Device and method for testing splitting performance of 3D printing concrete interface
By designing a 3D-printed concrete interface splitting tensile performance testing device, and using a reaction frame and splitting clamps for stable support of the specimen and monitoring of multiple indicators, the problem of low efficiency, poor accuracy and high safety hazards in existing testing methods is solved, and efficient and safe multi-indicator testing is achieved.
Patent Information
- Application Number
- CN202410929882.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-01
AI Technical Summary
Existing methods for testing the interlayer interface performance of 3D printed concrete suffer from problems such as low testing efficiency, high cost, poor accuracy, and significant safety hazards. In particular, the splitting tensile test is inconvenient for specimen placement and has limited testing parameters.
A 3D printed concrete interface splitting tensile performance testing device was designed, including a data acquisition system, a reaction frame, and a splitting clamp. The splitting clamp inside the reaction frame provides stable support for the specimen, and the deformation of the specimen is monitored by a lateral and vertical displacement monitoring mechanism. Combined with a load sensor, the load value is accurately measured to achieve balanced support and multi-index monitoring of the specimen.
It enables convenient and stable placement of test specimens, improves the accuracy and comprehensiveness of test results, reduces the risk of manual operation, and enhances testing efficiency and multi-indicator monitoring capabilities.
Smart Images

Figure CN118883281A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of intelligent manufacturing technology, and in particular to a 3D printed concrete interface splitting performance testing device and a testing method. Background Art
[0002] Compared with traditional construction technology, 3D printed concrete can be directly stacked layer by layer without any formwork support or vibration process. It has the advantages of formwork-free construction, high efficiency, low labor cost, and less construction waste. However, its stacking molding construction process also brings many problems. For example, during the construction process, interlayer interfaces will be generated due to differences in the degree of coagulation and hardening of concrete. The bonding performance of the interlayer interface is directly related to the overall quality of the concrete structure. Therefore, in order to ensure the quality of the project and the safety of the structure, a method that can scientifically evaluate the performance of the interlayer interface of 3D printed concrete must be selected.
[0003] Tensile strength is one of the most basic mechanical properties of concrete. The calculation of the cracking, crack width, deformation of concrete specimens, and the calculation of shear, torsion, punching and other bearing capacities are all related to tensile strength. Concrete is a material with low tensile strength. The tensile strength of ordinary concrete is only one twentieth to one tenth of its compressive strength.
[0004] The stacking molding process of 3D printed concrete causes pores to gather at the interfaces between vertical and horizontal layers and strips, resulting in lower tensile strength and weaker bonding at the interfaces. Sufficient interfacial tensile strength is also one of the key indicators to ensure that 3D printed concrete meets the overall service performance, which also determines the life of 3D printed concrete structures.
[0005] The existing pull-out method for testing the tensile strength of 3D printed concrete specimens is to glue pullers at both ends of the specimen, stretch it through a universal material testing machine, and test the load value when the interface breaks to obtain the interface tensile strength. However, this method has the problem of centering difficulties, and it is difficult to ensure that the load direction is completely perpendicular to the interface, resulting in tensile eccentricity, which will affect the accuracy of the tensile strength test.
[0006] At the same time, the pull-out method requires the specimen and the fixture to be bonded together by an adhesive. When the bond strength of the interface to be tested is high, debonding is likely to occur at the adhesive, resulting in test failure. In addition, this method is inefficient, costly, and will cause certain environmental pollution.
[0007] In view of the problems existing in direct testing of the axial tensile properties of concrete, a splitting tensile test is usually used to evaluate the tensile strength of concrete. The principle is: pads are arranged between the upper and lower surfaces of the concrete specimen and the pressure equipment to form corresponding strip loading surfaces on the upper and lower surfaces of the specimen. After the pressure equipment is operated, the specimen is split and damaged. The force value at the time of splitting can be converted to obtain the tensile strength of the specimen.
[0008] However, since the stress-bearing surface (loading surface) of the specimen must be consistent with the physical center section (predetermined failure surface) of the specimen during the test, the specimen needs to be supported by hand before the specimen is subjected to stress so that the loading surface is consistent with the predetermined failure surface, which results in high labor costs and easily leads to safety problems. For example, in a multifunctional asphalt concrete testing instrument disclosed in patent publication number CN85107635, during the splitting test, the specimen is arranged between the upper and lower pressurizers. In order to ensure the accuracy of the specimen arrangement position, the specimen needs to be temporarily supported by hand.
[0009] Another example is the 3D printed concrete interlayer splitting strength test device disclosed in patent publication number CN220708884U. To ensure the stability of the specimen placement, the specimen is first calibrated by adjusting the level ruler and placed in a horizontal state. Then, the upper and lower telescopic joints and the telescopic plate are adjusted to hold the specimen to achieve a fixed effect. Although no manual support is required, the entire fixing operation is relatively cumbersome, and the test indicator is only pressure load, which is relatively simple. Therefore, it is necessary to develop a more efficient and convenient 3D printed concrete interface splitting performance test device and test method. Summary of the invention
[0010] In order to solve the problems that the specimen cannot be conveniently placed during conventional splitting tensile tests and the test index is single, the present invention provides a 3D printed concrete interface splitting tensile performance testing device and a testing method, which can balance and support the concrete specimen so that it can be placed conveniently and stably, and can not only monitor the load index but also monitor the deformation of the specimen, thereby improving the accuracy of the test results and ensuring the comprehensiveness of the tensile performance evaluation of the specimen.
[0011] To achieve the above purpose, the technical solution adopted by the present invention is:
[0012] A 3D printed concrete interface splitting and tensioning performance testing device includes a data acquisition system and a reaction frame and a splitting and tensioning fixture controlled by the data acquisition system. The splitting and tensioning fixture is arranged in the reaction frame to facilitate the reaction frame to apply force in the splitting and tensioning fixture.
[0013] The splitting and tensioning fixture includes a bottom plate, a frame for placing the test piece, a force transmission column controlled by a reaction frame, a lateral displacement monitoring mechanism for monitoring the lateral deformation value of the test piece, a lifting assembly for driving the lateral displacement monitoring mechanism to rise and fall, and a vertical displacement monitoring mechanism for monitoring the displacement of the force transmission column;
[0014] The frame is vertically arranged above the bottom plate, and a lower arc-shaped pad and an elastic bottom support member for elastically supporting the test piece are arranged at the bottom of the frame. A plurality of the elastic bottom support members are evenly arranged around the lower arc-shaped pad, so as to evenly support the test piece and avoid manually supporting the test piece with hands;
[0015] The force transmission column is elastically slidably connected vertically on the top of the frame. The force transmission column extends upward from the frame and is connected to a load sensor. The force transmission column extends downward into the frame and is connected to an upper arc pad. The upper arc pad and the lower arc pad are arranged in corresponding intervals up and down, which is convenient for splitting loading of the specimen.
