali solution in each tank is increased by 2.5%; the alkali solution temperature is 15°C.
[0067] Embodiment 3: Different from Embodiment 1, in step S1, the alkaline point of the first alkali solution tank is 5%, and then the alkaline point of the alkali solution in each tank is increased by 5%; the temperature of the alkali solution is 30°C.
[0068] Example 4: Different from Example 1, in step S1, the rinsing tank contains a solution of 15 g / L nitric acid and 30 g / L hydrofluoric acid mixed in a mass ratio of 2:1.
[0069] Example 5: Different from Example 1, in step S1, the rinsing tank contains a solution of nitric acid with a concentration of 20 g / L and hydrofluoric acid with a concentration of 30-50 g / L mixed in a mass ratio of 2.5:1.
[0070] Example 6: Different from Example 1, in step S1, spherical cast steel sand with a particle size of 1-3 mm is used for shot blasting during the rinsing process, the shot blasting speed is 40 m / min, the spray angle is 30°, the shot blasting sand amount is 600 kg / min, and the shot blasting time is 120 s.
[0071] Example 7: Different from Example 1, in step S1, spherical cast steel sand with a particle size of 1-3 mm is used for shot blasting during the rinsing process, the shot blasting speed is 200 m / min, the spray angle is 50°, the shot blasting sand amount is 800 kg / min, and the shot blasting time is 30 s.
[0072] Example 8: Different from Example 1, in step S1, during the microwave-assisted heating process, the microwave power is 18 kW, the heating temperature is 25°C, and the microwave time is 25 min.
[0073] Example 9: Different from Example 1, in step S1, during the microwave-assisted heating process, the microwave power is 20 kW, the heating temperature is 40°C, and the microwave time is 5 min.
[0074] Embodiment 10: Different from Embodiment 1, in step S1, the soaking tank contains water at a temperature of 40°C; a spray port is provided on the top of the cleaning tank for spraying a degreasing agent A at a temperature of 50°C.
[0075] Example 11: Different from Example 1, in step S1, the soaking tank contains water with a temperature of 50°C; a spray port is provided on the top of the cleaning tank for spraying degreasing agent A with a temperature of 60°C.
[0076] Example 12: Different from Example 1, in step S2-1, the getter powder and the binder and the degreasing agent A flowing out from the bottom of the titanium strip roll are mixed in a mass ratio of 0.3:0.5:1 to obtain the degreasing agent B.
[0077] Example 13: Different from Example 1, in step S2-1, the getter powder and the binder and the degreasing agent A flowing out from the bottom of the titanium strip roll are mixed in a mass ratio of 0.5:0.7:1 to obtain the degreasing agent B.
[0078] Embodiment 14: Different from Embodiment 1, in step S2-1, the flow rate of the high pressure nozzle is 1.5m 3 / h, the nozzle pressure is 0.8MPa and the spray angle is 45°.
[0079] Embodiment 15: Different from Embodiment 1, in step S2-1, the flow rate of the high pressure nozzle is 2m 3 / h, the nozzle pressure is 1.8MPa and the spray angle is 65°.
[0080] Example 16: Different from Example 1, in step S2-2, the electrolyte in the electrolytic cell is a potassium hydroxide solution with a molar concentration of 0.15 mol / L, and every time the electrolyte temperature increases by 5°C, 1 / 8 of the remaining degreaser B and a low-foaming surfactant accounting for 0.5% of the mass percentage of the degreaser B are added (i.e., degreaser B is added 8 times, and the amount added each time is 1 / 8 of the remaining degreaser B), and the mixture is kept warm for 7 minutes.
[0081] Example 17: Different from Example 1, in step S2-2, the electrolyte in the electrolytic cell is a potassium hydroxide solution with a molar concentration of 0.2 mol / L, and every time the electrolyte temperature increases by 10°C, 1 / 4 of the remaining degreaser B and a low-foaming surfactant accounting for 0.7% of the mass percentage of the degreaser B are added (i.e., degreaser B is added 4 times, and the amount added each time is 1 / 4 of the remaining degreaser B), and the mixture is kept warm for 5 minutes.
