Preparation method of flexible sensor for human body response detection

By introducing rigid nodes and horseshoe-shaped microstructures in straight-line structures into honeycomb structures, combined with micro-nano 3D printing technology, the problem of unfitting the rigidity of the substrate and film in traditional sensors is solved, and the efficient mechanical performance regulation of flexible sensors is achieved, which improves the The ductility and elastic modulus of the material.

CN118882869APending Publication Date: 2024-11-01BEIJING INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410938785.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Due to the inadequate stiffness between the substrate and the film, traditional wearable mechanical sensors are difficult to control the modulus in flexible sensing, resulting in insufficient performance when subjected to deformation.

Method used

By introducing rigid nodes into honeycomb structures and horseshoe-shaped microstructures into linear structures, thin film layers are prepared in combination with micro-nano 3D printing technology, and equilibrium differential equations and geometric equations are used to calculate the parameters of the microstructures, and optimize the elastic modulus of the material and Poisson's. The ratio can achieve modulus regulation between the substrate and the film.

Benefits of technology

The ductility and elastic modulus of the material are improved, the modulus of the entire material is reduced, the force-electric coupling effect between the film and the substrate is more accurate, and the mechanical properties of the flexible sensor are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118882869A_ABST
    Figure CN118882869A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a flexible sensor for human body response detection. The flexible sensor sequentially comprises a substrate layer, a thin film layer and a packaging layer from bottom to top, reasonable geometric parameters of a thin film layer structure are selected, rigid nodes are introduced into a honeycomb structure, a horseshoe-shaped microstructure is introduced into a linear structure, and the thin film layer is prepared on the basis of a micro-nano 3D printing technology, so that the ductility of the material can be improved, the elastic modulus of the material can be improved, and the control range of the Poisson ratio of the material can be widened; and therefore, low-rigidity regulation and control are realized. The problem that the rigidity of the substrate and the rigidity of the thin film in an existing flexible sensor are not matched can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sensors, and in particular to a method for preparing a flexible sensor for human body response detection. Background Art

[0002] Wearable mechanical sensors can convert external load responses into electrical signals and display them in a graphical manner. Traditional wearable mechanical sensors generally use inorganic materials such as silicon as substrates, which have the characteristics of high stiffness and poor toughness. They cannot withstand large deformations and it is difficult to achieve modulus fit between the film and the substrate in flexible sensing. In recent years, with the development of additive manufacturing technology, metamaterials that achieve mechanical properties that traditional materials do not have through microstructure design at different scales have brought new opportunities to improve the mechanical properties of flexible sensors. Therefore, while ensuring that too much material is occupied, optimizing the microstructure design to achieve modulus regulation between the substrate and the film has important scientific significance and application value. Summary of the invention

[0003] The purpose of the present invention is to provide a structural design method for a flexible sensor, which can solve the problem of incompatibility in stiffness between the substrate and the film in the current flexible sensor by selecting suitable soft materials and adjusting the size parameters of the microstructure.

[0004] The characteristic of this flexible microstructure is that a rigid node is introduced into the traditional quadrilateral, triangle and other honeycomb structures, and a horseshoe-shaped microstructure is introduced into the original linear structure. This design concept can not only improve the ductility of the material, but also increase the control range of the elastic modulus and Poisson's ratio of the material, thereby achieving lower stiffness control.

[0005] The specific technical solutions are:

[0006] A method for preparing a flexible sensor for human body response detection includes, from bottom to top, a base layer, a thin film layer and a packaging layer; reasonable geometric parameters of the thin film layer structure are selected, the thin film layer introduces rigid nodes in the honeycomb structure, and introduces a horseshoe-shaped microstructure in the straight structure, and the thin film layer is prepared based on micro-nano 3D printing technology.

[0007] The base layer is made of polyimide material.

[0008] The horseshoe-shaped microstructure is made of silver nanomaterial with conductive properties.

[0009] The packaging layer is made of epoxy resin material.

[0010] The method for determining the geometric parameters of the thin film layer structure is:

[0011] Firstly, the redundant constraint force of the microstructure is solved based on the equilibrium differential equation and geometric equation of the structure. On this basis, the total strain energy of the entire structure is determined by the force.