[0016] Furthermore, the reaction frame includes a top plate, a base, a support column, a piston cylinder and a piston rod, the top plate and the base are arranged in parallel with each other at intervals, and a plurality of support columns are arranged between the top plate and the base to connect them, thereby improving the reliability of the reaction frame structure;
[0017] The piston cylinder is arranged at the center of the top plate, the piston cylinder is inverted, and the piston rod of the piston cylinder is downward and against the load sensor, so as to facilitate monitoring of the load value applied by the piston cylinder. The bottom plate is bolted to the base, so as to facilitate the disassembly and assembly of the splitting and pulling clamp. The bottom plate and the base are stacked up and down.
[0018] Furthermore, the cross-section of the frame is in the shape of a "U". The center of the frame is transparent from front to back, which is convenient for taking and placing the specimen. The elastic bottom support component includes a lower limit column and a supporting compression spring fixedly mounted on the lower limit column. The supporting compression spring extends vertically upward and rests on the bottom surface of the specimen, so as to flexibly support the specimen.
[0019] Furthermore, the force transmission column is a stepped column structure, the force transmission column is larger at the top and smaller at the bottom, the upper end of the force transmission column extends out of the frame, and the lower end extends into the frame;
[0020] The frame is provided with a vertical limit guide hole, which is a long hole and passes through the side wall of the frame. The lower end of the force transmission column is threadedly connected with a limit screw, which is arranged horizontally and passed through the limit guide hole to facilitate the upward and downward movement of the force transmission column.
[0021] Furthermore, a plurality of elastic top support members are provided between the upper end of the force transmission column and the frame for connection. The plurality of elastic top support members are evenly arranged around the force transmission column to ensure uniform support for the force transmission column. Each elastic top support member includes a top support compression spring and upper limit columns fixedly mounted on both ends of the top support compression spring. The top support compression spring is arranged vertically, and the upper limit columns at both ends are respectively arranged on the upper end of the force transmission column and the top of the frame, so as to realize the elastic installation of the force transmission column on the top of the frame.
[0022] Furthermore, the lower side of the upper arc pad is arc-shaped, the upper side of the lower arc pad is also arc-shaped, and the arc tops of the upper arc pad and the lower arc pad are opposite to each other, so as to ensure that the splitting load can be performed along the predetermined failure surface of the specimen. The diameter of the arc of the upper and lower arc pads is equal to the side length of the specimen.
[0023] Further, the lateral displacement monitoring mechanism comprises a plate frame, a left positioning screw, a right positioning screw and a sliding locker with a lateral displacement meter installed;
[0024] The plate frame and the bottom plate are arranged in parallel up and down, the plate frame is arranged around the three sides of the frame, the left end of the plate frame is threadedly connected with two left positioning screws, the head end of the left positioning screw passes through the side wall of the frame horizontally and abuts against the left side of the test piece, the right end of the plate frame is elastically slidably connected with the right positioning screw, the left positioning screw and the right positioning screw are arranged oppositely to each other on the left and right, the head end of the right positioning screw passes through the side wall of the frame and abuts against the right side of the test piece, and the coordinated clamping of the right positioning screw and the left positioning screw can facilitate the lateral displacement monitoring mechanism to be suspended on the test piece;
[0025] A transverse baffle is arranged on the right positioning screw, and a baffle limiting piece is arranged on the right end of the plate frame, and the baffle limiting piece is fitted with the transverse baffle to separate the head of the right positioning screw from the test piece, so that the test piece is not affected by the right positioning screw and can be conveniently placed in the frame;
[0026] The right end of the plate frame is laterally slidably connected to the sliding lock 1, which is convenient for adjusting the position of the sliding lock 1. A lateral displacement meter is arranged on the sliding lock 1, and the measuring rod of the lateral displacement meter is tightly against the cross baffle, which is convenient for monitoring the displacement of the right positioning screw.
[0027] Furthermore, two conical grooves are symmetrically provided at the center of the horizontal position on the left side of the specimen for abutment of two left positioning screws, and a conical groove is correspondingly provided at the horizontal center of the right side of the specimen for abutment of a right positioning screw, so as to ensure that the lateral displacement monitoring mechanism can always be attached to the specimen and coordinate with the deformation of the specimen during the stress deformation process;
[0028] The left side wall of the frame is provided with two vertically arranged positioning holes for inserting two left positioning screws, and the right side wall of the frame is provided with a vertically arranged positioning hole for inserting a right positioning screw, so as to provide a position space for the upward and downward movement of the positioning screws;
[0029] The lifting assembly is arranged on the bottom plate, and the lateral displacement monitoring mechanism is arranged above the lifting assembly. When the test piece is placed at the test position, the lifting assembly drives the lateral displacement monitoring mechanism to move upward, releases the left positioning screw and the right positioning screw, and makes them abut against the conical groove of the test piece. The lifting assembly is an eccentric lifting structure, and lifting assemblies are arranged on both sides of the frame. There is one lifting assembly on one side, which is convenient for adapting to the left end of the plate frame, and there are two lifting assemblies on the other side, and a rotating shaft is arranged for synchronous transmission, which is convenient for adapting to the right end of the plate frame. The plate frame is arranged between the multiple lifting assemblies above, which is convenient for driving the plate frame to move upward.
[0030] Furthermore, the vertical displacement monitoring mechanism includes a column, a sliding lock 2 equipped with a vertical displacement meter, and a vertical baffle, the column is vertically arranged on the bottom plate, the sliding lock 2 is adjustable up and down on the column, so as to facilitate the adjustment of the installation position of the sliding lock 2, and the sliding lock 2 is provided with a vertically arranged vertical displacement meter;
[0031] The vertical baffle is arranged on the force transmission column, and one end of the vertical baffle extends horizontally to above the vertical displacement meter. The measuring rod of the vertical displacement meter is pressed upward against the vertical baffle, which is convenient for monitoring the displacement of the force transmission column, that is, the vertical deformation of the specimen.