[0082] Example 18: Different from Example 1, in step S2-2, after the solution temperature in the electrolytic cell reaches 70°C, the titanium strip coil is taken out and rinsed by spraying with water at a pressure of 0.15 MPa and a water temperature of 40°C.
[0083] Example 19: Different from Example 1, in step S2-2, after the solution temperature in the electrolytic cell reaches 80°C, the titanium strip coil is taken out and rinsed by spraying with water at a pressure of 0.25 MPa and a water temperature of 50°C.
[0084] Example 20: Different from Example 1, in step S2-2, the current in the electrolytic cell is 2400A and the current density is 5A / dm 2 .
[0085] Example 21: Different from Example 1, in step S2-2, the current in the electrolytic cell is 2600A and the current density is 10A / dm 2 .
[0086] Example 22: Different from Example 1, in step S3, the titanium strip coil after electrolytic degreasing is sent to a vacuum furnace at 750°C for 25 minutes. 3 Helium is introduced at a flow rate of / h for annealing treatment, and tension straightening is performed after annealing is completed; wherein, the elongation during the tension straightening treatment is 0.2%.
[0087] Example 23: Different from Example 1, in step S3, the titanium strip coil after electrolytic degreasing is sent to a vacuum furnace at 800°C for 45 minutes. 3 Helium is introduced at a flow rate of / h for annealing treatment, and tension straightening is performed after annealing is completed; wherein, the elongation during the tension straightening treatment is 0.5%.
[0088] Embodiment 24: Different from Embodiment 1, in step S4, the operating speed of the continuous grinding and polishing machine group is 5m / min.
[0089] Example 25: Different from Example 1, in step S4, the operating speed of the continuous grinding and polishing machine group is 7m / min.
[0090] Embodiment 26: Different from Embodiment 1,
[0091] Degreasing agent A includes, by mass, 4 parts of acetone, 2 parts of sodium carbonate, 10 parts of benzotriazole, 3 parts of emulsified microcapsules, 5 parts of penetrant JFC, and 50 parts of deionized water;
[0092] The emulsified microcapsule comprises, by weight percentage, 32% of resin microspheres, 5% of a sodium silicate solution with a concentration of 30 g / L, 15% of a white carbon black dispersant, 3% of dextrin, 1.7% of silica sol, 1% of a curing agent, and the balance of water; wherein the curing agent is a commercially available conventional curing agent;
[0093] The preparation method of emulsified microcapsules is as follows:
[0094] The sodium silicate solution was divided into two parts, and the silica sol, water and one of the sodium silicate solutions were mixed to obtain a composite solution A, and then resin microspheres were added to the composite solution A at a solid-liquid ratio of 1:2.8 and ultrasonically dispersed for 18 minutes to obtain a suspension C;
[0095] Adding white carbon black dispersant and dextrin to the remaining sodium silicate solution in sequence, stirring and mixing at 85° C. to obtain a composite solution B;
[0096] The composite solution B was homogenized and emulsified for 1.3 min using a homogenizer at a rotation speed of 8500 rpm, and then centrifuged at 1250 rpm for 19 min to obtain an emulsion. Finally, the suspension C and the curing agent were mixed and added to the emulsion, and finally centrifuged and spray-dried at a rotation speed of 17000 rpm for 15 min to obtain emulsified microcapsules.
[0097] Example 27: Different from Example 26, the degreasing agent A comprises, by weight: 2 parts of acetone, 0.5 parts of sodium carbonate, 8 parts of benzotriazole, 3 parts of emulsifying microcapsules, 4 parts of penetrant JFC, and 35 parts of deionized water;
[0098] The emulsified microcapsule comprises, by mass percentage, 25% of resin microspheres, 2% of sodium silicate solution with a concentration of 25 g / L, 10% of white carbon black dispersant, 1% of dextrin, 1.5% of silica sol, 0.8% of curing agent and the balance of water.
