High-temperature rollable micro-nano hierarchical porous inorganic composite thermal insulation material and low-carbon preparation method thereof
Through the three-layer structure of micro-nano multi-stage pore inorganic composite insulation materials, combined with oxide ceramic fibers, oxide ceramic hollow beads and modified graphene, the existing high-temperature pipeline insulation materials are easily deformed and thermal conductivity at high temperatures. The problem of elevation achieves efficient thermal insulation performance and simplified preparation process, which is suitable for the application of high-temperature pipelines.
Patent Information
- Application Number
- CN202411127988.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Existing high-temperature pipeline insulation materials are prone to deformity at high temperatures, have an increase in thermal conductivity, have a long production cycle and high energy consumption, and have problems such as insufficient strength and easy cracking, making it difficult to meet the needs of efficient thermal insulation performance.
Micronano multi-stage pore inorganic composite thermal insulation material with a three-layer structure, the inner layer consists of oxide ceramic fibers, oxide ceramic hollow beads and modified graphene, and the middle layer is composed of oxide ceramic hollow beads and silica aerogel powder The outer layer consists of glass fiber and glass hollow beads, and is prepared by centrifugation to form a multi-stage pore structure to improve thermal insulation performance and curlability.
It realizes low thermal conductivity, good flexibility and high strength insulation performance at high temperatures, simplifies the preparation process, reduces cost and energy consumption, and is suitable for high-temperature pipelines of 800-900℃.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic thermal insulation materials, and in particular to a high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material and a low-carbon preparation method thereof. Background Art
[0002] High-temperature equipment and the pipelines between high-temperature equipment need to be equipped with thermal insulation materials. At present, the thermal insulation materials of high-temperature pipelines are mainly prepared from soft and curlable cotton felt materials, such as rock wool, aluminum silicate wool, glass wool, etc., which have good curling properties and can be wrapped on the pipeline in multiple layers according to the required thickness for insulation; hard inorganic thermal insulation materials with a certain strength prefabricated into a tube shell shape, such as calcium silicate, expanded perlite materials, etc., can also be used. They can be prefabricated according to the diameter of the insulation pipeline and buckled on the pipeline for insulation. The above-mentioned soft or hard insulation materials are usually prepared from a main raw material and a small amount of auxiliary materials. The pore size formed inside the material is relatively single, so that its thermal conductivity increases rapidly with the increase of temperature. Especially when used at higher temperatures, soft materials are easy to deform, and a large gap is generated between the insulation material and the insulation equipment such as the pipeline, causing serious heat loss; while hard materials are easy to pulverize and easily disconnected from the pipeline, losing their insulation ability. In recent years, multi-cavity ceramic composite insulation materials have emerged that are between soft materials and hard materials. They have a certain degree of curling, are not easy to deform, and have good insulation performance at higher temperatures. However, the preparation of current multi-cavity ceramic composite insulation materials requires a long drying process, high energy consumption, long production cycle, and has problems such as poor strength and easy cracking. There are still deficiencies in insulation performance, and the curling performance needs to be improved. Therefore, the preparation of inorganic insulation materials with better insulation performance is still a problem to be solved. Summary of the invention
[0003] The purpose of the present invention is to provide a high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material and a low-carbon preparation method thereof to solve the problems existing in the above-mentioned prior art. The composite thermal insulation material of the present invention has good comprehensive performance (fireproof, small thermal conductivity (small change in thermal conductivity at high temperature), good flexibility), is easy to use, and has a low preparation cost, which is in line with the current low-carbon preparation direction.
[0004] To achieve the above object, the present invention provides the following solutions:
[0005] One of the technical solutions of the present invention is: a high temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material, the composite thermal insulation material is a three-layer structure of inner, middle and outer layers;
[0006] In terms of weight, the raw materials of the inner layer include: 45-55 parts of oxide ceramic fibers, 25-35 parts of oxide ceramic hollow beads, 4-6 parts of perlite, 4-6 parts of modified graphene, 1-3 parts of a binder and 2-4 parts of a dispersant;
[0007] The raw materials of the middle layer include, by weight: 25-35 parts of oxide ceramic fibers, 45-55 parts of oxide ceramic hollow beads, 8-12 parts of silica aerogel powder, 4-6 parts of binder and 4-6 parts of dispersant;
[0008] Calculated by weight, the raw materials of the outer layer include: 45-55 parts of glass fiber, 25-35 parts of hollow glass beads, 8-12 parts of wood cellulose, 4-6 parts of binder and 4-6 parts of dispersant.
