Sodium-ion battery formation optimal cut-off voltage determination method

By recording and analyzing the charging and discharging process data of sodium ion batteries, combined with the dQ/dV-V curve chart, the optimal cutoff voltage of sodium ion batteries is determined, and the battery performance problems caused by improper voltage is solved, achieving rapid and accurate Testing methods reduce manufacturing costs and improve battery performance.

CN118884262AInactive Publication Date: 2024-11-01PINGYU ZHONGXING ENERGY CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411030556.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Improper voltage conversion of sodium ion batteries will lead to overcharge, loss of active substances and reduced cycle times, and the prior art will find it difficult to effectively determine the optimal cutoff voltage, affecting battery performance and manufacturing costs.

Method used

By grouping test of sodium ion batteries, the voltage, capacity and time data of the charging and discharging process were recorded, and combined with the dQ/dV-V curve chart, irreversible capacity and the first effect, the optimal cutoff voltage was determined.

Benefits of technology

It is possible to quickly and accurately determine the optimal cutoff voltage of the sodium ion battery without disassembling the battery, shorten the transformation cycle, reduce manufacturing costs, and improve battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118884262A_ABST
    Figure CN118884262A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium ion battery formation optimal cut-off voltage determination method, which comprises the following steps of: carrying out low-current charging on a battery subjected to liquid injection and high-temperature standing at a certain temperature, and recording voltage and accumulated capacity data in a charging process; after standing, continuously performing formation constant-current charging with the charging current greater than the small current until different cut-off voltages are obtained, and recording voltage, capacity and time data in the formation charging process; standing the battery, recording voltage and time data in the standing process, and recording voltage change rate dV / dt and time t data; discharging the battery after standing for the first time, recording voltage and capacity data in the discharging process, and calculating irreversible capacity and formation first effect; and drawing a dQ / dV-V curve graph of the formation charging and discharging processes, and analyzing and determining the optimal cut-off voltage of the battery formation in combination with the irreversible capacity and the formation first efficiency. The method can be realized only by analyzing charge and discharge data of the formation process, and has the advantages of simple test method, high accuracy and strong practicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium ion batteries, and in particular to a method for determining an optimal formation cut-off voltage of a sodium ion battery. Background Art

[0002] Sodium-ion battery is a rechargeable battery with sodium ions as charge carriers. It has the characteristics of high safety, low cost, wide temperature range and long cycle life. It can effectively replace lithium batteries in application scenarios such as low-speed vehicles and energy storage.

[0003] The formation process is a key process in the production and manufacturing of sodium-ion batteries. The formation voltage of sodium-ion batteries is a relatively more direct parameter that affects the internal and interfacial states of the battery. Too high a voltage will cause the battery to overcharge, causing excessive sodium ions to escape from the positive electrode active material and deposit on the negative electrode surface to form sodium dendrites. The electrolyte solvent will react with the active sodium deposited on the negative electrode surface, causing the loss of positive electrode active materials, battery capacity decay, and reduced cycle times. Too low a formation voltage is not conducive to fully activating the active substances in the battery, the interface side reactions are not thorough, the degree of activation inside the battery is low, and the density of the SEI film is poor. Therefore, it is crucial to set the optimal formation voltage for sodium-ion batteries with different battery systems. By determining and optimizing the optimal formation cut-off voltage, not only can the performance of the battery be improved, but the formation time can also be greatly shortened and the manufacturing cost can be reduced. Summary of the invention

[0004] The purpose of the present invention is to provide a method for determining the optimal cut-off voltage of a sodium ion battery formation, which can effectively shorten the formation cycle, has a simple testing method, high accuracy and strong practicality, in view of the above-mentioned problems currently existing.