[0099] Example 28: Different from Example 26, the degreasing agent A comprises, by weight: 5 parts of acetone, 3 parts of sodium carbonate, 12 parts of benzotriazole, 4 parts of emulsifying microcapsules, 6 parts of penetrant JFC, and 65 parts of deionized water;
[0100] The emulsified microcapsule comprises, by mass percentage, 40% of resin microspheres, 8% of 35 g / L sodium silicate solution, 20% of white carbon black dispersant, 5% of dextrin, 2% of silica sol, 1.2% of curing agent and the balance of water.
[0101] Example 29: Different from Example 26, in the preparation method of emulsified microcapsules,
[0102] The sodium silicate solution was divided into two parts, and the silica sol, water and one of the sodium silicate solutions were mixed to obtain a composite solution A, and then resin microspheres were added to the composite solution A at a solid-liquid ratio of 1:2.5 and ultrasonically dispersed for 15 minutes to obtain a suspension C;
[0103] Adding white carbon black dispersant and dextrin to the remaining sodium silicate solution in sequence, stirring and mixing at 80° C. to obtain a composite solution B;
[0104] The composite solution B was homogenized and emulsified for 1 min using a homogenizer at a speed of 8000 rpm, and then centrifuged at 1000 rpm for 20 min to obtain an emulsion. Finally, the suspension C and the curing agent were mixed and added to the emulsion, and finally centrifuged and spray-dried at a speed of 16000 rpm for 20 min to obtain emulsified microcapsules.
[0105] Example 30: Different from Example 26, in the preparation method of emulsified microcapsules,
[0106] The sodium silicate solution was divided into three parts, and the silica sol, water and one of the sodium silicate solutions were mixed to obtain a composite solution A, and then resin microspheres were added to the composite solution A at a solid-liquid ratio of 1:3 and ultrasonically dispersed for 20 minutes to obtain a suspension C;
[0107] Adding white carbon black dispersant and dextrin to the remaining sodium silicate solution in sequence, stirring and mixing at 90° C. to obtain a composite solution B;
[0108] The composite solution B was homogenized and emulsified for 1.5 min using a homogenizer at a speed of 9000 rpm, and then centrifuged at 1500 rpm for 18 min to obtain an emulsion. Finally, the suspension C and the curing agent were mixed and added to the emulsion. Finally, the suspension was centrifugally spray-dried at a speed of 18000 rpm for 10 min to obtain emulsified microcapsules.
[0109] Experimental Example: The description of this experimental example is based on the scheme described in Example 1, and is intended to illustrate the practical application effect of the present invention.
[0110] Experimental design: In order to illustrate the degreasing performance of the titanium strip coil prepared by the present invention, the following experimental groups were designed:
[0111] Control group 1: Different from Example 1, the soaking tank contains degreasing agent A at a temperature of 45°C; a spray port is provided on the top of the cleaning tank for spraying water at a temperature of 55°C.
[0112] Control group 2: Different from Example 1, in step S1, the shot blasting step is missing during the rinsing process.
[0113] Control group 3: Different from Example 1, in step S1, there is no microwave-assisted heating process during the immersion in each alkali solution tank.
[0114] Control group 4: Different from Example 1, in step S2-1, the degreasing agent A is directly sprayed along the gaps between the roll layers of the top titanium strip using a high-pressure rotary spray nozzle for degreasing.
[0115] Control group 5: Different from Example 1, the electrolysis treatment in step S2-2 was not performed.
[0116] Control group 6: The difference from Example 26 is that the emulsifying microcapsules in the degreasing agent A are replaced with a commercially available emulsifier.
[0117] Control group 7: Different from Example 26, in the preparation process of the emulsified microcapsules, the components were directly mixed and emulsified in a homogenizer, and finally centrifugally spray-dried at a rotation speed of 17000 rpm for 15 min to obtain the emulsified microcapsules.