[0032] The 3D printed concrete interface splitting tensile performance test method, based on the above-mentioned 3D printed concrete interface splitting tensile performance test device, comprises the following steps:
[0033] Step 1: Prepare a concrete cube splitting tensile test specimen containing a printed interface by 3D printing technology, prefabricate conical grooves on two sides of the test specimen parallel to the printed interface layer, and maintain the test specimen according to the standard;
[0034] Step 2: Operate the lifting assembly to support the lateral displacement monitoring mechanism, manually pull outward and rotate the right positioning screw to make the horizontal baffle plate stuck on the baffle limiter, and ensure that there is a large distance between the left positioning screw and the right positioning screw to provide enough space for placing the test piece;
[0035] The concrete specimen to be tested is placed on top of a plurality of elastic bottom support members, and the vertical plane where the centers of the upper arc pad and the lower arc pad are located is ensured to be consistent with the printed interface layer of the specimen, i.e., the predetermined failure surface;
[0036] Step 3: Continue to operate the lifting assembly to adjust the height of the left positioning screw and the right positioning screw until the heads of the left positioning screw and the right positioning screw are level with the corresponding conical grooves on the side of the specimen;
[0037] Reversely twist the right positioning screw to reset it. After resetting, the cross baffle will be against the top of the measuring rod of the lateral displacement meter. At the same time, completely loosen the right positioning screw so that the heads of the left and right positioning screws are inserted into the corresponding conical grooves on the side of the specimen, so that the lateral displacement monitoring mechanism is fastened to the specimen;
[0038] Then, operate the lifting assembly in reverse and no longer support the lateral displacement monitoring mechanism, so that the specimen can be deformed freely in the vertical direction; check the horizontal position of the specimen again to ensure that the printed interface layer of the specimen is consistent with the vertical plane where the center of the upper arc pad and the lower arc pad are located; adjust the position of the vertical displacement meter so that the top end of its measuring rod is against the vertical baffle;
[0039] Step 4: After the specimen, lateral displacement meter and vertical displacement meter are installed, turn on the data acquisition system and control computer, and drive the piston rod in the piston cylinder to perform a loading test on the specimen according to the set program. The data acquisition system can easily obtain the full splitting tensile load-deformation curve of the specimen damage, based on which a comprehensive index for evaluating the tensile performance of the specimen can be obtained.
[0040] Through the above technical solution, the beneficial effects of the present invention are:
[0041] The structure of the present invention is reasonable. Since the 3D printed concrete specimen is to be subjected to a splitting test under the clamping of the upper arc pad and the lower arc pad, in order to ensure the stability of the specimen placement and the test accuracy, a plurality of elastic bottom support members are evenly arranged around the lower arc pad, which can provide uniform elastic support for the specimen, ensure the balanced placement of the specimen, and avoid the potential danger of manual holding and the human influence on the test results. At the same time, it can ensure that the loading surface is consistent with the predetermined failure surface of the specimen, and the influence of the elastic bottom support member on the splitting tensile strength test accuracy of the specimen during the splitting tensile process can be ignored.
[0042] The piston cylinder in the reaction frame of the present invention acts on the force transmission column, causing it to move downward and split the specimen through the cooperation of the upper arc pad and the lower arc pad. The load applied by the piston cylinder is monitored by the load sensor, so as to accurately test the load borne by the specimen and obtain the splitting tensile strength value of the specimen. At the same time, the force transmission column is elastically slid on the top of the frame. Under the action of the elastic top support, the force transmission column tends to move upward, so that there is enough space between the upper and lower arc pads before and after the splitting tensile test, which is convenient for the placement and removal of the specimen. The up and down movement and circumferential rotation of the force transmission column are limited by the limit screws, which prompt the force transmission column to move within the specified range, ensuring the integrity of the splitting tensile fixture and the convenience of operation.
[0043] In the present invention, the vertical movement distance of the force transmission column is monitored by the vertical displacement monitoring mechanism, and the displacement of the force transmission column can be monitored by the vertical displacement meter. The installation position of the second sliding lock can be adjusted up and down, and then the position of the vertical displacement meter changes accordingly, which can meet the needs of measuring the maximum vertical deformation value of the specimen and the required gauge length of the vertical displacement meter range.
[0044] The lateral displacement monitoring mechanism in the present invention can monitor the lateral deformation value of the specimen, wherein the entire lateral displacement monitoring mechanism can be arranged in the air on the specimen through the clamping cooperation of the left positioning screw and the right positioning screw. A conical groove is provided on the specimen, and the cooperation between the positioning screw head and the conical groove can prevent the lateral displacement monitoring mechanism from detaching from the specimen. When working, the lateral displacement monitoring mechanism is not supported vertically by the lifting assembly and is arranged separately on the specimen. At this time, the left positioning screw and the right positioning screw are just clamped in the conical grooves reserved on both sides of the specimen, so that the lateral deformation value of the specimen can be accurately tested, that is, the lateral deformation value of the specimen during the force destruction process is measured by the relative displacement between the left positioning screw and the right positioning screw. Moreover, during the splitting process of the specimen, the lateral displacement monitoring mechanism can move freely in the vertical direction with the specimen, so that the test result of the lateral deformation value of the specimen is more accurate.
[0045] The lateral displacement monitoring mechanism of the present invention can meet the needs of measuring the maximum lateral deformation value of the specimen and the required gauge length of the lateral displacement meter range by adjusting the distance between the sliding lock and the transverse baffle to change the position of the transverse displacement meter, thereby accurately testing the deformation value of the specimen. When placing and removing the specimen, the right positioning screw is pulled outward and then rotated to facilitate the clamping of the transverse baffle on the baffle limiter, so that the right positioning screw is moved out of the frame and does not interfere with the placement of the specimen, freeing both hands to place the specimen in the correct position, and also facilitating the removal of the specimen after destruction.
[0046] The lifting assembly of the present invention realizes the lifting and lowering control of the lateral displacement monitoring mechanism by rotating the eccentric wheel through the rotating handle. When the eccentric wheel supports the lateral displacement monitoring mechanism, the tips of the left positioning screw and the right positioning screw can be clamped in the conical grooves reserved on the two sides of the specimen. By rotating the rotating handle clockwise, the lateral displacement monitoring mechanism loses the vertical support of the lifting assembly, and the lateral displacement monitoring mechanism can move freely in the vertical direction with the specimen, ensuring the accuracy of the monitoring of the lateral deformation value of the specimen. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 It is a schematic diagram of the overall structure of the 3D printing concrete interface splitting tensile performance testing device of the present invention.
[0048] Figure 2 It is a front view of the splitting and tensioning fixture of the 3D printing concrete interface splitting and tensioning performance testing device of the present invention.
[0049] Figure 3 It is a side view of the splitting and tensioning fixture of the 3D printing concrete interface splitting and tensioning performance testing device of the present invention.
[0050] Figure 4 It is a schematic diagram of the lateral displacement monitoring mechanism of the 3D printing concrete interface splitting tensile performance testing device of the present invention.
[0051] Figure 5 It is a schematic diagram of conical grooves opened on two opposite sides of a concrete specimen of the 3D printing concrete interface splitting tensile performance testing device of the present invention.
[0052] Figure 6 It is a schematic diagram of the lifting assembly of the 3D printing concrete interface splitting tensile performance testing device of the present invention.
[0053] Figure 7 It is a schematic diagram of the vertical displacement monitoring mechanism of the 3D printing concrete interface splitting tensile performance testing device of the present invention.
[0054] Figure 8 It is a schematic diagram of the full curve of splitting load-lateral vertical deformation of the 3D printed specimen destroyed by the 3D printed concrete interface splitting performance testing method of the present invention.