[0005] The technical solution of the present invention is as follows:

[0006] A method for determining an optimal cut-off voltage for formation of a sodium ion battery comprises the following steps:

[0007] S1. Take the batteries of the same batch that have been injected and left to stand, divide them into three groups, charge them with a small current I0, and record the voltage V0 and cumulative capacity Q0 data during the charging process;

[0008] S2, after the battery is left to stand for another time, continue to perform formation constant current charging with a charging current I1 greater than the small current I0, charge to different cut-off voltages, and record the voltage V1, capacity Q1 and time data of the formation charging process;

[0009] S3, placing the battery after formation charging to different cut-off voltages at rest, recording the voltage and time data during the resting process, and recording the voltage change rate dV / dt data;

[0010] S4, discharging the stationary batteries for the first time with a discharge current I2 until the battery discharge cut-off voltage is reached, recording the voltage V2 and capacity Q2 data during the discharge process, and calculating the irreversible capacity and the first formation effect;

[0011] S5. Draw a dQ / dV-V curve for the voltage and capacity data during the low-current charging in step S1, the formation charging in step S2, and the discharge in step S3. Combined with the irreversible capacity and the initial formation efficiency, analyze and determine the optimal formation cut-off voltage of the battery to be tested.

[0012] Furthermore, the standing temperature in S1 is 40-60° C., the standing time is 12-36 hours, and the small current I0 is 0.01-0.02° C.

[0013] Furthermore, the standing time in S2 is 2 to 5 minutes, and the charging current I1 is 0.05C to 1C; the three values ​​selected for the cut-off voltage V1 are determined according to the design voltage of the battery to be tested, including the design voltage of the battery to be tested and at least one adjacent voltage lower and higher than the design voltage of the battery, and the difference between adjacent voltages is less than or equal to 1.5.

[0014] Furthermore, the standing time in S3 is 1 min to 60 min, and the recording of voltage and time data during the standing process ends when the battery voltage changes less than or equal to 1 mV.

[0015] Furthermore, the discharge current I2 in S4 is consistent with the formation charging current I1, the irreversible capacity is the difference between the total charging capacity and the total discharge capacity Q2, and the formation first effect is the ratio of the total discharge capacity Q2 to the total charging capacity, where the total charging capacity is the sum of Q0 and Q1.

[0016] Furthermore, the dQ / dV-V curve in S5 can be combined with the voltage change rate, irreversible capacity and first formation effect when charged to different cut-off voltages to comprehensively judge the optimal cut-off voltage for the sodium ion battery; wherein when the irreversible capacity is lower, the first formation effect is higher, the voltage change rate decreases slowly, and the area of ​​the reduction reaction peak of the dQ / dV-V curve is the median, the formation cut-off voltage can be determined as the optimal cut-off voltage for the battery.

[0017] Furthermore, the temperature during the charging process is consistent with the temperature during the static process, ranging from 20 to 45°C.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] A method for determining an optimal formation cut-off voltage for a sodium ion battery can comprehensively determine the optimal formation cut-off voltage for various sodium ion battery systems by combining a dQ / dV-V curve diagram of a charge and discharge process, a formation voltage change rate, an irreversible capacity value, and a first efficiency value without disassembling the battery. The method has a short experimental cycle, a simple test method, high accuracy, and strong practicability. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a diagram of the interface of the negative electrode sheet of a battery after being fully charged and disassembled after formation according to an embodiment of the present invention.

[0021] Figure 2 This is a diagram showing the high temperature storage capacity retention rate of the battery after capacity conversion according to an embodiment of the present invention.

[0022] Figure 3 It is a cycle curve diagram of the battery after capacity conversion according to the embodiment of the present invention. DETAILED DESCRIPTION

[0023] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0024] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0025] See also Figure 1-3 , a method for determining the optimal cut-off voltage for sodium ion battery formation,

[0026] A method for determining an optimal cut-off voltage for formation of a sodium ion battery comprises the following steps:

[0027] S1. Take the batteries of the same batch that have been filled with liquid and left to stand at high temperature, divide them into three groups, charge them with a small current I0, and record the voltage V0 and cumulative capacity Q0 data during the charging process;

[0028] The high temperature standing after liquid injection is to ensure that the electrolyte is fully infiltrated, increase the contact area and reaction activity between the electrolyte and the electrode, and promote the formation of a more stable SEI film on the negative electrode surface. In addition, due to the effect of temperature during the standing period, the unstable substances will further react or transform, which is conducive to a more stable internal structure of the battery and reduces the probability of side reactions in the subsequent charging and discharging process. The first charge uses a small current of 0.01 to 0.02C to activate electrode materials that are not in the best physical property state, so that the battery can reach the ideal performance state.