[0118] Degreasing performance evaluation method: Use Example 1-Example 30 and Control Example 1-Control Example 7 to prepare a titanium strip coil, then rinse it with deionized water after unwinding, observe whether a continuous water film can be formed on the surface of the titanium strip coil, and record the proportion of the water film area.
[0119] 1. Explore the influence of pre-degreasing operation sequence and operation method on the degreasing performance of titanium strip coils
[0120] Conclusion: Figure 2From the comparison of Examples 1-11 and Control Examples 1-3, it can be seen that the degreasing performance of the titanium strip coil is reduced after the order of pre-degreasing of the titanium strip coil is adjusted in Control Example 1. By soaking in low-concentration and then high-concentration alkali solution, the direct impact of the high-concentration alkali solution on the titanium strip coil substrate can be reduced, and the risk of corrosion to the substrate can be reduced. At the same time, although the acid cleaning step will cause certain corrosion to the strip, in this process, since the acid cleaning is located after the alkali solution treatment, it can help remove certain residues generated during the alkali solution treatment and further clean the surface. Multiple soaking treatments can ensure that the oil stains fully react with the alkali solution and improve the degreasing efficiency; in addition, the degreasing agent rinse as the last step can ensure that the oil stains remaining on the surface of the titanium strip coil are completely removed; but after adjusting the order, the wet water area ratio of the degreasing completed can still reach 99.0%;
[0121] However, the lack of shot blasting during the acid rinsing process in Control Example 2 resulted in the wet water area ratio of the prepared titanium strip coil after degreasing only reaching 93%. The lack of shot blasting will cause a significant decrease in the degreasing performance of the titanium strip coil; shot blasting can make the surface of the titanium strip coil obtain a more uniform and consistent roughness, which helps to improve the adhesion of the degreaser, thereby promoting the degreasing effect of the degreaser on the titanium strip coil; the lack of microwave-assisted heating during the alkali solution immersion process in Control Example 3 caused the degreasing performance of the titanium strip coil to show a significant decrease. This is because microwave-assisted treatment can promote the cleanliness of the alkali solution on the surface of the titanium strip coil, and since the titanium strip coil is not unwound, the action of microwaves can accelerate the decomposition and removal of grease and impurities in the gaps on the surface of the titanium strip coil, thereby improving the treatment effect of the alkali solution on the surface of the titanium strip coil.
[0122] 2. Investigate the influence of degreasing treatment steps on the degreasing performance of titanium strip
[0123] Conclusion: Figure 3 It can be seen from the trend graphs of Example 1, Examples 12-23 and Control Groups 4-5 that the lack of the preparation step of degreasing agent B in Control Group 4, and the failure to add getter powder and binder will also cause the degreasing performance of the titanium strip surface to decline. This is because the components of degreasing agent B can effectively promote electrolytic degreasing; during the electrolytic degreasing process, the oil stains are peeled off from the surface of the steel strip by the bubbles generated by electrolysis, and the degreasing agent B containing getter powder can enhance this peeling effect and improve the degreasing efficiency by adsorbing more oil stain particles; as can be seen from the diagram, electrolytic degreasing is a necessary step, and the lack of the electrolytic degreasing treatment step will cause the degreasing effect of the titanium strip surface to weaken, while the present application can further deepen the cleaning by following the powder degreasing treatment with electrolytic degreasing to remove more difficult-to-handle oil stains and residues; this combined degreasing method can improve the thoroughness and efficiency of degreasing.