[0055] The numbers in the attached drawings are: 1 bottom plate, 2 frame, 3 force transmission column, 4 plate frame, 5 lifting seat, 6 lower arc pad, 7 lower limit column, 8 limit guide hole, 9 positioning through hole, 10 support spring, 11 test piece, 12 upper limit column, 13 top support spring, 14 upper arc pad, 15 limit screw, 16 vertical baffle, 17 load sensor, 18 left positioning screw, 19 right positioning screw, 20 baffle limit piece, 21 horizontal baffle, 22 compression spring, 23 sliding lock one , 24 lock hole one, 25 locking bolt one, 26 vertical bolt one, 27 lateral displacement meter, 28 column, 29 sliding hole, 30 lateral bolt one, 31 sliding lock two, 32 lock hole two, 33 locking bolt two, 34 vertical displacement meter, 35 rotating shaft, 36 eccentric wheel, 37 rotating handle, 38 conical groove, 39 predetermined failure surface, 40 top plate, 41 base, 42 support column, 43 piston cylinder, 44 piston rod, 45 computer, 46 controller. DETAILED DESCRIPTION
[0056] The specific implementation of the present invention is described in detail below with reference to the accompanying drawings:
[0057] like Figure 1 to Figure 7 As shown in FIG. 1 , the 3D printed concrete interface splitting performance testing device includes a data acquisition system and a reaction frame and a splitting fixture controlled by the data acquisition system, such as Figure 1 As shown. The data acquisition system includes a computer 45 and a controller 46 connected to the computer 45. The monitoring signals generated by various sensors used in the entire splitting and tensioning fixture are transmitted to the controller 46 through cables, and then transmitted to the computer 45 after signal amplification and conversion. The computer 45 can display the measured data in real time through the display screen and record it in real time. At the same time, the computer 45 analyzes the built-in software system and then continues to issue instructions to control the reaction frame to accurately perform corresponding actions, thereby completing the loading and unloading operations of the concrete specimen 11.
[0058] The reaction frame can be used to apply a load to the concrete specimen 11. The reaction frame includes a top plate 40, a base 41, support columns 42, a piston cylinder 43 and a piston rod 44. The top plate 40 and the base 41 are arranged in parallel at an upper and lower interval. A plurality of support columns 42 are arranged between the top plate 40 and the base 41, thereby connecting and fixing the top plate 40 and the base 41 to form a rectangular space frame 2.
[0059] A piston cylinder 43 is provided at the center of the top plate 40. The piston cylinder 43 is inverted, and the piston rod 44 of the piston cylinder 43 extends downward. The operation of the piston cylinder 43 is controlled by a computer 45 and a controller 46. The piston cylinder 43 is used to apply a load to the splitting fixture and is the power source of the entire reaction frame. The piston rod 44 in the piston cylinder 43 can be driven to complete the ascending and descending movements according to a set program, so as to realize the loading and unloading of the splitting fixture.
[0060] A splitting fixture is arranged inside the reaction frame. The piston cylinder 43 in the reaction frame applies a load and acts on the concrete specimen 11 through the splitting fixture. At the same time, the splitting fixture can conveniently and stably place the concrete specimen 11, and the load and deformation values during the force failure process of the specimen 11 can be monitored through various sensors.
[0061] In this embodiment, the splitting fixture includes a bottom plate 1, a frame 2 for placing the specimen 11, a force transmission column 3 controlled by the reaction frame, a lateral displacement monitoring mechanism for monitoring the lateral deformation value of the specimen 11, a lifting assembly for driving the lateral displacement monitoring mechanism to move up and down, and a vertical displacement monitoring mechanism for monitoring the displacement of the force transmission column 3, as Figure 2 and Figure 3 shown.
[0062] The bottom plate 1 is the installation foundation of the entire splitting fixture. When the bottom plate 1 is installed, the bottom plate 1 is bolted to the base 41 of the reaction frame. After installation, the bottom plate 1 and the base 41 are arranged in an upper and lower stacked manner, realizing the detachable installation of the splitting fixture and the reaction frame.
[0063] A frame 2 is vertically arranged above the bottom plate 1. The concrete specimen 11 can be placed inside the frame 2. The cross section of the frame 2 is in the shape of a "hui" character, that is, the front and back of the center of the frame 2 are transparent. The two sides of the frame 2 have the function of preventing splashing, preventing the concrete debris from splashing outwards during the splitting failure process of the specimen 11.
[0064] A lower arc pad 6 is provided at the center above the bottom of the frame 2. The upper side of the lower arc pad 6 is arc-shaped, and the arc top of the lower arc pad 6 faces upward to form a splitting loading edge line, which is the arc top line here. In order to achieve stable placement and positioning of the test piece 11 without manual support, an elastic bottom support member for elastically supporting the test piece 11 is also provided on the frame 2. The elastic bottom support member can play a role of balancing support for the test piece 11 above it. Specifically, four elastic bottom support members are evenly arranged on the left and right sides of the lower arc pad 6, which can evenly support the test piece 11, so that the predetermined failure surface 39 of the test piece, that is, the 3D printing interface layer, can always coincide with the arc top line of the lower arc pad 6.
[0065] The elastic bottom support member includes a lower limit column 7 and a support compression spring 10 fixedly sleeved above the lower limit column 7, and the support compression spring 10 extends vertically upward and abuts against the bottom surface of the specimen 11. The common support of the four elastic bottom support members can ensure that the predetermined failure surface 39 of the specimen 11 is consistent with the loading surface formed by the upper arc pad 14 and the lower arc pad 6, and the influence of the four support compression springs 10 on the splitting tensile strength test accuracy of the specimen 11 during the splitting tensile process can be ignored.
[0066] A circular hole is provided at the center of the top of the frame 2, and a force transmission column 3 is elastically slidably connected vertically in the circular hole. The force transmission column 3 can move up and down relative to the frame 2. The piston cylinder 43 of the reaction frame acts on the force transmission column 3. A load can be applied to the concrete specimen 11 in the frame 2 through the force transmission column 3, thereby causing the specimen 11 to be split and damaged.
[0067] The force transmission column 3 is a stepped column structure, with a large diameter at the top and a small diameter at the bottom. The upper end of the force transmission column 3 extends out of the frame 2, and the upper end of the force transmission column 3 is always located outside the frame 2 for movement; the force transmission column 3 extends upward outside the frame 2 and is connected to a load sensor 17, and the piston rod 44 of the piston cylinder 43 can be downward and against the load sensor 17, thereby monitoring the force acting on the specimen 11.