[0012] Then, the partial derivative of the force in the corresponding direction based on the total strain energy is the displacement required in the force direction;

[0013] Finally, the equivalent modulus and Poisson's ratio of the microstructure are calculated based on the equivalent strain and equivalent stress of the microstructure.

[0014] 6. The method for preparing a flexible sensor for human body response detection according to claim 5, characterized in that: the equilibrium differential equation and geometric equation are:

[0015] Arc quadrilateral:

[0016] ∑M O (F) = M1 + M2 - Pr = 0

[0017]

[0018] In the formula is the arc integral angle variable, ligament length L, ligament thickness t, middle circular node radius r and horseshoe radius r0, A is the cross-sectional area of ​​the ligament, I is the inertia product of the ligament about the z-axis, M1, M2, P are the constraints and external loads on the structure, E S is the elastic modulus of the material, and U is the total strain energy of the structure.

[0019] Arc Hexahandedness:

[0020] F R1 +F R2 +F R3 +F R4 +F R5 +F R6 =0

[0021] F R1 -F R4 -0.5F R3 -0.5F R5 +0.5F R6 +0.5F R2 =0

[0022] F R5 +F R6 -F R2 -F R3 =0

[0023]

[0024] In the formula is the arc integral angle variable, ligament length L, ligament thickness t, middle circular node radius r and horseshoe radius r0, A is the cross-sectional area of ​​the ligament, I is the inertia product of the ligament about the z axis, F Ri (i=1-6) is the equation for the mutual restraint between ligaments, M ii (i=1-6), F ii (i=1-6) are the internal bending moment and shear force of the arc structure, F iN (i=1-6), F iQ (i=1-6) are the axial force and shear force projected to the ligament direction respectively. E S is the elastic modulus of the material, and U is the total strain energy of the structure.

[0025] Arc Trichirality:

[0026] F R1 +F R2 +F R3 =0

[0027] F R1 =F R2

[0028] F R3 -0.5F R1 -0.5F R2 =0

[0029]

[0030] In the formula is the arc integral angle variable, ligament length L, ligament thickness t, middle circular node radius r and horseshoe radius r0, A is the cross-sectional area of ​​the ligament, I is the inertia product of the ligament about the z axis, F Ri (i=1-3) is the equation for the mutual restraint between ligaments, M ii (i=1-3), F ii are the internal bending moment and shear force of the arc structure, F iN (i=1-3), F iQ (i=1-3) are the axial force and shear force projected to the ligament direction respectively. E S is the elastic modulus of the material, and U is the total strain energy of the structure.

[0031] Equivalent modulus and Poisson's ratio:

[0032] Arc quadrilateral:

[0033]

[0034] Where α, β, and γ are dimensionless structural parameters, eff is the dimensionless effective length, E Sis the elastic modulus of the parent material, E y and v are the equivalent elastic modulus and Poisson’s ratio of the arc quadrilateral structure.

[0035] Arc Hexahandedness:

[0036]

[0037] Where α, β, γ are dimensionless size parameters of the structure, ζ, η are dimensionless load parameters, and E S is the elastic modulus of the parent material, E y and v are the equivalent elastic modulus and Poisson’s ratio of the arc hexachiral structure.

[0038] Arc Trichirality:

[0039]

[0040] Where α, β, γ are dimensionless size parameters of the structure, ζ, η are dimensionless load parameters, and E S is the elastic modulus of the parent material, E y and v are the equivalent elastic modulus and Poisson’s ratio of the arc hexachiral structure.

[0041] And α=t / L, β=r0 / L, γ=r / L, ζ j (j=1-15), η j (j=1-13) is related to the structural parameters and is defined as:

[0042] η1=(f1 2 +f4 2 )(2cos2θ+πcosθsinθ)β 3 ; η2=(f1+f4)sinθcosθ(0.5-2β)α 2 ; η3=(f1+f4)sinθcosθ(1-64β 3 );

[0043]

[0044] Where ah is a dimensionless load parameter, which is related to the structural topology.