[0124] 3. Investigate the effects of annealing treatment, flattening treatment parameters, and the composition and preparation method of degreasing agent A on the degreasing performance of titanium strip coils
[0125] Conclusion: Figure 4 From the trend changes of Example 1, Example 22-Example 30, and Control Group 6-Control Example 7, it can be seen that the direct application of commercially available emulsifiers in Control Group 6 also has a significant effect on the degreasing efficiency of the titanium strip. This is because the release rate of the emulsifier can be effectively controlled by embedding the emulsifier in the emulsifying microcapsule. When the emulsifier is embedded in the emulsifying microcapsule, its dispersibility and stability are enhanced, which helps to more effectively interact with the oil during the degreasing process, thereby improving the separation efficiency of the degreasing agent. In the control group 7, the surface degreasing effect of the titanium strip prepared by directly homogenizing and emulsifying the components and then centrifugally spray drying during the preparation of the emulsifying microcapsule also showed a significant decrease. This is Because the method of the present application can first prepare the resin microspheres into a suspension, it can ensure that the microspheres are evenly dispersed in the system to avoid agglomeration or sedimentation, and then the suspension is mixed with a curing agent and then combined with an emulsion to form a more stable emulsified microcapsule system. Through the preparation of emulsified microcapsules, the resin microsphere suspension and the curing agent can be more evenly coated in the emulsion, thereby further improving the emulsification effect of the emulsified microcapsules on oils and fats; and from the comparison of Example 1 and Examples 26-30, it can be seen that the degreasing agent A prepared by the method of the present application has a significant improvement in the degreasing performance of the titanium strip coil, reaching 100%. Taking all factors into consideration, Example 26 is the optimal solution.
Claims
1. A processing method for improving the degreasing performance of titanium strip coils, characterized in that: The following steps are involved: S1. Pre-degreasing The titanium strip coil is sequentially passed through the first alkali solution tank, the soaking tank, the second alkali solution tank, the rinsing tank, the third alkali solution tank, and the cleaning tank for ultrasonic treatment for 5-10 minutes to obtain a pre-degreased titanium strip coil; the alkali point of the first alkali solution tank is 3-5%, and then the alkali point of the alkali solution in each tank is increased by 2.5-5%; the rinsing tank contains a solution obtained by mixing nitric acid with a concentration of 15-20g / L and hydrofluoric acid with a concentration of 30-50g / L in a mass ratio of 2-2.5:1; the alkali solution temperature is 15-30°C; The soaking tank contains water at a temperature of 40-50°C; a spray port is provided at the top of the cleaning tank for spraying a degreasing agent A at a temperature of 50-60°C, and a brush roller is rotatably provided above the cleaning tank; S2. Degreasing treatment S2-1, powder degreasing: The suction powder and the binder are mixed with the degreasing agent A flowing out from the bottom of the titanium strip in a mass ratio of 0.3-0.5:0.05-0.1:1 to obtain the degreasing agent B, which is evenly divided into 2-3 portions; the pre-degreased titanium strip is then placed vertically, and one portion of the degreasing agent B is sprayed along the gaps between the layers of the top titanium strip using a high-pressure rotary spray nozzle for degreasing; the flow rate of the high-pressure nozzle is 1.5-2m 3 / h, nozzle pressure is 0.8-1.8MPa, spray angle is 45-65°; S2-2, Electrolytic degreasing The titanium strip coil is placed in an electrolytic cell, with the titanium strip coil as the cathode and the electrode plate as the anode, and then powered on. The electrolyte in the electrolytic cell is a potassium hydroxide solution with a molar concentration of 0.15-0.2 mol / L. When the electrolyte temperature rises by 5-10°C, 1 / 8-1 / 4 of the remaining degreasing agent B and a low-foaming surfactant accounting for 0.5-0.7% of the mass percentage of the degreasing agent B are added, and the temperature is kept for 5-7 minutes. After the degreasing agent B is added, the titanium strip coil is taken out and rinsed with water spray at a pressure of 0.15-0.25 MPa and a water temperature of 40-50°C. The current in the electrolytic cell is 2400-2600A, and the current density is 5-10A / dm 2 ; S3, annealing The titanium strip coil after electrolytic degreasing is sent into a vacuum furnace at 750-800℃ for 25-45m 3 Helium is introduced at a flow rate of / h for annealing, and tension straightening is performed after annealing is completed; S4, leveling treatment The titanium strip coil that has undergone the tension and straightening treatment is subjected to surface flattening treatment to obtain a titanium strip coil that has undergone flattening treatment.
