Wide-color-gamut asymmetric Fabry-Perot cavity structure color film

By using a combination of substrate, metal layer, dielectric layer and semiconductor layer in an asymmetric Fabripelo interference cavity, adjusting the semiconductor layer thickness to select light transmitting a specific wavelength, the lack of color richness and processing in the prior art is solved. Complex problems have achieved efficient structural color film production.

CN118884594APending Publication Date: 2024-11-01XIDIAN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411130403.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing asymmetric Fabripelo interference cavity has insufficient color richness, and the processing process is complicated and cannot be compatible with laser thinning technology, resulting in low production efficiency of structural color films.

Method used

The asymmetric Fabripeo interference cavity consisting of a substrate, metal layer, dielectric layer and semiconductor layer is used to select visible light transmitting a specific wavelength by adjusting the thickness of the semiconductor layer. It is compatible with femtosecond laser thinning technology to simplify the processing process.

Benefits of technology

It significantly improves the production efficiency of asymmetric Fabripe Perot cavity structure color films, achieves high saturation and rich color display, and is compatible with high-speed processing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118884594A_ABST
    Figure CN118884594A_ABST
Patent Text Reader

Abstract

The invention relates to a wide-color-gamut asymmetric Fabry-Perot cavity structure color film, which relates to the field of vacuum film application and comprises a substrate, a metal layer, a dielectric layer and a semiconductor layer, the substrate, the metal layer, the dielectric layer and the semiconductor layer are sequentially arranged from bottom to top; the metal layer, the dielectric layer and the semiconductor layer form a Fabry-Perot multi-beam interference cavity; wherein the thickness of the semiconductor layer is used for selectively transmitting visible light with a specific wavelength. The asymmetric Fabry-Perot cavity structure color film with the wide color gamut is provided with the supported substrate and the non-Fabry-Perot interference cavity composed of the metal layer, the dielectric layer and the semiconductor layer, the structure is compatible with the femtosecond laser thinning technology, and the production efficiency of the asymmetric Fabry-Perot cavity structure color film is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the application field of vacuum films, and in particular to an asymmetric Fabry-Perot cavity structural color film with a wide color gamut. Background Art

[0002] Structural color is also called physical color. Unlike chemical color, the formation of structural color does not rely on the absorption of light of a specific wavelength, but relies on the interference, diffraction or multiple scattering effects of the microscopic structure of the surface of the object to produce color. Compared with chemical color, physical color has the characteristics of stable and lasting color, environmental sustainability, adjustable color and flexible design. In recent years, it has gradually replaced chemical color.

[0003] Fabry-Perot interferometer cavities are often used in scientific research and industry to produce structural colors. A Fabry-Perot interferometer cavity consists of two materials with high reflectivity and partial transmittance. Visible light is emitted after multi-beam interference occurs in the cavity. The emitted light has a very high transmittance at a specific frequency, and can therefore display a specific color.

[0004] The Fabry-Perot interferometer used to make structural color films is divided into symmetric and asymmetric types. Symmetric Fabry-Perot interferometers are gradually replaced by asymmetric ones because they cannot produce highly saturated and rich colors. At present, asymmetric Fabry-Perot interferometers use two different metals as reflective surfaces to produce highly saturated colors, but the colors are not rich enough, and the processing process is complicated and cannot be compatible with laser thinning technology. Summary of the invention

[0005] In order to solve the above problems existing in the prior art, the present invention provides an asymmetric Fabry-Perot cavity structural color film with a wide color gamut.

[0006] According to a first aspect of an embodiment of the present invention, there is provided an asymmetric Fabry-Perot cavity structural color film with a wide color gamut, comprising:

[0007] substrate, metal layer, dielectric layer and semiconductor layer;

[0008] The substrate, the metal layer, the dielectric layer and the semiconductor layer are arranged in sequence from bottom to top;

[0009] The metal layer, the dielectric layer and the semiconductor layer constitute a Fabry-Perot multi-beam interference cavity; wherein the thickness of the semiconductor layer is used to selectively transmit visible light of a specific wavelength.

[0010] Optionally, the metal layer is a metal with balanced reflectivity over the entire visible light band.

[0011] Optionally, the dielectric layer is a transparent dielectric material.

[0012] Optionally, the thickness of the metal layer is greater than 100 nm.

[0013] Optionally, the dielectric layer has a thickness of 160nm-240nm.

[0014] Optionally, the semiconductor layer has a thickness of 30nm-100nm.

[0015] Optionally, the thickness of the semiconductor layer is controlled by a physical deposition method or a subtractive method.

[0016] The technical solution provided by the present invention may include the following beneficial effects:

[0017] The wide color gamut asymmetric Fabry-Perot cavity structural color film disclosed in the present invention has a supporting substrate and a non-Fabry-Perot interference cavity composed of a metal layer, a dielectric layer and a semiconductor layer. The structure is compatible with femtosecond laser thinning technology, which greatly improves the production efficiency of the asymmetric Fabry-Perot cavity structural color film.

[0018] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0020] Figure 1 The figure is a schematic structural diagram of an asymmetric Fabry-Perot cavity structural color film with a wide color gamut according to an exemplary embodiment.

[0021] Figure 2 It is a schematic diagram of a prior art processing process according to an exemplary embodiment.