[0045] Based on the energy method, the present invention deduces the equivalent elastic modulus and Poisson's ratio of the arc chiral microstructure, and verifies the validity of the theoretical derivation results through experiments and simulation methods. Based on the above theoretical guidance, a functional film with adjustable mechanical properties can be prepared through reasonable structural design without taking up too much material. The microstructure design of the film can greatly reduce the modulus of the overall material, softening the original hard matrix material, and providing theoretical guidance for realizing the precise electromechanical coupling effect between the film and the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1a One of the microstructure schematic diagrams of the flexible sensor designed for the present invention;

[0047] Figure 1b The second schematic diagram of the microstructure of the flexible sensor designed for the present invention;

[0048] Figure 1c The third schematic diagram of the microstructure of the flexible sensor designed for the present invention;

[0049] Figure 2a This is one of the force schematic diagrams of the microstructure designed in the present invention under the action of an external load P;

[0050] Figure 2b The second schematic diagram of the force of the microstructure designed by the present invention under the action of the external load P;

[0051] Figure 2c The third schematic diagram of the force of the microstructure designed by the present invention under the action of the external load P;

[0052] Figure 3 A diagram of the microstructure 3D printing preparation process designed for the present invention;

[0053] Figure 4a The comparison among theory, experiment and finite element method when the four-chiral arc chiral microstructure of the present invention is stretched uniaxially;

[0054] Figure 4b The comparison among theory, experiment and finite element method when the six-chiral arc chiral microstructure of the present invention is stretched uniaxially;

[0055] Figure 4c The comparison among theory, experiment and finite element method when the three-chiral arc chiral microstructure of the present invention is stretched in one direction;

[0056] Figure 5 A schematic diagram of the preparation of the flexible sensor of the present invention;

[0057] Figure 6a This is the law of how the modulus of the four-chiral arc chiral microstructure of the present invention changes with the horseshoe radius when it is stretched uniaxially.

[0058] Figure 6b This is the law of how the modulus of the six-chiral arc chiral microstructure of the present invention changes with the horseshoe radius when it is stretched unidirectionally.

[0059] Figure 6c This is the law of how the modulus of the trichirality arc chiral microstructure of the present invention changes with the horseshoe radius when it is stretched uniaxially. DETAILED DESCRIPTION

[0060] The invention is described in detail below with reference to the accompanying drawings:

[0061] 1 Theoretical derivation:

[0062] based on Figure 1a The derivation process of the arc quadrilateral microstructure design is as follows:

[0063] Step 1: Establish the mechanical model of arc chiral structure and related assumptions;

[0064] The arc chiral structure can be represented by five structural parameters: ligament length L, ligament thickness t, intermediate circular node radius r, horseshoe radius r0, and out-of-plane depth b. For the convenience of description, four dimensionless parameters are defined as: α = t / L, β = r0 / L, γ = r / L, ξ = b / L.

[0065] When the ligament length in the arc chiral structure is much larger than the ligament length, the ligament can be regarded as a beam structure. Therefore, the Euler-Bernoulli beam hypothesis commonly used in material mechanics can be used for analysis, ignoring the shear deformation of the structure. Based on the small deformation theory and linear elasticity hypothesis, the rigid rotation of the circular node is ignored in the calculation and the original size of the structure can be used instead of the deformation size of the structure.

[0066] Step 2: Calculate the constraint force of the arc chiral structure;

[0067] When the arc chiral structure is subjected to a vertical load P, such as Figure 2a , the structure as a whole cannot maintain static equilibrium, and the internal bending moments M1 and M2 of the ligaments are in static equilibrium with the structure. The moment equilibrium equation for the circular node column is:

[0068] ∑M O (F) = M1 + M2 - Pr = 0 (1) The total energy of the structure is divided into bending strain energy and membrane strain energy. The total energy is:

[0069]

[0070] The relative displacement between the parallel ligaments needs to be kept constant, and the deformation coordination equation is:

[0071]

[0072] Combining (1)-(3) can solve the constraint moments M1 and M2, then

[0073]

[0074] Substituting the required M1 and M2 into formula (2), the total energy is calculated as:

[0075]

[0076] The strain in the y direction under the action of force P is:

[0077]

[0078] The structural equivalent elastic modulus can be calculated as:

[0079]

[0080] Considering the overlap between the ligament and the cell, the effective length is calculated as