[0009] Further, the oxide ceramic hollow beads include aluminum oxide hollow microbeads and / or silicon oxide hollow microbeads;
[0010] The oxide ceramic fibers include one or more of alumina fibers, zirconium oxide fibers, and aluminum silicate fibers;
[0011] The modified graphene is graphene coated with chromium or iron on the surface, and the coating thickness is 0.1-0.2 μm; the sheet diameter of the graphene is 10-20 μm, and the thickness is 100-300 nm.
[0012] The iron or chromium coated on the surface of graphene can effectively reflect thermal radiation from high-temperature pipes, further improving the thermal insulation effect.
[0013] Further, the binder includes polyvinyl alcohol;
[0014] The dispersant consists of a foaming agent and polyborosiloxane in a weight ratio of 3:2.
[0015] Further, the glass fiber has a diameter of 5 to 10 microns and a length of 7 to 9 centimeters;
[0016] The diameter of the wood cellulose and oxide ceramic fibers are both 5 to 10 microns and the length is both 3 to 5 centimeters;
[0017] The particle size of the oxide ceramic hollow beads is 10 to 30 microns;
[0018] The particle size of the agglomerates of the silica aerogel powder is 10 to 50 microns;
[0019] There are a large number of nanopores inside the agglomerates of silica aerogel powder. Together with the oxide ceramic hollow beads, they fill the larger pores formed by the fibers to form multi-level pores ranging from microns to nanometers, which greatly improves the thermal insulation performance and increases the overall density and strength of the composite thermal insulation material.
[0020] The size of the perlite is 200 mesh;
[0021] The particle size of the hollow glass beads is 20 to 50 microns.
[0022] Furthermore, in the raw materials of the middle layer, the oxide ceramic hollow beads are composed of silicon oxide hollow microspheres and aluminum oxide hollow microspheres in a weight ratio of 30:20; in the raw materials of the inner layer, the oxide ceramic hollow beads are composed of silicon oxide hollow microspheres and aluminum oxide hollow microspheres in a weight ratio of 20:10;
[0023] The silicon oxide hollow microspheres and the aluminum oxide hollow microspheres are distributed differently in the middle layer and the inner layer, forming different porosities, which plays a great role in improving the thermal insulation performance of the thermal insulation material.
[0024] The inner layer of the composite insulation material contacts high-temperature components such as high-temperature pipes, the outer layer is combined with the inner layer and contacts the external environment, and the middle layer connects the inner and outer layers. The porosity of the composite insulation material increases from the outer layer to the middle layer, and decreases from the middle layer to the inner layer.
[0025] Oxide ceramic fiber materials have high temperature resistance, and oxide ceramic fibers with a certain length (about 3 to 5 cm) can make the insulation material have good overall connection performance and curlability. The length of the oxide ceramic fibers used in the middle and inner layers is slightly shorter, which can increase the contact area between the fibers and the particles, which is beneficial to improve the porosity. The length of the glass fibers in the outer layer is slightly longer, which can increase the flexibility of the material, but the fiber length cannot be too long or too short. Too long fiber length (up to 10 cm) is not conducive to the mixing and uniformity of the materials, and too short length (less than 3 cm) affects the toughening effect and curlability. The fibers in the outer layer include longer glass fibers and shorter wood cellulose, which give it a better toughening effect. The fiber ratio of the outer layer and the inner layer is higher, which can make the material have better curling performance; the glass hollow beads and oxide ceramic hollow beads play a filling role between the fibers. On the one hand, they can fill the larger pores formed by the fibers to improve the thermal insulation capacity. On the other hand, they can give the thermal insulation material a certain strength so that it will not deform under its own weight and high temperature conditions; in the middle layer, the oxide ceramic hollow beads and silica aerogel powder are added together to form multi-level pores of microns and nanometers. This multi-level pore plays an important role in improving the thermal insulation performance of the thermal insulation material. In addition, the porosity increases from the outer layer to the middle layer, while the porosity decreases from the middle layer to the inner layer, which is conducive to the improvement of thermal insulation performance and curling performance; the perlite in the inner layer can expand when used at high temperature, so that the thermal insulation material and equipment such as pipelines maintain close contact. Graphene coated with iron or chromium can play the role of far-infrared radiation and inhibit radiation heat transfer; binders (polyvinyl alcohol) and dispersants can improve the rheological properties and pore formation performance of the inner, middle and outer layers. The composite thermal insulation material with the three-layer structure has excellent thermal insulation performance, especially when used at a high temperature of more than 600°C, the performance is more outstanding than that of existing thermal insulation materials.