[0029] S2, after the battery is left to stand for another time, continue to perform formation constant current charging with a charging current I1 greater than the small current I0, charge to different cut-off voltages, and record the voltage V1, capacity Q1 and time data of the formation charging process;

[0030] The purpose of standing still is to make the battery in a stable state and ensure that the gas generated during the charging process is effectively discharged. Setting the charging current I1 greater than the small current I0 for the first full charge can fully activate the positive electrode active material and can charge to the cut-off voltage relatively quickly. In addition, due to the different selection of positive electrode material systems for sodium ion batteries, the battery design voltage is different. According to the conventional positive electrode material design voltage of 3.4 to 4.2V, different formation cut-off voltages include the design voltage of the battery to be tested and at least one adjacent voltage lower and higher than the battery design voltage, and the adjacent voltage difference is less than or equal to 1.5V;

[0031] S3, leaving the battery after formation charging to different cut-off voltages to stand for a period of time, recording the voltage and time data during the standing process, and recording the voltage change rate dV / dt data;

[0032] When the battery is at rest, the temperature and pressure ranges are consistent with those during formation charging, and the charge is stopped when it is detected that the battery voltage has basically not changed. The condition is that the battery voltage change is less than or equal to 1mV. It can be considered that the battery is in a quasi-equilibrium state under this condition, and the voltage and capacity hardly change, and dq / dv approaches ∞.

[0033] S4, discharging the stationary batteries for the first time with a discharge current I2 until the battery discharge cut-off voltage is reached, recording the voltage V2 and capacity Q2 data during the discharge process, and calculating the irreversible capacity and the first formation effect;

[0034] In order to ensure the consistency of polarization effects during the charge and discharge process and reduce accidental errors in the data, the discharge current I2 is consistent with the formation charge current I1, the irreversible capacity is the difference between the total charge capacity and the total discharge capacity Q2, and the first effect is the ratio of the total discharge capacity Q2 to the total charge capacity, where the total charge capacity is the sum of Q0 and Q1.

[0035] S5. Draw a dQ / dV-V curve for the voltage and capacity data during the low-current charging in step S1, the formation charging in step S2, and the discharge in step S3. Combined with the irreversible capacity and the initial formation efficiency, analyze and determine the optimal formation cut-off voltage of the battery to be tested.

[0036] The high temperature static temperature in S1 is 40-60° C., the static time is 12-36 hours, and the small current I0 is 0.01-0.02° C.

[0037] The standing time in S2 is 2 to 5 minutes, and the charging current I1 is 0.05C to 1C; the cut-off voltage V1 is selected from three values, which are determined according to the design voltage of the battery to be tested, including the design voltage of the battery to be tested and at least one adjacent voltage lower and higher than the design voltage of the battery, and the difference between the adjacent voltages is less than or equal to 1.5.

[0038] The standing time in S3 is 1 min to 60 min, and the recording of voltage and time data during the standing process ends when the battery voltage changes less than or equal to 1 mV.

[0039] The discharge current I2 in S4 is consistent with the formation charging current I1, the irreversible capacity is the difference between the total charging capacity and the total discharge capacity Q2, and the formation first effect is the ratio of the total discharge capacity Q2 to the total charging capacity, where the total charging capacity is the sum of Q0 and Q1.

[0040] The dQ / dV-V curve in S5 can be combined with the voltage change rate, irreversible capacity and first formation effect when charged to different cut-off voltages to comprehensively judge the optimal cut-off voltage for the sodium ion battery; wherein the formation cut-off voltage when the irreversible capacity is lower, the first formation effect is higher, the voltage change rate decreases slowly, and the area of ​​the reduction reaction peak of the dQ / dV-V curve is moderate can be determined as the optimal cut-off voltage for the battery.

[0041] The temperature during the charging process is consistent with the temperature during the static process, ranging from 20 to 45°C.