[0081] L e =L-2√(2rt-t 2 ) (8)

[0082] L e Substituting into equation (7) the effective elastic modulus is

[0083]

[0084] The dimensionless formula (9) is:

[0085]

[0086] in

[0087] In order to calculate the Poisson's ratio of the structure, it is necessary to apply a virtual force F. According to the symmetry of the structural force, the constraint moments M1 and M2 are:

[0088]

[0089] The total energy of the structure can be expressed as:

[0090]

[0091] like Figure 2a , the horizontal strain under the external load P is:

[0092]

[0093] According to the definition of Poisson's ratio:

[0094]

[0095] The Poisson's ratio can be solved by combining equations (6), (11) and (14) and transformed into dimensionless form:

[0096]

[0097] The above part is the theoretical solution of the arc four-handed structure. The theoretical derivation process of the six-handed structure is as follows:

[0098] like Figure 2bAs shown in Figure 2, when the arc hexachiral structure is subjected to an axial force P, an internal constraint force F will be generated between the ligaments of adjacent cells. R At the same time, in order to solve the horizontal displacement in the x direction, it is necessary to apply the corresponding horizontal force F in the horizontal direction of the structure, and the static equilibrium equation is:

[0099] F R1 +F R2 +F R3 +F R4 +F R5 +F R6 =0 (16)

[0100] F R1 -F R4 -0.5F R3 -0.5F R5 +0.5F R6 +0.5F R2 =0 (17)

[0101] F R5 +F R6 -F R2 -F R3 =0 (18)

[0102] Secondly, the structure needs to satisfy the deformation coordination equation:

[0103]

[0104] The total energy of the structure is:

[0105]

[0106] Among them, M ii With F ii for:

[0107]

[0108] And F iN With F iQ As shown in Table 1, in order to solve the above equation, it is necessary to change F Ri (i=1-6) is dimensionless:

[0109] F Ri =f i (θ,r0,t,L)*P(i=1-6) (25)

[0110] Table 1

[0111]

[0112] The strain in the y direction under the external load P is:

[0113]

[0114] The structural equivalent elastic modulus is:

[0115]

[0116] Then the equivalent modulus of the structure is dimensionless:

[0117]

[0118] According to the definition formula of Poisson's ratio, the structural equivalent Poisson's ratio is calculated as;

[0119]

[0120] Then the structural Poisson's ratio is calculated as:

[0121]

[0122] The derivation process of arc trichirality theory is as follows:

[0123] like Figure 2c , the static equilibrium equation of the structure is;

[0124] ∑M=0, that is, F R1 +F R2 +F R3 =0 (31)

[0125] ∑F x =0, that is, F R1 =F R2 (32)

[0126] ∑F y =0, that is, F R3 -0.5F R1 -0.5F R2 =0 (33)

[0127] The total strain energy of the structure is:

[0128]

[0129] The equivalent modulus of the structure is dimensionless:

[0130]

[0131] The equivalent Poisson's ratio of the structure is dimensionless:

[0132]

[0133] In formulas (29)-(36), ah and ζ j (j=1-15) is defined as:

[0134]

[0135] ζ1=(f1 2 +f4 2 )b 3 (π+0.5πcos2θ-2sin2θ);ζ2=(f1 2 +f4 2 )bpa 2 ;ζ3=(f1 2 +f4 2 )sin 2 θ(0.5-2β)α 2 ;ζ4=(f1 2 +f4 2 )cos 2 θ(1-64b 3 );

[0136] ζ5=β 3 {(a 2 +c 2 +e 2 +g 2 )*π+0.5π(b 2 +d 2 +f 2 +h 2 )+6(ab+cd+ef+gh)};ζ6=πα 2 (a 2 +b 2 +c 2 +d 2 +e 2 +f 2 +g 2 +h 2 );

[0137]

[0138] or j (j=1-13) is defined as:

[0139] η1=(f1 2 +f4 2 )(2cos2θ+πcosθsinθ)β 3 ;η2=(f1+f4)sinθcosθ(0.5-2β)α 2 ;η3=(f1+f4)sinθcosθ(1-64b 3 );

[0140]