[0026] Technical solution 2 of the present invention: A low-carbon preparation method of the above-mentioned high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material, comprising the following steps:
[0027] (1) Preparation of outer layer slurry: After adding dispersant to water and mixing evenly, add glass fiber and wood cellulose, stir for 10 hours, fully disperse to obtain mixed slurry, then add hollow glass beads and binder, continue stirring for 5 to 10 hours, and let stand for 4 to 6 hours to obtain outer layer slurry;
[0028] (2) Preparation of middle layer slurry: After adding the dispersant to water and mixing evenly, add the oxide ceramic fiber and stir for 10 hours to fully disperse the mixed slurry. Then add the oxide ceramic hollow beads, silica aerogel powder and binder, continue stirring for 5 to 10 hours, and let stand for 4 to 6 hours to obtain the middle layer slurry.
[0029] (3) Preparation of inner layer slurry: After adding the dispersant to water and mixing evenly, add the oxide ceramic fiber and modified graphene, stir for 10 hours, fully disperse to obtain a mixed slurry, then add the oxide ceramic hollow beads, perlite and binder, continue stirring for 5 to 10 hours, and let stand for 4 to 6 hours to obtain the inner layer slurry;
[0030] (4) placing an outer layer of slurry in a centrifugal barrel (made of stainless steel), rotating the centrifugal barrel at a centrifugal linear velocity of 8 to 10 m / s, then decelerating to a centrifugal linear velocity of 4 to 6 m / s, and finally increasing to a centrifugal linear velocity of 8 to 12 m / s, to obtain an outer layer of thermal insulation material attached to the wall of the centrifugal barrel;
[0031] (5) placing the middle layer slurry in the centrifugal bucket, rotating the centrifugal bucket at a centrifugal linear velocity of 10 to 12 m / s, then decelerating to a centrifugal linear velocity of 5 to 7 m / s, and finally increasing to a centrifugal linear velocity of 10 to 14 m / s, and the middle layer is attached to the outer layer;
[0032] (6) placing the inner layer slurry in the centrifugal barrel, rotating the centrifugal barrel at a centrifugal linear velocity of 12 to 14 m / s, then decelerating to a centrifugal linear velocity of 6 to 8 m / s, and finally increasing to a centrifugal linear velocity of 10 to 14 m / s, and the inner layer is attached to the above-mentioned middle layer;
[0033] (7) The three-layer thermal insulation material obtained in step (6) is naturally dried until the moisture content of the outer layer is 8-12%, and is removed from the centrifugal bucket to obtain the high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material (thermal insulation material).
[0034] Furthermore, in steps (4) to (6), the rotation time under each centrifugal linear velocity condition is 10 to 15 minutes.
[0035] The thermal insulation material has a specific water content after being formed, so that the thermal insulation material has good curling performance.
[0036] Steps (1) to (3) can be performed simultaneously, and the process of segmented dispersion and mixing can achieve the best mixing uniformity of each layer of slurry. After the outer layer of slurry is placed in the centrifugal bucket, the centrifugal bucket rotates. Driven by centrifugal force, the outer layer of slurry will adhere to the side wall surface of the centrifugal bucket. As the water content in the outer layer of slurry decreases, the outer layer of slurry can be completely attached to the side wall surface of the centrifugal bucket. The centrifugal linear velocity refers to the speed of the edge of the centrifugal bucket wall. The rotation process of the outer layer of slurry in the centrifugal bucket is divided into three stages. The centrifugal linear velocity in the first stage is 8 to 10 m / s, so that the outer layer of slurry quickly climbs along the wall of the centrifugal bucket and basically evenly adheres to the wall of the centrifugal bucket; the centrifugal linear velocity in the second stage is 4 to 6 m / s, and the deceleration is to continue to reduce the water content in the outer layer of slurry while making the outer layer gradually dense; the centrifugal linear velocity of the centrifugal bucket in the third stage increases again to 8 to 12 m / s, so that the water content in the outer layer is further reduced and the density of the outer layer is further increased. Controlling the centrifugal rotation time of each stage to 10 to 15 minutes can ensure the density of each layer of material and allow sufficient time for each component particle of different particle size and weight to be evenly distributed during the rotation process of the vibration state. In addition, the centrifugal method can remove a large amount of water in the preparation process of the thermal insulation material, avoid the subsequent long-term drying process, and achieve the purpose of low-carbon preparation.
