Single crystal lithium magnesium alloy, preparation method thereof and lithium metal battery

By performing directional rolling and aging heat treatment at a controlled temperature, the (110) single crystal orientation transformation of lithium magnesium alloy is achieved, solving the problem of difficulty in controlling the orientation of lithium magnesium alloy in the traditional method, and improving the performance and stability of the battery.

CN118880466APending Publication Date: 2024-11-01SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410957204.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional preparation methods are difficult to accurately control the crystallization orientation of lithium-magnesium alloys, resulting in unstable material properties, limiting its application in lithium metal batteries.

Method used

By oriented rolling under a controlled temperature environment, the grain rearrangement inside the lithium magnesium alloy is induced, and the transformation from the polycrystalline to (110) single crystal orientation is achieved, and a single crystal lithium magnesium alloy is obtained through aging heat treatment.

Benefits of technology

It significantly improves the preparation efficiency and electrochemical performance of single crystal materials, reduces the diffusion path of lithium ions during charging and discharging, and enhances the cycle stability and reliability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880466A_ABST
    Figure CN118880466A_ABST
Patent Text Reader

Abstract

The invention discloses a single crystal lithium magnesium alloy, a preparation method thereof and a lithium metal battery, a lithium magnesium alloy foil is placed in a controllable temperature environment to be directionally rolled until the deformation quantity is 50%-95% so as to induce grain rearrangement in the alloy and guide (110) single crystal orientation, and then the single crystal lithium magnesium alloy is obtained through aging heat treatment. According to the invention, the rolling temperature and the deformation quantity of the lithium alloy foil are controlled to realize the transformation of the lithium magnesium alloy from polycrystal orientation (110) single crystal orientation, the prepared single crystal structure reduces the resistance of the crystal boundary, the diffusion path of lithium ions in the charging and discharging process is reduced, and the preparation efficiency of the single crystal material and the electrochemical performance of the lithium alloy are further obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a technology in the field of lithium metal batteries, specifically a single crystal lithium-magnesium alloy with a specific (110) orientation, a preparation method thereof, and a lithium metal battery. Background Art

[0002] As one of the important candidates for the next generation of energy storage materials, lithium-magnesium alloys have attracted much attention due to their high theoretical capacity, low density and good electrochemical properties. Single crystal materials have shown great potential in improving the energy density, cycle stability and safety of batteries due to their excellent mechanical properties and electrochemical kinetics. However, traditional preparation methods make it difficult to accurately control the crystal orientation of the alloy, resulting in unstable material properties and limiting its practical application. Summary of the invention

[0003] In view of the deficiency that the prior art cannot prepare single crystal material structures and use them in the battery field, the present invention proposes a single crystal lithium-magnesium alloy and a preparation method thereof and a lithium metal battery. By controlling the rolling temperature and the deformation amount of the lithium alloy foil, the lithium-magnesium alloy is transformed from a polycrystalline to a (110) single crystal orientation. The prepared single crystal structure reduces the resistance of the grain boundary and reduces the diffusion path of lithium ions during the charge and discharge process, thereby significantly improving the preparation efficiency of the single crystal material and the electrochemical properties of the lithium alloy.

[0004] The present invention is achieved through the following technical solutions:

[0005] The invention relates to a method for preparing a single crystal lithium-magnesium alloy. The lithium-magnesium alloy foil is placed in a controllable temperature environment and directional rolled to a deformation amount of 50% to 95% to induce grain rearrangement inside the alloy and guide the (110) single crystal orientation, and then subjected to aging heat treatment to obtain the single crystal lithium-magnesium alloy.

[0006] The proportion of lithium in the lithium-magnesium alloy foil is 10.3-99.9wt.%.

[0007] The purity of the lithium-magnesium alloy foil is above 98wt% and the thickness is 50μm-1mm.

[0008] The controllable temperature environment refers to: controlling the temperature to be 50°C to 180°C under an inert atmosphere.

[0009] The inert atmosphere is argon or helium atmosphere.

[0010] The directional rolling is preferably unidirectional rolling, and more preferably unidirectional rolling 2 to 10 times.

[0011] The aging heat treatment is preferably performed using a muffle furnace, and more preferably the temperature is set at 50° C. to 180° C. for 1 hour.