[0141] 2 Simulation model

[0142] Use Figure 1a to Figure 1c The arc chiral structure shown in the figure is modeled by finite element method. The geometric parameters of the modeling are α = 0.05, β = 0.1, γ = 0.2, η = 0.3, and the ligament length L = 20 mm. Since the value of α is small, the ligament can be regarded as an Euler beam, and the finite element method uses B22 beam elements for meshing. Under the condition of ensuring accurate finite element solution and high computational efficiency, the mesh size is selected as 0.25 mm. The elastic modulus of the material is E S =1400MPa, Poisson's ratio v = 0.45, density is 1120kg / m 3 . The established model was subjected to uniaxial tensile finite element simulation.

[0143] 3. Experimental sample printing and testing:

[0144] The corresponding samples were made by printing Tough 20Resin photosensitive resin samples at Anhui Tuantuan Intelligent Technology Co., Ltd. The printing process is as follows Figure 3 As shown, firstly, a 3D solid model is designed by CAD, and the model is sliced ​​by discrete program, and the scanning path is designed. The generated data will accurately control the movement of the laser scanner and the lifting platform; the laser beam passes through the scanner controlled by the numerical control device, and irradiates the surface of the liquid photosensitive resin according to the designed scanning path, so that a layer of resin in a specific area of ​​the surface is solidified. When a layer is processed, a cross section of the part is generated; then the lifting platform is lowered a certain distance, and another layer of liquid resin is covered on the solidified layer, and then the second layer is scanned. The second solidified layer is firmly bonded to the previous solidified layer, and the three-dimensional workpiece prototype is stacked layer by layer. After the prototype is taken out of the resin, it is solidified, polished, and then electroplated, painted or colored to obtain the required product. The tensile test was carried out on the C45.105 MTS material mechanics testing machine, and the loading speed was set to 5mm / min.

[0145] 4. Comparison of results:

[0146] like Figure 4a , Figure 4b as well as Figure 4c As shown, no matter the modulus or Poisson's ratio, the errors of the theoretical, finite element and experimental solutions of the arc chiral structure are all within 10%, indicating the applicability of the derived theoretical solutions of the modulus and Poisson's ratio.

[0147] 5 Applications:

[0148] like Figure 5As shown in the figure, a necessary condition for the normal operation of the flexible sensor is that the Young's modulus of the substrate needs to be greater than the Young's modulus of the film. When the Young's modulus of the substrate is much greater than that of the film, the flexible electronics is in a stable working state; when the Young's modulus of the substrate is much smaller than that of the film, the flexible electronics will not work properly due to the breakage of the film; when the modulus of the substrate is not much different from that of the film, the strain field of the entire sensor can be controlled under the external load. Therefore, it is still a challenging scientific problem to design the relevant structural film to adapt the stiffness to the substrate.

[0149] like Figure 6a , Figure 6b and Figure 6c As shown in the figure, compared with the original bright resin material, the modulus of the arc chiral structure designed by microstructure is much lower than the modulus of the parent material. At the same time, the macroscopic mechanical properties of the material can be regulated by adjusting the size parameters of the microstructure, and the regulation ability depends on the topological form of the microstructure. The normalized modulus of the arc hexachiral structure can be regulated from 0.001 to 0.012, while the arc quadrichiral structure can be regulated from 0.001 to 0.005, and the trichirality regulation range is 0.0001 to 0.0003. Therefore, the harder materials in engineering can be softened through clever microstructure design to design a reasonable film, which can then be integrated with the soft material PI commonly used as the substrate, and then encapsulated with epoxy resin to design high-performance flexible sensors.

Claims

1. A method for preparing a flexible sensor for human body response detection, characterized in that: From bottom to top, it includes a base layer, a film layer and a packaging layer; reasonable geometric parameters of the film layer structure are selected, the film layer introduces rigid nodes in the honeycomb structure, and introduces a horseshoe-shaped microstructure in the straight structure, and the film layer is prepared based on micro-nano 3D printing technology.

2. The method for preparing a flexible sensor for human body response detection according to claim 1, characterized in that: The base layer is made of polyimide material.

3. The method for preparing a flexible sensor for human body response detection according to claim 1, characterized in that: The horseshoe-shaped microstructure is made of silver nanomaterial with conductive properties.