[0037] The thermal insulation material of the present invention is a three-layer structure with varying porosity formed by three feedings. The outer layer has the most fibers and contains a certain amount of water, giving the material better curling performance; the middle layer has the largest porosity and forms micron-nano multi-level cavities to improve thermal insulation performance; the inner layer improves the material's high temperature resistance. The thermal insulation material prepared by the method of the present invention can be cut to obtain a planar thermal insulation material. The diameter and height of the centrifugal barrel determine the length and width of the thermal insulation material. The size of the centrifugal barrel can be selected according to specific requirements.
[0038] The third technical solution of the present invention: an application of the above-mentioned high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material in the thermal insulation of high-temperature equipment.
[0039] The present invention discloses the following technical effects:
[0040] (1) The composite thermal insulation material of the present invention has good comprehensive properties, such as fire resistance, low thermal conductivity (small change in thermal conductivity at high temperature), good flexibility, etc.
[0041] (2) After repeated tests and inspections, the present invention has determined the component ratio and the combination of the three-layer structure of the composite thermal insulation material, and combined with the different particle sizes of multiple components and the modification of the components, the thermal insulation material has excellent thermal insulation performance. The inner layer has good far-infrared radiation performance, reducing radiation heat transfer; the middle layer has excellent thermal convection and thermal conduction barrier capabilities; and the outer layer has good thermal conduction barrier capabilities. In addition, the porosity of the two adjacent layers of materials is controlled so that the porosity of the two adjacent layers of materials has a certain gradient, further increasing the thermal insulation performance of the thermal insulation material. The outer layer of the thermal insulation material has a specific moisture content and a high fiber content, which makes the thermal insulation material have excellent curling ability. The inner layer uses high-temperature resistant raw materials so that it can be used in high-temperature pipelines and equipment at 800 to 900°C. At the same time, the preparation method of the thermal insulation material of the present invention is simpler in process than the prior art, which shortens the preparation time, greatly reduces the preparation cost and saves energy, thereby achieving low-carbon preparation. DETAILED DESCRIPTION
[0042] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0043] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0044] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0045] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0046] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0047] The “parts” described in the following examples are all “parts by weight”.
[0048] The centrifugal bucket used in the present invention is made of stainless steel, has a size of φ1000-φ1200 mm, and a height of 450-550 mm.
[0049] Example 1
[0050] A low-carbon preparation method for a high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material:
[0051] (1) Preparation of outer layer slurry: 5 parts of dispersant were added to 100 parts of water and mixed evenly, then 50 parts of glass fiber and 10 parts of wood cellulose were added, stirred (stirring speed was 10 m / s) for 10 hours, and the mixed slurry was fully dispersed, then 30 parts of hollow glass beads and 5 parts of binder were added, and the stirring was continued for 8 hours, and the mixture was allowed to stand for 5 hours to obtain the outer layer slurry;
[0052] Wherein, the dispersant is composed of a foaming agent (sodium dodecylbenzene sulfonate) and polyborosiloxane in a weight ratio of 3:2;
[0053] The diameter of glass fiber is 5 to 10 microns and the length is 7 to 9 centimeters;
[0054] The diameter of lignocellulose is 5 to 10 micrometers and the length is 3 to 5 centimeters;
[0055] The particle size of hollow glass beads is 20 to 50 microns;
[0056] The binder is polyvinyl alcohol.
[0057] (2) Preparation of middle layer slurry: 5 parts of dispersant were added to 100 parts of water, mixed evenly, and then 30 parts of oxide ceramic fibers were added, stirred (stirring speed was 12 m / s) for 10 hours, and the mixed slurry was fully dispersed. Then, 50 parts of oxide ceramic hollow beads, 10 parts of silica aerogel powder and 5 parts of binder were added, and the stirring was continued for 8 hours. The mixture was allowed to stand for 5 hours to obtain the middle layer slurry.