[0012] The present invention relates to a single crystal lithium-magnesium alloy prepared by the above method, wherein lithium and magnesium elements are evenly distributed, and the alloy material has a consistent (110) single crystal orientation.

[0013] The present invention relates to an application based on the above-mentioned single crystal lithium-magnesium alloy, which is used as a negative electrode material to match with a diaphragm and an electrolyte to assemble a lithium metal symmetrical battery.

[0014] The electrolyte is, but not limited to, any one of the following: a mixed solution of 1M lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) in dioxolane (DOL) / ethylene glycol dimethyl ether (DME) and 2% LiNO3, a mixed solution of 0.2M LiPF6, 0.2MLiBF4, 0.8M lithium difluorooxalatoborate (LiDFOB) in diethyl carbonate (DEC): fluoroethylene carbonate (FEC) = 2:1 Vol%, a mixed solution of 1M LiTFSI in DME:DOL = 1:1 Vol%, or a mixed solution of 1M LiPF6 in ethylene carbonate (EC):DEC = 1:1 Vol%. Technical Effects

[0015] The present invention can quickly and accurately control the oriented growth of the alloy, promote the preferential growth of grains along a specific direction (110), and form a continuous and uniform single crystal structure. The method significantly shortens the production cycle, improves the yield of single crystal materials, reduces manufacturing costs, promotes uniform deposition of lithium, and effectively enhances the stability and reliability of battery recycling. The symmetrical battery is 3mA cm -2 -1mAh cm -2 Under the same conditions, the battery can be stably cycled for nearly 100 h at a low overpotential of 50 mV, and the critical current density in the LLZTO solid-state battery can reach 2 mA cm -2 , demonstrating its effect in improving electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is an experimental flow chart of the lithium-magnesium alloy prepared in Example 1;

[0017] Figure 2 This is an optical photograph of the lithium-magnesium alloy prepared in Example 1;

[0018] Figure 3 The XRD diagram of the lithium-magnesium alloy prepared in Example 1 and Comparative Example 1;

[0019] Figure 4 The symmetrical battery of Example 1 and Comparative Example 1 is 3 mA cm -2 -5mAh cm -2SEM image of the deposition morphology of the electrode surface after conditional electrodeposition, the electrolyte is 1M LiPF6 in EC:DEC=1:1Vol%;

[0020] Figure 5 The symmetrical battery of Example 2 and Comparative Example 2 is 3 mA cm -2 -1mAh cm -2 Comparison of cycle voltage-time curves under the conditions, the electrolyte is 1M LiPF6 in EC:DEC=1:1Vol%. Figure 6 This is a critical current density test diagram of the lithium-magnesium alloy solid-state battery prepared in Example 2. DETAILED DESCRIPTION Example 1

[0021] This embodiment includes the following steps:

[0022] Step 1) In a glove box filled with argon, a lithium-magnesium alloy with a thickness of 200 μm and a lithium content of 27 wt.% was placed in a roller press.

[0023] Step 2) Set the roller press temperature to 100°C.

[0024] Step 3) The lithium-magnesium alloy in step 1) is rolled forward 3 times until the deformation is 80%.

[0025] Step 4) placing the lithium-magnesium alloy prepared in step 3) in a muffle furnace and performing an aging treatment at 100° C. for 1 hour.

[0026] Step 5) naturally cool to room temperature to obtain a single crystal lithium-magnesium alloy. Comparative Example 1

[0027] This embodiment includes the following steps:

[0028] Step 1) In a glove box filled with argon, a lithium-magnesium alloy with a thickness of 200 μm and a lithium content of 27 wt.% was placed in a roller press.

[0029] Step 2) Set the roller press temperature to 100°C.

[0030] Step 3) The lithium-magnesium alloy in step 1) is rolled once in the forward direction until the deformation amount reaches 20%.

[0031] Step 4) placing the lithium-magnesium alloy prepared in step 3) in a muffle furnace and performing an aging treatment at 100° C. for 1 hour.

[0032] Step 5) naturally cooling to room temperature to obtain a lithium-magnesium alloy.

[0033] The single crystal lithium-magnesium alloy negative electrode prepared in Example 1 and the lithium-magnesium alloy negative electrode prepared in Comparative Example 1 were characterized by XRD. The results are as follows: Figure 1 The XRD of the lithium-magnesium alloy prepared in Comparative Example 1 shows diffraction peaks of (110), (200) and (211) crystal planes, indicating that the alloy foil contains three crystal planes; the alloy foil obtained after the rolling treatment in Example 1 only shows a single crystal plane peak of (110), indicating that a (110) single crystal lithium-magnesium alloy has been prepared.