[0068] The force transmission column 3 extends downward into the frame 2 and is connected to an upper arc pad 14, the lower side of the upper arc pad 14 is also arc-shaped, and the arc top of the upper arc pad 14 is downwardly facing to form an arc top line. The upper arc pad 14 and the lower arc pad 6 are arranged in a corresponding manner at intervals, and the arc top lines of the upper arc pad 14 and the lower arc pad 6 are relatively formed to form a loading surface.
[0069] In order to realize the elastic sliding of the force transmission column 3, four elastic top supports are arranged between the upper end of the force transmission column 3 and the frame 2, and the connection and installation of the force transmission column 3 are realized through the elastic top supports. The four elastic top supports are evenly arranged around the force transmission column 3, and each elastic top support comprises a top support compression spring 13 and an upper limit column 12 fixedly sleeved on both ends of the top support compression spring 13. The top support compression spring 13 is arranged vertically, and the upper limit columns 12 at both ends are respectively arranged on the upper end of the force transmission column 3 and the top of the frame 2. Under the action of the elastic top supports, the force transmission column 3 can be rebounded and supported, so that the force transmission column 3 is in a suspended state.
[0070] Since the force transmission column 3 can move up and down under the drive of the piston cylinder 43, in order to achieve the limit of movement, vertical limit guide holes 8 are opened on the left and right side walls of the frame 2. The limit guide holes 8 are long holes and penetrate the two side walls of the frame 2. At the same time, the lower end of the force transmission column 3 is threadedly connected to the limit screw 15, which is arranged horizontally and penetrates the limit guide hole 8. Under the cooperation of the limit screw 15 and the limit guide hole 8, the up and down movement of the force transmission column 3 can be limited, and at the same time, the force transmission column 3 can be prevented from rotating circumferentially and falling out upward.
[0071] The reaction frame can apply load to the concrete specimen 11 in the frame 2, and with the cooperation of the upper arc pad 14 and the lower arc pad 6, the specimen 11 is split. The deformation of the specimen 11 during splitting can be monitored through the lateral displacement monitoring mechanism and the vertical displacement monitoring mechanism.
[0072] The lateral displacement monitoring mechanism includes a plate frame 4, a left positioning screw 18, a right positioning screw 19 and a sliding lock 23 equipped with a lateral displacement meter 27. Figure 4 The plate frame 4 and the bottom plate 1 are arranged in parallel up and down, and the cross section of the plate frame 4 is similar to the "6" in the liquid crystal digital font, and the plate frame 4 is arranged around the frame 2 on three sides.
[0073] The left end of the plate frame 4 has an "L"-shaped cross section. The left end of the plate frame 4 is arranged on one side of the frame 2. The left end of the plate frame 4 is threadedly connected with two left positioning screws 18. The two left positioning screws 18 are located on the same plane and are spaced apart. The head end of the left positioning screw 18 passes through the left side wall of the frame 2 horizontally and abuts against the left side of the specimen 11. By turning the left positioning screw 18, its contact with the surface of the specimen 11 can be controlled.
[0074] The cross section of the right end of the plate frame 4 is a "mouth"-shaped frame. The right end of the plate frame 4 is arranged on the other side of the frame 2. A right positioning screw 19 is elastically slidably connected transversely in the "mouth"-shaped frame at the right end of the plate frame 4. The left positioning screw 18 and the right positioning screw 19 are arranged opposite to each other on the left and right. The right positioning screw 19 is arranged between the two left positioning screws 18. The two left positioning screws 18 and the right positioning screw 19 are arranged on the same horizontal plane. When the plate frame 4 is fastened to the specimen, the line connecting the top cone of a right positioning screw 19 and the top cones of the two left positioning screws 18 is an isosceles triangle. The head end of the right positioning screw 19 passes through the side wall of the frame 2 and abuts against the right side of the specimen 11. By pulling the right positioning screw 19, its contact and separation with the surface of the specimen 11 can be controlled.
[0075] The sliding structure of the right positioning screw 19 is as follows: the right positioning screw 19 is longer than the left positioning screw 18, and the right positioning screw 19 is horizontally inserted into the "mouth"-shaped structure at the right end of the plate frame 4. A transverse baffle 21 is provided on the right positioning screw 19, and the movement of the right positioning screw 19 will drive the transverse baffle 21 to move together. At the same time, a compression spring 22 is sleeved on the right positioning screw 19, and one end of the compression spring 22 is against the right limb of the plate frame 4, and the other end is against the transverse baffle 21. The compression spring 22 tends to stretch, which can drive the right positioning screw 19 to move toward the left positioning screw 18, and then the right positioning screw 19 is tightly against the side of the test piece 11.
[0076] Since the right positioning screw 19 tends to extend into the frame 2, in the process of installing and removing the test piece 11, in order to avoid the interference of the right positioning screw 19, the right positioning screw 19 needs to be temporarily moved outward to ensure the smooth placement and removal of the test piece 11. At this time, a baffle stopper 20 is provided at the right end of the plate frame 4. The baffle stopper 20 fits the transverse baffle 21 and can make the head of the right positioning screw 19 separate from the test piece 11, that is, the pressure of the compression spring 22 is manually overcome to pull the right positioning screw 19 outward, and then the right positioning screw 19 is rotated, and the transverse baffle 21 will also move and rotate together. When the transverse baffle 21 is against the baffle stopper 20, the right positioning screw 19 will be temporarily fixed. At this time, the distance between the left positioning screw 18 and the right positioning screw 19 is the largest, which is convenient for placing and removing the test piece 11.
[0077] Since the left positioning screw 18 and the right positioning screw 19 are respectively against the two opposite sides of the test piece 11, in order to ensure the stability of the abutment, two conical grooves 38 are provided on the left side of the test piece 11 for the abutment of the two positioning screws; at the same time, a conical groove 38 is provided on the right side of the test piece 11 for the abutment of a right positioning screw 19. Figure 5 shown.
[0078] The lateral deformation of the specimen 11 can be obtained through the relative displacement between the left positioning screw 18 and the right positioning screw 19. To detect the lateral deformation, a first sliding lock 23 is horizontally slidably connected to the right end of the plate frame 4, that is, the installation position of the first sliding lock 23 is adjustable.
[0079] The cross-section of the first sliding lock 23 is in an "L" shape. The hooked part of the first sliding lock 23 hooks the right end of the plate frame 4 and can move on the right end of the plate frame 4. To lock after moving, a first vertical bolt 26 is provided on the first sliding lock 23. The head of the first vertical bolt 26 abuts against the plate frame 4 to fix the first sliding lock 23. By turning the first vertical bolt 26, the first sliding lock 23 can be locked or unlocked, thus facilitating the adjustment of its position on the plate frame 4.