[0058] Wherein, the dispersant is composed of a foaming agent and polyborosiloxane in a weight ratio of 3:2;
[0059] The diameter of oxide ceramic fibers (aluminum silicate fibers) is 5 to 10 microns and the length is 3 to 5 centimeters;
[0060] The particle size of the oxide ceramic hollow beads is 10 to 30 microns; the oxide ceramic hollow beads are composed of silicon oxide hollow microbeads and aluminum oxide hollow microbeads in a weight ratio of 30:20;
[0061] The particle size of the agglomerates of silica aerogel powder is 10 to 50 microns;
[0062] The binder is polyvinyl alcohol.
[0063] (3) Preparation of inner layer slurry: 3 parts of dispersant were added to 100 parts of water and mixed evenly, and then 50 parts of oxide ceramic fiber and 5 parts of modified graphene were added, stirred (stirring speed was 14 m / s) for 10 hours, and the mixed slurry was fully dispersed. Then 30 parts of oxide ceramic hollow beads, 5 parts of perlite and 2 parts of binder were added, and the stirring was continued for 10 hours. The mixture was allowed to stand for 6 hours to obtain the inner layer slurry;
[0064] Wherein, the dispersant is composed of a foaming agent and polyborosiloxane in a weight ratio of 3:2;
[0065] The diameter of oxide ceramic fibers (alumina fibers) is 5 to 10 microns and the length is 3 to 5 centimeters;
[0066] The modified graphene is graphene coated with chromium on the surface, and the coating thickness is 0.1 μm; the diameter of the graphene sheet is 10-20 μm, and the thickness is 100-300 nm;
[0067] The particle size of the oxide ceramic hollow beads is 10 to 30 microns; the oxide ceramic hollow beads are composed of silicon oxide hollow microbeads and aluminum oxide hollow microbeads in a weight ratio of 20:10;
[0068] The size of perlite is 200 mesh;
[0069] The binder is polyvinyl alcohol.
[0070] (4) placing the outer layer slurry in a centrifugal bucket, rotating the centrifugal bucket at a centrifugal linear velocity of 8 m / s (rotation time of 15 minutes), then decelerating to a centrifugal linear velocity of 4 m / s (rotation time of 15 minutes), and finally accelerating to a centrifugal linear velocity of 8 m / s (rotation time of 15 minutes), to obtain an outer layer of thermal insulation material attached to the wall of the centrifugal bucket;
[0071] (5) placing the middle layer slurry in the centrifuge bucket, rotating the bucket at a centrifugal linear velocity of 10 m / s (rotation time of 15 minutes), then decelerating to a centrifugal linear velocity of 5 m / s (rotation time of 15 minutes), and finally increasing to a centrifugal linear velocity of 10 m / s (rotation time of 15 minutes), and the middle layer is attached to the outer layer;
[0072] (6) The inner layer slurry is placed in the centrifuge bucket, and the centrifuge bucket is rotated at a centrifugal linear velocity of 12 m / s (rotation time is 15 minutes), then decelerated to a centrifugal linear velocity of 6 m / s (rotation time is 15 minutes), and finally accelerated to a centrifugal linear velocity of 12 m / s (rotation time is 15 minutes), and the inner layer is attached to the above-mentioned middle layer;
[0073] (7) The three-layer thermal insulation material obtained in step (6) is naturally dried until the moisture content of the outer layer is 10%, and is removed from the centrifugal bucket to obtain a high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material (thermal insulation material).
[0074] The inner layer porosity of the thermal insulation material prepared in this embodiment is 75%, and the pore size is a few microns to 30 microns (determined by the gaps between the oxide ceramic hollow beads and the oxide ceramic fibers and the particles);
[0075] The middle layer has a porosity of 80% and a pore size of several micrometers to 30 micrometers and 30 nanometers to 50 nanometers (determined by the gaps between silica aerogel powder, oxide ceramic hollow beads and oxide ceramic fibers and particles);
[0076] The porosity of the outer layer is 70%, and the pore size is from a few microns to 50 microns (determined by the gaps between the hollow glass beads and fibers (glass fibers, wood cellulose) and particles).