[0042] The formation temperature mainly affects the formation effect by affecting the viscosity and conductivity of the electrolyte and the diffusion rate of ions in the electrode material. Generally, in the formation process, applying high temperature can reduce the viscosity of the electrolyte, accelerate the diffusion of ions, and ensure that electrons and ions combine quickly under high current; formation at high temperature can not only make the SEI film layer on the electrode surface react more fully, but also enhance the liquid absorption of the diaphragm, which is beneficial to reduce the bloating of the battery. However, high-temperature formation will reduce the stability of the SEI film and cause the battery cycle performance to deteriorate. This is because high temperature will aggravate the dissolution of the SEI film and the co-embedding of solvent molecules, while the SEI film tends to be stable under low temperature conditions. After a lot of verification, for different material systems of sodium ion batteries, the formation temperature of 20-45°C can achieve the viscosity and conductivity of the electrolyte and the diffusion rate of ions in the electrode material to meet the test requirements.

[0043] Experimental verification

[0044] This example uses a 50mm*160mm*119mm polyanion + hard carbon system aluminum shell sodium ion battery in the form of a laminate (59 positive layers and 60 negative layers), with a cell design capacity of 56Ah, an electrolyte of LG6085 from a blue solid manufacturer, an injection volume of 390g, and a high temperature standstill for 36 hours after injection. 24 batteries from the same batch were selected and divided into 3 groups, with 8 batteries in each group.

[0045] The three groups of batteries were charged and discharged: at a temperature of 30°C and a vacuum environment of -60KPa, the first 0.01C low-current charging was carried out to activate the electrode material of the battery, and the voltage V0 and cumulative capacity Q0 data of the battery during the low-current I0 charging process were recorded; after standing for 2 minutes, the batteries were continued to be charged at 0.2C formation, and charged to different formation cut-off voltages V1, where the different formation cut-off voltages V1 were set to 3.3V, 3.4V, and 3.5V. The batteries charged to different formation cut-off voltages were continued to stand for 20 minutes, and the voltage and time data of the battery during the standing process were recorded; after the standing period, the first discharge was carried out at a 0.2C discharge current, and all three groups of batteries were discharged to a cut-off voltage of 1.5V, and the voltage V2, capacity Q2 and time data of the discharge process were recorded.

[0046] Analyze and determine the optimal cut-off voltage: Based on the test results, such as Figure 1As shown, the voltage change rate at the formation cut-off voltage of 3.3V is relatively slow, and the voltage change rate at 3.5V is faster. The faster the voltage change rate, the larger the battery polarization impedance, the greater the internal polarization, and the poor formation uniformity. Calculation of the irreversible capacity and the first formation effect at different formation cut-off voltages shows that the irreversible capacity value of 3.5V is the highest, the irreversible capacity values ​​of 3.3V and 3.4V are consistent, and the first formation effects of 3.4V and 3.5V are equivalent. Analysis of the dQ / dV-V curves of different formation cut-off voltages shows that the reduction peak area of ​​3.5V is the largest and the reduction reaction is the most intense during the entire formation charge and discharge process. This is due to the increase in the side reaction of the electrolyte solvent at the 3.5V formation cut-off voltage, which also leads to more irreversible capacity consumption and reduced first effect. The area of ​​the 3.3V reduction peak is relatively small, indicating that the active material is not fully activated at the 3.3V formation cut-off voltage, and the sodium ion is insufficiently deintercalated, which is also the reason for the low discharge capacity. Comprehensive analysis of the formation voltage of 3.4V determined that it is the optimal cut-off voltage for the formation of the sodium ion battery of this system. It should be explained that the calculation of irreversible capacity and first formation efficiency, the drawing of dV / dt data and d / dV-V curves are all based on the average value of each group of batteries.

[0047] Table 1

[0048]

[0049] To further confirm the reliability of this method, the sodium ion batteries formed at different formation cut-off voltages provided in this embodiment were subjected to interface evaluation and electrical performance tests. The specific items are as follows:

[0050] Sodium precipitation: After formation, fully charge and disassemble to observe the interface state of the negative electrode sheet ( Figure 1 shown);

[0051] Storage performance test: capacity retention after storage at high temperature of 55°C for 7 (D) days and capacity recovery retention rate after charging ( Figure 2 shown);

[0052] Cycle performance test: Capacity retention test of 500 charge and discharge cycles at 0.5C at room temperature ( Figure 3 shown).