[0080] A lateral displacement gauge 27 is provided on the first sliding lock 23. When installing the lateral displacement gauge 27, a first lock hole 24 is opened on the first sliding lock 23, and the lateral displacement gauge 27 is inserted into the first lock hole 24. At the same time, a first locking bolt 25 is provided on the first sliding lock 23. The head of the first locking bolt 25 abuts against the lateral displacement gauge 27 to fix the installation of the lateral displacement gauge 27, that is, by turning the first locking bolt 25, the lateral displacement gauge 27 in the first lock hole 24 can be clamped and fixed. After installation, the measuring rod of the lateral displacement gauge 27 abuts against the transverse baffle 21, and thus the displacement change of the right positioning screw 19 will be transmitted to the lateral displacement gauge 27.
[0081] For the above lateral displacement monitoring mechanism, through the cooperation and clamping of two left positioning screws 18 and one right positioning screw 19, the entire lateral displacement monitoring mechanism can be arranged on the specimen 11, and thus the lateral displacement monitoring mechanism is equivalent to being suspended. To achieve the vertical support of the lateral displacement monitoring mechanism, a lifting assembly is provided on the bottom plate 1. The lateral displacement monitoring mechanism is arranged above the lifting assembly. The lifting assembly can drive the lateral displacement monitoring mechanism to move upward to a specified position, that is, the lifting assembly drives the left positioning screw 18 and the right positioning screw 19 to move upward synchronously to ensure accurate abutment in the conical groove 38.
[0082] Lifting assemblies are arranged on both sides of the frame 2. The number of lifting assemblies on one side is one, corresponding to the left end of the plate frame 4, and the number of lifting assemblies on the other side is two, corresponding to the right end of the plate frame 4. Moreover, a rotating shaft 35 is provided between these two lifting assemblies for synchronous transmission. The connection lines between the three lifting assemblies form an isosceles triangle, and the plate frame 4 is arranged above the three lifting assemblies, which can push the plate frame 4 upward.
[0083] The lifting assembly is an eccentric lifting structure. Specifically, the lifting assembly includes a lifting seat 5, an eccentric wheel 36 rotatably arranged on the lifting seat 5, and a rotating handle 37 for driving the eccentric wheel 36. The lifting of the plate frame 4 is controlled by the rotation of the eccentric wheel 36. It is required that the plate frame 4 after the upward movement can drive the two types of positioning screws on the left and right to accurately abut against the conical groove 38, such as Figure 6 shown.
[0084] Since the lifting assembly can drive the lateral displacement monitoring mechanism to move upward, the left positioning screw 18 and the right positioning screw 19 in the lateral displacement monitoring mechanism are both penetrated on the frame 2. In order to ensure that the left positioning screw 18 and the right positioning screw 19 can move up and down smoothly, two vertically arranged positioning through holes 9 are opened on the left side wall of the frame 2 for the penetration of the two left positioning screws 18, and one vertically arranged positioning through hole 9 is opened on the right side wall of the frame 2 for the penetration of one right positioning screw 19, thereby providing space for the movement of the positioning screws.
[0085] The vertical displacement monitoring mechanism includes a column 28, a sliding lock 31 equipped with a vertical displacement meter 34, and a vertical baffle 16. Figure 7 The column 28 is vertically arranged on the bottom plate 1, and the sliding lock 2 31 is adjustable up and down arranged on the column 28. Specifically, a sliding hole 29 is opened on the column 28, and a transverse bolt 1 30 is inserted into the sliding hole 29. The transverse bolt 1 30 can move up and down along the sliding hole 29. One end of the transverse bolt 1 30 extends out of the sliding hole 29 to connect the sliding lock 2 31, so that the sliding lock 2 31 is conveniently installed on the column 28. By twisting the transverse bolt 1 30, the locking and unlocking of the sliding lock 2 31 can be controlled, so that the position of the sliding lock 2 31 can be adjusted and fixed.
[0086] The second sliding lock 31 is provided with a vertical displacement meter 34 arranged vertically. When the vertical displacement meter 34 is installed, the second sliding lock 31 is provided with a second locking hole 32, and the vertical displacement meter 34 is inserted into the second locking hole 32. At the same time, the second sliding lock 31 is provided with a second locking bolt 33, and the head of the second locking bolt 33 is tightly against the vertical displacement meter 34 to achieve the installation and fixation of the vertical displacement meter 34. That is, by twisting the second locking bolt 33, the vertical displacement meter 34 in the second locking hole 32 can be clamped and fixed.
[0087] The vertical baffle 16 is disposed on the force transmission column 3 and arranged at the upper end of the force transmission column 3. The force transmission column 3 can drive the vertical baffle 16 to move up and down together. The vertical baffle 16 has a certain length, and one end of the vertical baffle 16 extends horizontally to the top of the vertical displacement meter 34. The measuring rod of the vertical displacement meter 34 is tightly pressed against the vertical baffle 16 upward, and the displacement change of the force transmission column 3 will be transmitted to the vertical displacement meter 34.
[0088] The 3D printed concrete interface splitting tensile performance test method uses a 3D printed concrete interface splitting tensile performance test device to carry out the test. In this embodiment, the concrete material is aluminate cement, and the interface splitting tensile performance of the aluminate cement specimen can be tested accordingly. The raw materials of specimen 11 are CA50-Ⅲ (A700) aluminate cement, grade Ⅱ fly ash, standard sand, polycarboxylate high-efficiency water reducer, retarder, steel fiber and tap water. The mixture ratio is shown in Table 1:
[0089] Table 1: Concrete mix ratio (kg / m 3 )
[0090] Quartz sand Aluminate cement Fly ash water Water reducing agent Retarder Steel Fiber 1313 781 138 165 1.17 1.17 60
[0091] In this embodiment, since the specimen material is aluminate cement, the 3D printing aluminate cement concrete interface splitting tensile performance test method includes the following steps:
[0092] Step 1: Prepare a cubic concrete interface splitting performance test specimen 11 by 3D printing technology. The size of the specimen 11 is 40mm×40mm×40mm. The specimen 11 must have a printed interface layer parallel to the two opposite sides, and the interface layer is as much as possible in the middle, with the printed interface layer as the predetermined failure surface 39. Print three specimens 11 with the same raw material mix ratio. When printing, reserve a conical groove 38 on the two opposite sides of the specimen 11. If no conical groove 38 is reserved, a hand drill can be used to drill a conical groove 38 that meets the size requirements on the two opposite sides of the specimen 11 before the test.
[0093] After printing, the specimen 11 is cured according to the standard. Specifically, the printed block is cut into a size and structure that meets the test requirements before final setting, and then the specimen 11 is placed in a standard curing room for 28 days. The specimen 11 cured to 28 days is taken out of the standard curing room, the surface moisture is wiped off, the position of the predetermined failure surface 39 of the specimen 11 is determined, and the position line of the predetermined failure surface 39 is drawn in the middle of the concrete specimen 11.