[0077] The thermal insulation material of this embodiment adopts a three-layer structure. A certain amount of graphene coated with chromium and iron is added to the innermost layer, which can increase the far-infrared radiation capacity, and the emissivity is 0.92. Adding an appropriate amount of silica aerogel powder to the middle layer can obtain multi-size pores from nanometer to micrometer level, which can greatly reduce thermal convection. The room temperature thermal conductivity is as low as 0.036W / mk, and the thermal conductivity at 600℃ is less than 0.088W / mk, which is about half of that of aluminum silicate wool. When the same thermal insulation effect is achieved, the thickness used is only half of that of aluminum silicate wool. The inner layer adopts high-temperature resistant oxide ceramic fibers and oxide ceramic hollow beads, which can make the thermal insulation material of the present invention be used for high temperatures of 800-900℃, which is higher than common inorganic thermal insulation materials such as aerogel felt and aluminum silicate wool. The tensile strength of the thermal insulation material prepared by the method of the present invention is 125kPa.
[0078] The present invention combines fibers and hollow microspheres to give the thermal insulation material a certain degree of flexibility and strength. Therefore, the thermal insulation material prepared by the method of the present invention has a tensile strength greater than 120 kPa; a room temperature thermal conductivity less than 0.04 W / mk, and a 600°C thermal conductivity less than 0.09 W / mk; a curling performance that can be folded to 90°; and no cracking occurs after 100 repetitions.
[0079] Comparative Example 1
[0080] Same as Example 1, except that the raw material of the inner layer does not contain oxide ceramic fibers;
[0081] The raw materials of the middle layer do not contain oxide ceramic fibers;
[0082] The outer layer does not contain glass fiber in its raw materials;
[0083] The specific method is as follows:
[0084] (1) Preparation of outer layer slurry: 5 parts of dispersant were added to 100 parts of water and mixed evenly, then 10 parts of wood cellulose were added and stirred (stirring speed was 10 m / s) for 10 hours to fully disperse the mixed slurry, then 30 parts of hollow glass beads and 5 parts of binder were added, and stirring was continued for 8 hours, and the mixture was allowed to stand for 5 hours to obtain the outer layer slurry;
[0085] Wherein, the dispersant is composed of a foaming agent (sodium dodecylbenzene sulfonate) and polyborosiloxane in a weight ratio of 3:2;
[0086] The diameter of lignocellulose is 5 to 10 micrometers and the length is 3 to 5 centimeters;
[0087] The particle size of hollow glass beads is 20 to 50 microns;
[0088] The binder is polyvinyl alcohol.
[0089] (2) Preparation of middle layer slurry: 5 parts of dispersant were added to 100 parts of water, and the mixture was stirred evenly (stirring speed was 12 m / s) for 10 hours to obtain a mixed slurry. Then, 50 parts of oxide ceramic hollow beads, 10 parts of silica aerogel powder and 5 parts of binder were added, and the mixture was stirred for 8 hours and allowed to stand for 5 hours to obtain a middle layer slurry.
[0090] Wherein, the dispersant is composed of a foaming agent and polyborosiloxane in a weight ratio of 3:2;
[0091] The particle size of the oxide ceramic hollow beads is 10 to 30 microns; the oxide ceramic hollow beads are composed of silicon oxide hollow microbeads and aluminum oxide hollow microbeads in a weight ratio of 30:20;
[0092] The particle size of the agglomerates of silica aerogel powder is 10 to 50 microns;
[0093] The binder is polyvinyl alcohol.
[0094] (3) Preparation of inner layer slurry: 3 parts of dispersant were added to 100 parts of water, mixed evenly, and then 5 parts of modified graphene were added, stirred (stirring speed was 14 m / s) for 10 hours, and the mixed slurry was fully dispersed. Then 30 parts of oxide ceramic hollow beads, 5 parts of perlite and 2 parts of binder were added, and the stirring was continued for 10 hours. The mixture was allowed to stand for 6 hours to obtain the inner layer slurry;
[0095] Wherein, the dispersant is composed of a foaming agent and polyborosiloxane in a weight ratio of 3:2;
[0096] The modified graphene is graphene coated with chromium on the surface, and the coating thickness is 0.1 μm; the diameter of the graphene sheet is 10-20 μm, and the thickness is 100-300 nm;
[0097] The particle size of the oxide ceramic hollow beads is 10 to 30 microns; the oxide ceramic hollow beads are composed of silicon oxide hollow microbeads and aluminum oxide hollow microbeads in a weight ratio of 20:10;
[0098] The size of perlite is 200 mesh;
[0099] The binder is polyvinyl alcohol.