2. A processing method for improving the degreasing performance of a titanium strip coil as claimed in claim 1, characterized in that: In step S1, during the rinsing process, spherical cast steel sand with a particle size of 1-3 mm is used for shot blasting, the shot blasting speed is 40-200 m / min, the spraying angle is 30-50°C, the shot blasting sand amount is 600-800 kg / min, and the shot blasting time is 30-120 s.
3. A processing method for improving the degreasing performance of a titanium strip coil as claimed in claim 1, characterized in that: In step S1, the alkali solution in the first alkali solution tank, the second alkali solution tank and the third alkali solution tank is a sodium hydroxide solution, and microwave-assisted heating is performed while immersing in each alkali solution tank; wherein the microwave power is 18-20kW, the heating temperature is 25-40°C, and the microwave time is 5-25min.
4. A processing method for improving the degreasing performance of a titanium strip coil as claimed in claim 1, characterized in that: In step S1, the brush roller is one of a nylon brush roller, a non-woven fabric brush roller, and a ceramic brush roller.
5. A processing method for improving the degreasing performance of a titanium strip coil as claimed in claim 1, characterized in that: In step S1, the degreasing agent A comprises, by weight: 2-5 parts of acetone, 0.5-3 parts of sodium carbonate, 8-12 parts of benzotriazole, 3-4 parts of emulsifying microcapsules, 4-6 parts of penetrant JFC, and 35-65 parts of deionized water; The emulsified microcapsule comprises, by mass percentage, 25-40% of resin microspheres, 2-8% of 25-35g / L sodium silicate solution, 10-20% of white carbon black dispersant, 1-5% of dextrin, 1.5-2% of silica sol, 0.8-1.2% of curing agent and the balance of water.
6. A processing method for improving the degreasing performance of a titanium strip coil as claimed in claim 5, characterized in that: The preparation method of the emulsified microcapsule is as follows: The sodium silicate solution is divided into 2-3 parts, and the silica sol, water and one of the sodium silicate solutions are mixed to obtain a composite solution A, and then resin microspheres are added to the composite solution A at a solid-liquid ratio of 1:2.5-3 and ultrasonically dispersed for 15-20 minutes to obtain a suspension C; Sequentially add white carbon black dispersant and dextrin to the remaining sodium silicate solution, stir and mix at 80-90° C. to obtain a composite solution B; The composite solution B is homogenized and emulsified by a homogenizer at a speed of 8000-9000 rpm for 1-1.5 min, and then centrifuged at 1000-1500 rpm for 18-20 min to obtain an emulsion. Finally, the suspension C and the curing agent are mixed and added to the emulsion, and finally centrifugally spray-dried at a speed of 16000-18000 rpm for 10-20 min to obtain emulsified microcapsules.
7. A processing method for improving the degreasing performance of a titanium strip coil as claimed in claim 1, characterized in that: In step S2-1, the getter powder is titanium powder or zirconium powder, and the binder is polyoxymethylene.
8. A processing method for improving the degreasing performance of a titanium strip coil as claimed in claim 1, characterized in that: In step S3, the elongation during the straightening treatment is 0.2-0.5%.
9. A processing method for improving the degreasing performance of a titanium strip coil as claimed in claim 1, characterized in that: In step S4, the surface smoothing treatment adopts a continuous grinding and polishing machine group, and the process parameters are as follows: the running speed of the continuous grinding and polishing machine group is 5-7m / min, and the mesh number of the grinding head sand belt is 200-300 meshes.
Citation Information
Patent Citations
Machining method for de-stressing thin pure titanium strip coils
CN105414178A
Cold-rolled titanium coil degreasing method
CN107699907A
Production process of pure-titanium cold-rolled bright-surface titanium belt
CN114367534A
Method for forming an insulating glass film on surfaces of an oriented silicon steel sheet
US3932237A