[0094] Step 2: Operate the lifting assembly to support the lateral displacement monitoring mechanism, manually pull outward and rotate the right positioning screw 19 to cause the transverse baffle 21 to be stuck on the baffle limit plate 20, and ensure that the left positioning screw 18 and the right positioning screw 19 maintain a sufficient distance to provide sufficient space for placing and removing the test piece 11.
[0095] At this time, the marked concrete cube specimen 11 is placed centrally between the four elastic bottom support members to ensure that the vertical plane where the center arc top line of the lower arc pad 6 is located is consistent with the predetermined failure surface 39 of the specimen 11, and the bottom surface of the specimen 11 contacts the arc top line of the lower arc pad 6.
[0096] Step 3, continue to operate the lifting assembly to adjust the height position of the left positioning screw 18 and the right positioning screw 19 until the left positioning screw 18 and the right positioning screw 19 are horizontally aligned with the corresponding side conical grooves of the test piece. Reversely twist the right positioning screw 19 to reset it. After reset, the cross baffle 21 abuts against the top of the measuring rod of the lateral displacement meter 27. At the same time, completely loosen the right positioning screw 18, so that the heads of the left positioning screw 18 and the right positioning screw 19 are inserted into the corresponding side conical grooves 38 of the test piece 11, and then the lateral displacement monitoring mechanism is fastened to the test piece 11, and the test piece 11 cooperates with the test piece 11 to produce lateral deformation.
[0097] The lifting assembly is operated in reverse to separate from the plate frame 4, and no longer supports the lateral displacement monitoring mechanism. At this time, the lateral displacement monitoring mechanism is only clamped and fixed on the test piece 11 by the positioning screws. During the above operation, if the predetermined failure surface 39 of the test piece 11 is inconsistent with the plane where the arc top lines of the upper and lower arc-shaped pads are located, the position of the test piece 11 can be adjusted by moving the lateral displacement monitoring mechanism to keep it consistent.
[0098] The height position of the vertical displacement meter 34 is adjusted so that its measuring rod is against the vertical baffle 16 . When the vertical displacement meter 34 displays a small value, the second sliding lock 31 is fastened to the column 28 .
[0099] Step 4: After the specimen 11, the lateral displacement meter 27 and the vertical displacement meter 34 are installed, the data acquisition system and the piston cylinder 43 in the reaction frame are turned on, and the piston rod 44 in the piston cylinder 43 is driven according to the set program in the computer 45 to perform a loading test on the specimen 11. The specimen 11 can be split and damaged by the close contact between the lower arc pad 6, the upper arc pad 14 and the surface of the specimen 11. During the damage process, the splitting tensile load-lateral deformation full curve and the splitting tensile load-vertical deformation full curve of the damage of a specimen 11 can be easily obtained through the data acquisition system. Three specimens 11 are tested in each group, and the synthetic splitting tensile load-lateral deformation full curve and the synthetic splitting tensile load-vertical deformation full curve of the damage of the three specimens 11 can be obtained, such as Figure 8 As shown. Based on this, comprehensive indicators such as strength, deformation and toughness for evaluating the tensile properties of the specimen 11 can be obtained.
[0100] The present invention monitors the load applied by the piston cylinder 43 through the load sensor 17, so as to accurately test the load borne by the test piece 11 and obtain the splitting tensile strength value of the test piece 11. At the same time, the lateral displacement monitoring mechanism is combined with the vertical displacement detection mechanism to accurately monitor the lateral deformation value and the vertical deformation value of the test piece 11 after the splitting damage. By combining multiple monitoring data, the full curve of the splitting tensile load-lateral deformation and the full curve of the splitting tensile load-vertical deformation of the test piece 11 can be obtained, which meets the industry's demand for reasonable evaluation of the tensile performance of the interlayer interface of 3D printed concrete materials.
[0101] The embodiments described above are only preferred embodiments of the present invention and are not intended to limit the scope of implementation of the present invention. Therefore, any equivalent changes or modifications made according to the structures, features and principles described in the patent scope of the present invention should be included in the scope of the patent application of the present invention.
Claims
1. 3D printing concrete interface splitting performance test device, It is characterized in that It comprises a data acquisition system and a reaction frame and a splitting and pulling fixture controlled by the data acquisition system, wherein the splitting and pulling fixture is arranged in the reaction frame; The splitting and tensioning fixture comprises a base plate (1), a frame (2) for placing a test piece (11), a force transmission column (3) controlled by a reaction frame, a lateral displacement monitoring mechanism for monitoring the lateral deformation value of the test piece (11), a lifting assembly for driving the lateral displacement monitoring mechanism to move up and down, and a vertical displacement monitoring mechanism for monitoring the displacement of the force transmission column (3); The frame (2) is vertically arranged above the bottom plate (1), a lower arc-shaped pad (6) and an elastic bottom support member for elastically supporting the test piece (11) are arranged at the bottom of the frame (2), and a plurality of the elastic bottom support members are evenly arranged around the circumference of the lower arc-shaped pad (6); The top of the frame (2) is vertically elastically slidably connected with the force transmission column (3), the force transmission column (3) extends upward from the frame (2) and is connected to a load sensor (17), the force transmission column (3) extends downward into the frame (2) and is connected to an upper arc-shaped pad (14), and the upper arc-shaped pad (14) and the lower arc-shaped pad (6) are arranged in a corresponding manner at intervals up and down.
2. The 3D printing concrete interface splitting tensile performance testing device according to claim 1, It is characterized in that The reaction frame comprises a top plate (40), a base (41), a support column (42), a piston cylinder (43) and a piston rod (44); the top plate (40) and the base (41) are arranged in parallel with each other at intervals, and a plurality of support columns (42) are arranged between the top plate (40) and the base (41) for connection; The piston cylinder (43) is disposed at the center of the top plate (40), the piston cylinder (43) is inverted, the piston rod (44) of the piston cylinder (43) is downwardly facing the load sensor (17), the bottom plate (1) is bolted to the base (41), and the bottom plate (1) and the base (41) are stacked up and down.
3. The 3D printing concrete interface splitting tensile performance testing device according to claim 1, It is characterized in that The frame (2) has a U-shaped cross section, and the center of the frame (2) is transparent from front to back. The elastic bottom support member comprises a lower limit column (7) and a support compression spring (10) fixedly sleeved on the lower limit column (7), and the support compression spring (10) extends vertically upward and abuts against the bottom surface of the test piece (11).
4. The 3D printing concrete interface splitting tensile performance testing device according to claim 1, It is characterized in that The force transmission column (3) is a stepped column structure, the force transmission column (3) is larger at the top and smaller at the bottom, the upper end of the force transmission column (3) extends outside the frame (2), and the lower end extends into the frame (2); The frame (2) is provided with a vertical limit guide hole (8), the limit guide hole (8) is a long hole and passes through the side wall of the frame (2), the lower end of the force transmission column (3) is threadedly connected to a limit screw (15), the limit screw (15) is arranged horizontally, and the limit screw (15) is inserted into the limit guide hole (8).