[0034] The single crystal lithium-magnesium alloy negative electrode prepared in Example 1 and the lithium-magnesium alloy negative electrode prepared in Comparative Example 1 were subjected to 3 mA cm-1 in 1M LiPF6 inEC:DEC=1:1 Vol% electrolyte. -2 -5mAh cm -2 Electrodeposition was carried out under the following conditions, and the deposition morphology of lithium metal on the surface of single crystal lithium-magnesium alloy negative electrode and polycrystalline lithium-magnesium alloy negative electrode was characterized by SEM. Figure 2 As shown, the deposition morphology of metallic lithium on the surface of the single-crystalline lithium-magnesium alloy negative electrode presents a uniform and dense columnar deposition, while the lithium dendrites on the polycrystalline lithium negative electrode are randomly distributed, indicating the uniform deposition and dendrite-free characteristics of the single-crystalline lithium-magnesium alloy during battery operation.

[0035] The single crystal lithium-magnesium alloy negative electrode prepared in Example 1 and the lithium-magnesium alloy negative electrode prepared in Comparative Example 1 were subjected to 3 mA cm-2 electrolysis in 1M LiPF6 inEC:DEC=1:1 Vol% electrolyte. -2 -1mAh cm -2 Symmetrical battery cycle tests under different conditions were performed and compared. Figure 3 As shown, the symmetrical battery assembled with the single crystal lithium-magnesium alloy negative electrode prepared in Example 1 has a lower cycle overpotential and a longer stable cycle time. Example 2

[0036] This embodiment includes the following steps:

[0037] Step 1) In a glove box filled with argon, a lithium-magnesium alloy with a thickness of 200 μm and a lithium content of 70 wt.% was placed in a roller press.

[0038] Step 2) Set the roller press temperature to 100°C.

[0039] Step 3) The lithium-magnesium alloy in step 1) is rolled forward 3 times until the deformation is 80%.

[0040] Step 4) placing the lithium-magnesium alloy prepared in step 3) in a muffle furnace and performing an aging treatment at 100° C. for 1 hour.

[0041] Step 5) Then naturally cool to room temperature to obtain a single crystal lithium-magnesium alloy. Example 3

[0042] This embodiment includes the following steps:

[0043] Step 1) In a glove box filled with argon, a lithium-magnesium alloy with a thickness of 500 μm and a lithium content of 27 wt.% was placed in a roller press.

[0044] Step 2) Set the roller press temperature to 100°C.

[0045] Step 3) The lithium-magnesium alloy in step 1) is rolled forward 3 times until the deformation is 80%.

[0046] Step 4) placing the lithium-magnesium alloy prepared in step 3) in a muffle furnace and performing an aging treatment at 100° C. for 1 hour.

[0047] Step 5) naturally cool to room temperature to obtain a single crystal lithium-magnesium alloy. Example 4

[0048] This embodiment includes the following steps:

[0049] Step 1) In a glove box filled with argon, a lithium-magnesium alloy with a thickness of 200 μm and a lithium content of 27 wt.% was placed in a roller press.

[0050] Step 2) Set the roller press temperature to 60°C.

[0051] Step 3) The lithium-magnesium alloy in step 1) is rolled forward 3 times until the deformation is 80%.

[0052] Step 4) placing the lithium-magnesium alloy prepared in step 3) in a muffle furnace and performing aging treatment at 60° C. for 1 hour.

[0053] Step 5) naturally cool to room temperature to obtain a single crystal lithium-magnesium alloy. Example 5

[0054] This embodiment includes the following steps:

[0055] Step 1) In a glove box filled with argon, a lithium-magnesium alloy with a thickness of 200 μm and a lithium content of 27 wt.% was placed in a roller press.

[0056] Step 2) Set the roller press temperature to 100°C.

[0057] Step 3) The lithium-magnesium alloy in step 1) is rolled 5 times in the forward direction until the deformation is 80%.

[0058] Step 4) placing the lithium-magnesium alloy prepared in step 3) in a muffle furnace and performing an aging treatment at 100° C. for 1 hour.