[0100] Steps (4) to (7) are the same as in Example 1.
[0101] The thermal insulation material prepared in this comparative example has poor flexibility and loses its curling property, and is easily cracked and powdered after drying.
[0102] Comparative Example 2
[0103] Same as Example 1, except that the raw material of the inner layer does not contain oxide ceramic hollow beads;
[0104] The raw materials of the middle layer do not contain oxide ceramic hollow beads;
[0105] The raw materials of the outer layer do not contain hollow glass beads;
[0106] The specific preparation method is as follows:
[0107] (1) Preparation of outer layer slurry: 5 parts of dispersant were added to 100 parts of water and mixed evenly, and then 50 parts of glass fiber and 10 parts of wood cellulose were added and stirred (stirring speed was 10 m / s) for 10 hours to fully disperse the mixed slurry, and then 5 parts of binder were added, and the mixture was stirred for 8 hours and allowed to stand for 5 hours to obtain the outer layer slurry;
[0108] The dispersant is composed of a foaming agent (sodium dodecylbenzene sulfonate) and polyborosiloxane in a weight ratio of 3:2;
[0109] The diameter of glass fiber is 5 to 10 microns and the length is 7 to 9 centimeters;
[0110] The diameter of lignocellulose is 5 to 10 micrometers and the length is 3 to 5 centimeters;
[0111] The binder is polyvinyl alcohol.
[0112] (2) Preparation of middle layer slurry: 5 parts of dispersant were added to 100 parts of water, mixed evenly, and then 30 parts of oxide ceramic fiber were added, stirred (stirring speed was 12 m / s) for 10 hours, and the mixed slurry was fully dispersed. Then 10 parts of silica aerogel powder and 5 parts of binder were added, and the stirring was continued for 8 hours. The mixture was allowed to stand for 5 hours to obtain the middle layer slurry.
[0113] Wherein, the dispersant is composed of a foaming agent and polyborosiloxane in a weight ratio of 3:2;
[0114] The diameter of oxide ceramic fibers (aluminum silicate fibers) is 5 to 10 microns and the length is 3 to 5 centimeters;
[0115] The particle size of the agglomerates of silica aerogel powder is 10 to 50 microns;
[0116] The binder is polyvinyl alcohol.
[0117] (3) Preparation of inner layer slurry: 3 parts of dispersant were added to 100 parts of water and mixed evenly, and then 50 parts of oxide ceramic fiber and 5 parts of modified graphene were added and stirred (stirring speed was 14 m / s) for 10 hours to fully disperse the mixed slurry, and then 5 parts of perlite and 2 parts of binder were added, and the stirring was continued for 10 hours. The mixture was allowed to stand for 6 hours to obtain the inner layer slurry;
[0118] Wherein, the dispersant is composed of a foaming agent and polyborosiloxane in a weight ratio of 3:2;
[0119] The diameter of oxide ceramic fibers (alumina fibers) is 5 to 10 microns and the length is 3 to 5 centimeters;
[0120] The modified graphene is graphene coated with chromium on the surface, and the coating thickness is 0.1 μm; the diameter of the graphene sheet is 10-20 μm, and the thickness is 100-300 nm;
[0121] The size of perlite is 200 mesh;
[0122] The binder is polyvinyl alcohol.
[0123] Steps (4) to (7) are the same as in Example 1.
[0124] The thermal insulation material prepared in this comparative example has poor deformation resistance and thermal insulation capacity, is easily compressed and deformed, and has significantly improved high-temperature thermal conductivity, with the thermal conductivity being nearly doubled at 600°C.