5. The 3D printing concrete interface splitting tensile performance testing device according to claim 4, It is characterized in that A plurality of elastic supporting members are arranged between the upper end of the force transmission column (3) and the frame (2) for connection. The plurality of elastic supporting members are evenly arranged around the force transmission column (3). Each elastic supporting member comprises a supporting compression spring (13) and upper limit columns (12) fixedly sleeved on both ends of the supporting compression spring (13). The supporting compression spring (13) is arranged vertically, and the upper limit columns (12) at both ends are respectively arranged at the upper end of the force transmission column (3) and the top of the frame (2).
6. The 3D printing concrete interface splitting tensile performance testing device according to claim 1, It is characterized in that The lower side surface of the upper arc-shaped pad strip (14) is arc-shaped, and the upper side surface of the lower arc-shaped pad strip (6) is also arc-shaped, and the arc tops of the upper arc-shaped pad strip (14) and the lower arc-shaped pad strip (6) are opposite to each other.
7. The 3D printing concrete interface splitting tensile performance testing device according to claim 1, It is characterized in that The lateral displacement monitoring mechanism comprises a plate frame (4), a left positioning screw (18), a right positioning screw (19), and a sliding lock (23) equipped with a lateral displacement meter (27); The plate frame (4) and the bottom plate (1) are arranged in parallel up and down, the plate frame (4) is arranged around three sides of the frame (2), the left end of the plate frame (4) is threadedly connected with two left positioning screws (18), the head end of the left positioning screw (18) passes through the side wall of the frame (2) horizontally and abuts against the left side wall of the test piece (11), the right end of the plate frame (4) is elastically slidably connected with the right positioning screw (19) horizontally, the left positioning screw (18) and the right positioning screw (19) are arranged opposite to each other on the left and right sides, the head end of the right positioning screw (19) passes through the side wall of the frame (2) and abuts against the right side wall of the test piece (11); A transverse baffle (21) is arranged on the right positioning screw (19), and a baffle limiting piece (20) is arranged on the right end of the plate frame (4), wherein the baffle limiting piece (20) is in contact with the transverse baffle (21) so that the head of the right positioning screw (19) is separated from the test piece (11); The right end of the plate frame (4) is laterally slidably connected to the sliding lock (23), and the sliding lock (23) is provided with a lateral displacement meter (27), and the measuring rod of the lateral displacement meter (27) is tightly against the transverse baffle (21).
8. The 3D printing concrete interface splitting tensile performance testing device according to claim 7, It is characterized in that The left side wall of the test piece (11) is provided with two conical grooves (38) for abutting two positioning screws, and the right side wall of the test piece (11) is provided with a conical groove (38) for abutting a right positioning screw (19); The left side wall of the frame (2) is provided with two vertically arranged positioning through holes (9) for inserting two left positioning screws (18); the right side wall of the frame (2) is provided with a vertically arranged positioning through hole (9) for inserting a right positioning screw (19); The lifting assembly is arranged on the bottom plate (1), and the lateral displacement monitoring mechanism is arranged above the lifting assembly. The lifting assembly drives the left positioning screw (18) and the right positioning screw (19) to move upward synchronously and abut against the conical groove (38). The lifting assembly is an eccentric lifting structure. Lifting assemblies are arranged on both sides of the frame (2). The number of lifting assemblies on one side is one, and the number of lifting assemblies on the other side is two. A rotating shaft (35) is arranged for synchronous transmission. The plate frame (4) is arranged between the plurality of lifting assemblies.
9. The 3D printing concrete interface splitting tensile performance testing device according to claim 1, It is characterized in that The vertical displacement monitoring mechanism comprises a column (28), a second sliding lock (31) equipped with a vertical displacement meter (34), and a vertical baffle (16); the column (28) is vertically arranged on the bottom plate (1); the second sliding lock (31) is vertically adjustable on the column (28); and the second sliding lock (31) is provided with a vertically arranged vertical displacement meter (34); The vertical baffle (16) is arranged on the force transmission column (3), one end of the vertical baffle (16) extends horizontally to above the vertical displacement meter (34), and the measuring rod of the vertical displacement meter (34) is tightly pressed upward against the vertical baffle (16). 10.3D printing concrete interface splitting performance test method, It is characterized in that The 3D printed concrete interface splitting tensile performance testing device according to claims 1 to 9 comprises the following steps: Step 1: Prepare a concrete cubic splitting tensile test specimen (11) containing a printed interface by 3D printing technology, prefabricate conical grooves (38) on two sides of the test specimen (11) parallel to the printed interface layer, and perform maintenance on the test specimen according to standards; Step 2: operate the lifting assembly to support the lateral displacement monitoring mechanism, manually pull outward and rotate the right positioning screw (19) to cause the transverse baffle (21) to be stuck on the baffle stopper (20), and ensure that a large distance is maintained between the left positioning screw (18) and the right positioning screw (19); Placing the concrete specimen (11) to be tested on top of a plurality of elastic bottom support members, ensuring that the vertical plane where the centers of the upper arc pad (14) and the lower arc pad (6) are located is consistent with the printed interface layer of the specimen (11), i.e., the predetermined failure surface (39); Step 3, continue to operate the lifting assembly to adjust the height positions of the left positioning screw (18) and the right positioning screw (19) until the heads of the left positioning screw (18) and the right positioning screw (19) are horizontally aligned with the corresponding tapered grooves (38) on the side of the test piece (11); The right positioning screw (19) is reversely twisted to reset it. After reset, the cross baffle (21) abuts against the top of the measuring rod of the lateral displacement meter (27). At the same time, the left positioning screw (18) is completely loosened, so that the heads of the left positioning screw (18) and the right positioning screw (19) are inserted into the corresponding conical grooves (38) on the side of the test piece (11), so that the lateral displacement monitoring mechanism is fastened to the test piece (11); Then, the lifting assembly is operated in the reverse direction and the lateral displacement monitoring mechanism is no longer supported; the horizontal position of the test piece (11) is checked again to ensure that the predetermined failure surface (39) of the test piece (11) is consistent with the vertical plane where the centers of the upper arc pad (14) and the lower arc pad (6) are located; and the position of the vertical displacement meter (34) is adjusted so that the top end of its measuring rod is against the vertical baffle (16); Step 4: After the test piece (11), the lateral displacement meter (27) and the vertical displacement meter (34) are installed, the data acquisition system and the control computer (45) are turned on, and the piston rod in the piston cylinder (43) is driven according to the set program to perform a loading test on the test piece (11). The data acquisition system can be used to easily obtain the full splitting load-deformation curve of the test piece (11) and obtain a comprehensive index for evaluating the tensile performance of the test piece.
Citation Information