[0053] The test results show that the overall interface is good at the formation cut-off voltage of 3.4V, while there are many black spots on the interface at 3.3V, which is caused by insufficient sodium embedding at this voltage. The interface at 3.5V is poor and small particles of sodium are precipitated. The battery storage and cycle performance at the formation cut-off voltage of 3.4V is significantly better than that at 3.3V and 3.5V.

[0054] The above results show that the optimal formation cut-off voltage determined by the sodium ion battery formation optimal cut-off voltage method is very accurate and reliable.

[0055] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.

Claims

1. A method for determining the optimal cut-off voltage of a sodium ion battery, characterized in that: The following steps are involved: S1. Take the batteries of the same batch that have been injected and left to stand, divide them into three groups, charge them with a small current I0, and record the voltage V0 and cumulative capacity Q0 data during the charging process; S2, after the battery is left to stand for another time, continue to perform formation constant current charging with a charging current I1 greater than the small current I0, charge to different cut-off voltages, and record the voltage V1, capacity Q1 and time data of the formation charging process; S3, placing the battery after formation charging to different cut-off voltages at rest, recording the voltage and time data during the resting process, and recording the voltage change rate dV / dt data; S4, discharging the stationary batteries for the first time with a discharge current I2 until the battery discharge cut-off voltage is reached, recording the voltage V2 and capacity Q2 data during the discharge process, and calculating the irreversible capacity and the first formation effect; S5. Draw a dQ / dV-V curve for the voltage and capacity data during the low-current charging in step S1, the formation charging in step S2, and the discharge in step S3. Combined with the irreversible capacity and the initial formation efficiency, analyze and determine the optimal formation cut-off voltage of the battery to be tested.

2. A method for determining the optimal cut-off voltage of a sodium ion battery according to claim 1, characterized in that: The temperature of the static state in S1 is 40-60° C., the static state time is 12-36 hours, and the small current I0 is 0.01-0.02° C.

3. A method for determining the optimal cut-off voltage of a sodium ion battery according to claim 1, characterized in that: The standing time in S2 is 2 to 5 minutes, and the charging current I1 is 0.05C to 1C; the three values ​​selected for the cut-off voltage are determined according to the design voltage of the battery to be tested, including the design voltage of the battery to be tested and at least one adjacent voltage lower and higher than the design voltage of the battery, and the difference between the adjacent voltages is less than or equal to 1.

5.

4. A method for determining the optimal cut-off voltage of a sodium ion battery according to claim 1, characterized in that: The standing time in S3 is 1 min to 60 min, and the recording of voltage and time data during the standing process ends when the battery voltage changes less than or equal to 1 mV.

5. A method for determining the optimal cut-off voltage of a sodium ion battery according to claim 1, characterized in that: The discharge current I2 in S4 is consistent with the formation charging current I1, the irreversible capacity is the difference between the total charging capacity and the total discharge capacity Q2, and the formation first effect is the ratio of the total discharge capacity Q2 to the total charging capacity, where the total charging capacity is the sum of Q0 and Q1.

6. The method for determining the optimal cut-off voltage of a sodium ion battery according to claim 1, wherein: The dQ / dV-V curve in S5 can be combined with the voltage change rate, irreversible capacity and first formation effect when charged to different cut-off voltages to comprehensively judge the optimal cut-off voltage for the sodium ion battery; wherein when the irreversible capacity is lower, the first formation effect is higher, the voltage change rate decreases slowly, and the formation cut-off voltage when the area of ​​the reduction reaction peak of the dQ / dV-V curve is the median value can be determined as the optimal cut-off voltage for the battery.

7. The method for determining the optimal cut-off voltage of a sodium ion battery according to claim 1, characterized in that: The temperature during the charging process is consistent with the temperature during the static process, ranging from 20 to 45°C.

Citation Information

Patent Citations

  • Method for determining formation voltage of lithium ion battery

    CN117368748A

  • Battery formation management method, system, equipment and medium

    CN117712526A

  • Super-conductive nanoparticle, super-conductive nanoparticle powder, and lithium battery comprising the powder

    US20110118123A1

  • Non-aqueous electrolyte and lithium ion secondary battery

    WO2016110123A1