[0059] Step 5) naturally cool to room temperature to obtain a single crystal lithium-magnesium alloy. Example 6

[0060] This embodiment includes the following steps:

[0061] Step 1) In a glove box filled with argon, a lithium-magnesium alloy with a thickness of 200 μm and a lithium content of 27 wt.% was placed in a roller press.

[0062] Step 2) Set the roller press temperature to 100°C.

[0063] Step 3) The lithium-magnesium alloy in step 1) is rolled forward 3 times until the deformation is 60%.

[0064] Step 4) placing the lithium-magnesium alloy prepared in step 3) in a muffle furnace and performing an aging treatment at 100° C. for 1 hour.

[0065] Step 5) naturally cool to room temperature to obtain a single crystal lithium-magnesium alloy. Comparative Example 2

[0066] This embodiment includes the following steps:

[0067] Step 1) In a glove box filled with argon, a lithium-magnesium alloy with a thickness of 200 μm and a lithium content of 5 wt.% was placed in a roller press.

[0068] Step 2) Set the roller press temperature to 100°C.

[0069] Step 3) The lithium-magnesium alloy in step 1) is rolled forward 3 times until the deformation is 80%.

[0070] Step 4) placing the lithium-magnesium alloy prepared in step 3) in a muffle furnace and performing an aging treatment at 100° C. for 1 hour.

[0071] Step 5) naturally cooling to room temperature to obtain a lithium-magnesium alloy.

[0072] Compared with the prior art, the method achieves the transformation of lithium-magnesium alloy from polycrystalline to (110) single crystal orientation and subsequent battery performance improvement by controlling the rolling temperature and the deformation amount of lithium alloy foil.

[0073] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.

Claims

1. A method for preparing a single crystal lithium-magnesium alloy, characterized in that: The lithium-magnesium alloy foil is placed in a controllable temperature environment and directional rolled to a deformation amount of 50% to 95% to induce grain rearrangement inside the alloy and guide the (110) single crystal orientation, and then subjected to aging heat treatment to obtain a single crystal lithium-magnesium alloy.

2. The method for preparing a single crystal lithium-magnesium alloy according to claim 1, wherein: The proportion of lithium in the lithium-magnesium alloy foil is 10.3-99.9wt.%.

3. The method for preparing a single crystal lithium-magnesium alloy according to claim 1, wherein: The purity of the lithium-magnesium alloy foil is above 98wt% and the thickness is 50μm-1mm.

4. The method for preparing a single crystal lithium-magnesium alloy according to claim 1, wherein: The controllable temperature environment refers to: controlling the temperature to be 50°C to 180°C under an inert atmosphere.

5. The method for preparing a single crystal lithium-magnesium alloy according to claim 1, wherein: The inert atmosphere is argon or helium atmosphere.

6. The method for preparing a single crystal lithium-magnesium alloy according to claim 1, wherein: The directional rolling is performed 2 to 10 times in one direction.

7. The method for preparing a single crystal lithium-magnesium alloy according to claim 1, wherein: The aging heat treatment is carried out using a muffle furnace with the temperature set at 50°C to 180°C for 1 hour.

8. An application of a single crystal lithium-magnesium alloy prepared by the method according to any one of claims 1 to 7, characterized in that: As the negative electrode material, it is matched with the separator and electrolyte to assemble a lithium metal symmetrical battery.

9. The use according to claim 8, characterized in that: The electrolyte is any one of the following: a mixed solution of 1M lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) in dioxolane (DOL) / ethylene glycol dimethyl ether (DME) and 2% LiNO3, a mixed solution of 0.2M LiPF6, 0.2M LiBF4, 0.8M lithium difluorooxalatoborate (LiDFOB) in diethyl carbonate (DEC): fluoroethylene carbonate (FEC) = 2:1 Vol%, a mixed solution of 1M LiTFSI in DME:DOL = 1:1 Vol%, or a mixed solution of 1MLiPF6 in ethylene carbonate (EC):DEC = 1:1 Vol%.

Citation Information

Cited By

  • Preparation method of single crystal lithium alloy negative electrode and metal lithium battery

    CN119230761A

  • Preparation method of single-crystal lithium alloy negative electrode and metal lithium battery

    CN119230761B

  • Preparation method of high-determinacy single crystal lithium metal negative electrode

    CN121451290A