4. The method for preparing a flexible sensor for human body response detection according to claim 1, characterized in that: The packaging layer is made of epoxy resin material.

5. The method for preparing a flexible sensor for human body response detection according to claim 1, characterized in that: The method for determining the geometric parameters of the thin film layer structure is: Firstly, the redundant constraint force of the microstructure is solved based on the equilibrium differential equation and geometric equation of the structure. On this basis, the total strain energy of the entire structure is determined by the force. Then, the partial derivative of the force in the corresponding direction based on the total strain energy is the displacement required in the force direction; Finally, the equivalent modulus and Poisson's ratio of the microstructure are calculated based on the equivalent strain and equivalent stress of the microstructure.

6. The method for preparing a flexible sensor for human body response detection according to claim 5, characterized in that: The equilibrium differential equation and geometric equation are: Arc quadrilateral: ∑M O (F)=M1+M2-Pr=0 In the formula is the arc integral angle variable, ligament length L, ligament thickness t, middle circular node radius r and horseshoe radius r0, A is the cross-sectional area of ​​the ligament, I is the inertia product of the ligament about the z-axis, M1, M2, P are the constraints and external loads on the structure, E S is the elastic modulus of the material, U is the total strain energy of the structure; Arc Hexahandedness: F R1 +F R2 +F R3 +F R4 +F R5 +F R6 =0 F R1 -F R4 -0.5F R3 -0.5F R5 +0.5F R6 +0.5F R2 =0 F R5 +F R6 -F R2 -F R3 =0 In the formula is the arc integral angle variable, ligament length L, ligament thickness t, middle circular node radius r and horseshoe radius r0, A is the cross-sectional area of ​​the ligament, I is the inertia product of the ligament about the z axis, F Ri (i=1-6) is the equation for the mutual restraint between ligaments, M ii (i=1-6), F ii (i=1-6) are the internal bending moment and shear force of the arc structure, F iN (i=1-6), F iQ (i=1-6) are the axial force and shear force projected to the ligament direction respectively; E S is the elastic modulus of the material, U is the total strain energy of the structure; Arc Trichirality: F R1 +F R2 +F R3 =0 F R1 =F R2 F R3 -0.5F R1 -0.5F R2 =0 In the formula is the arc integral angle variable, ligament length L, ligament thickness t, middle circular node radius r and horseshoe radius r0, A is the cross-sectional area of ​​the ligament, I is the inertia product of the ligament about the z axis, F Ri (i=1-3) is the equation for the mutual restraint between ligaments, M ii (i=1-3), F ii are the internal bending moment and shear force of the arc structure, F iN (i=1-3), F iQ (i=1-3) are the axial force and shear force projected to the ligament direction respectively; E S is the elastic modulus of the material, and U is the total strain energy of the structure.

7. The method for preparing a flexible sensor for human body response detection according to claim 5, characterized in that: Equivalent modulus and Poisson's ratio: Arc quadrilateral: Where α, β, and γ are dimensionless structural parameters, eff is the dimensionless effective length, E S is the elastic modulus of the parent material, E y and v are the equivalent elastic modulus and Poisson’s ratio of the arc quadrilateral structure; Arc Hexahandedness: Where α, β, γ are dimensionless size parameters of the structure, ζ, η are dimensionless load parameters, and E S is the elastic modulus of the parent material, E y and v are the equivalent elastic modulus and Poisson’s ratio of the arc hexachiral structure; Arc Trichirality: Where α, β, γ are dimensionless size parameters of the structure, ζ, η are dimensionless load parameters, and E S is the elastic modulus of the parent material, E y and v are the equivalent elastic modulus and Poisson’s ratio of the arc trichirality structure; And α=t / L, β=r0 / L, γ=r / L, ζ j (j=1-15), η j (j=1-13) is related to the structural geometric parameters and is defined as: η1=(f1 2 +f4 2 )(2cos2θ+πcosθsinθ)β 3 ; η2=(f1+f4)sinθcosθ(0.5-2β)α 2 ; η3=(f1+f4)sinθcosθ(1-64β 3 ); Where ah is a dimensionless load parameter, which is related to the structural topology.