[0125] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A high temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material, It is characterized in that The composite thermal insulation material has a three-layer structure of inner, middle and outer layers; In terms of weight, the raw materials of the inner layer include: 45-55 parts of oxide ceramic fibers, 25-35 parts of oxide ceramic hollow beads, 4-6 parts of perlite, 4-6 parts of modified graphene, 1-3 parts of a binder and 2-4 parts of a dispersant; The raw materials of the middle layer include, by weight: 25-35 parts of oxide ceramic fibers, 45-55 parts of oxide ceramic hollow beads, 8-12 parts of silica aerogel powder, 4-6 parts of binder and 4-6 parts of dispersant; Calculated by weight, the raw materials of the outer layer include: 45-55 parts of glass fiber, 25-35 parts of hollow glass beads, 8-12 parts of wood cellulose, 4-6 parts of binder and 4-6 parts of dispersant.
2. The high temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material according to claim 1, It is characterized in that The oxide ceramic hollow beads include aluminum oxide hollow microbeads and / or silicon oxide hollow microbeads; The oxide ceramic fibers include one or more of alumina fibers, zirconium oxide fibers, and aluminum silicate fibers; The modified graphene is graphene coated with chromium or iron on the surface, and the coating thickness is 0.1-0.2 μm; the sheet diameter of the graphene is 10-20 μm, and the thickness is 100-300 nm.
3. The high temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material according to claim 1, It is characterized in that The binder includes polyvinyl alcohol; The dispersant consists of a foaming agent and polyborosiloxane in a weight ratio of 3:
2.
4. The high temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material according to claim 1, It is characterized in that The glass fiber has a diameter of 5 to 10 microns and a length of 7 to 9 centimeters; The diameter of the wood cellulose and oxide ceramic fibers are both 5 to 10 microns and the length is both 3 to 5 centimeters; The particle size of the oxide ceramic hollow beads is 10 to 30 microns; The particle size of the agglomerates of the silica aerogel powder is 10 to 50 microns; The size of the perlite is 200 mesh; The particle size of the hollow glass beads is 20 to 50 microns.
5. A low-carbon preparation method for the high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material as claimed in any one of claims 1 to 4, It is characterized in that The following steps are involved: The raw materials of the outer layer, the middle layer and the inner layer are added into water respectively, dispersed evenly and then allowed to stand to obtain outer layer slurry, middle layer slurry and inner layer slurry; The outer layer slurry, the middle layer slurry and the inner layer slurry are sequentially coated on the substrate to obtain the high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material.
6. The preparation method according to claim 5, It is characterized in that The standing time is 4 to 6 hours.
7. The preparation method according to claim 5, It is characterized in that The coating method includes centrifugal coating; The coating method of the outer layer slurry specifically comprises: rotating at a centrifugal linear speed of 8 to 10 m / s, then decelerating to 4 to 6 m / s, and finally increasing to 8 to 12 m / s; The coating method of the middle layer slurry specifically comprises: rotating at a centrifugal linear velocity of 10 to 12 m / s, then decelerating to 5 to 7 m / s, and finally increasing to 10 to 14 m / s; The coating method of the inner layer slurry specifically includes: rotating at a centrifugal linear velocity of 12 to 14 m / s, then decelerating to 6 to 8 m / s, and finally increasing to 10 to 14 m / s.
8. The preparation method according to claim 7, It is characterized in that The spinning time under each centrifugal linear speed condition was 10 to 15 minutes.
9. The preparation method according to claim 5, It is characterized in that The preparation method further comprises: after coating the inner layer slurry, naturally drying the slurry until the water content of the outer layer is 8-12%.
10. Use of the high-temperature rollable micro-nano multi-level porous inorganic composite thermal insulation material as claimed in any one of claims 1 to 4 in thermal insulation of high-temperature equipment.
Citation Information
Patent Citations
Electrothermal film based on graphene / iron oxide composite material and preparation method thereof
CN110149738A
Ultra-light heat-insulating and scouring-resistant functional integrated composite material and preparation method thereof
CN113246556A
Rollable micro-nano hierarchical porous ceramic composite thermal insulation material and preparation method thereof
CN114180881A
Sound insulation and heat insulation composite material with gradient structure and construction method thereof
CN117565487A
Pipeline or equipment heat preserving jacket made of soft material
CN204493994U
Cited By
Inorganic composite thermal insulation material for high-temperature liquid sodium pipeline and preparation method of inorganic composite thermal insulation material
CN119430845A
Inorganic composite heat-insulating material for high-temperature liquid sodium pipeline and preparation method thereof
CN119430845B
Inorganic resin fireproof thermal insulation material as well as preparation method and application thereof
CN122010593A