[0022] Figure 3 It is a schematic diagram of the processing process of the present invention according to an exemplary embodiment.

[0023] Figure 4 The FDTD simulation of an asymmetric Fabry-Perot cavity structural color thin film corresponding to different semiconductor layer thicknesses is shown according to an exemplary embodiment.

[0024] Figure 5 The figure is a chromatogram of an asymmetric Fabry-Perot cavity structural color thin film corresponding to different semiconductor layer thicknesses manufactured using a physical deposition technique according to an exemplary embodiment.

[0025] Figure 6 is a physical picture of an asymmetric Fabry-Perot cavity structural color film according to an exemplary embodiment.

[0026] Description of Reference Numerals

[0027] 1. Substrate; 2. Metal layer; 3. Dielectric layer; 4. Semiconductor layer. DETAILED DESCRIPTION

[0028] Figure 1 FIG. 1 is a schematic diagram showing a wide color gamut asymmetric Fabry-Perot cavity structural color film according to an exemplary embodiment. Figure 1 As shown, it comprises: a substrate (1), a metal layer (2), a dielectric layer (3) and a semiconductor layer (4);

[0029] A substrate (1), a metal layer (2), a dielectric layer (3) and a semiconductor layer (4) are arranged in sequence from bottom to top;

[0030] The metal layer (2), the dielectric layer (3) and the semiconductor layer (4) constitute a Fabry-Perot multi-beam interference cavity; wherein the thickness of the semiconductor layer (4) is used to selectively transmit visible light of a specific wavelength.

[0031] It can be understood that the substrate (1) is a semiconductor silicon substrate, which mainly plays a supporting role, and the metal layer (2), the dielectric layer (3) and the semiconductor layer (4) constitute an asymmetric Fabry-Perot interference cavity to produce structural colors with high reflectivity and high color range. The metal layer (2) and the semiconductor layer (4) act as the "mirror" of the asymmetric Fabry-Perot interference cavity, the purpose of which is to ensure that visible light can be continuously reflected and partially transmitted, and the purpose of the transparent dielectric layer (3) is to ensure the full-band propagation of visible light. The asymmetric Fabry-Perot interference cavity composed of the metal layer (2), the dielectric layer (3) and the semiconductor layer (4) can enhance the transmittance of light of a specific wavelength, and control the thickness of the semiconductor layer to selectively transmit light of a specific wavelength.

[0032] Optionally, the metal layer (2) is a metal with balanced reflectivity over the entire visible light band.

[0033] For example, the metal layer (2) may be made of metal such as aluminum or silver, which has a balanced reflectivity over the entire wavelength band.

[0034] Optionally, the thickness of the metal layer (2) is greater than 100 nm.

[0035] Optionally, the dielectric layer (3) is a transparent dielectric material.

[0036] For example, the dielectric layer (3) may be made of transparent dielectric materials such as ITO or aluminum nitride.

[0037] Optionally, the thickness of the dielectric layer (3) is 160nm-240nm.

[0038] Optionally, the thickness of the semiconductor layer (4) is 30nm-100nm.

[0039] Optionally, the thickness of the semiconductor layer (4) is controlled by a physical deposition method or a subtractive method.

[0040] For example, the material used for the semiconductor layer (4) is silicon, and the thickness of the semiconductor layer (4) can be controlled by physical deposition methods such as evaporation and sputtering, or by subtractive methods such as femtosecond laser. By changing the thickness of the semiconductor layer (4), different structural colors can be generated.

[0041] In one embodiment, Figure 2 FIG. 1 is a schematic diagram of a prior art processing process according to an exemplary embodiment. Figure 2 As shown, the prior art uses metal-transparent dielectric-non-same metal to form a Fabry-Perot interference cavity to produce structural colors. This structure needs to change the hue of the color produced by changing the thickness of the underlying metal film. The film growth process is related to the distance between the material and the target material. Therefore, for underlying metals of different thicknesses, different coating processes must be used to grow the same upper film. The production of each color block requires a completely independent process. Therefore, it is basically impossible to achieve the production of structural color film patterns (the film pattern consists of tens of thousands of color blocks). Each color block is basically only a dozen microns, and it takes dozens of minutes to deposit the underlying metal of a color block. The structural color film proposed by the prior art is not compatible with rapid processing technology, making pattern processing almost difficult to complete.

[0042] The present invention provides a new asymmetric Fabry-Perot interferometer cavity, which is composed of metal-dielectric layer-semiconductor. By changing the thickness of the semiconductor layer, it is compatible with high-speed processing technology (femtosecond laser processing, etc.), and the bottom metal and dielectric layer have a unified process to achieve a change in hue. Figure 3 FIG. 1 is a schematic diagram of the processing process of the present invention according to an exemplary embodiment. Figure 3 As shown in the figure, by optimizing the manufacturing process of structural color films, the femtosecond laser processing technology is compatible with the greatly reduced pattern processing time and improved processing efficiency. (Thin film deposition usually takes tens of minutes to several hours, while femtosecond laser processing can usually be completed in a few minutes).

[0043] In one embodiment, the simulation is performed using FDTD simulation software. Figure 4 The present invention is a chromatogram of asymmetric Fabry-Perot cavity structural color thin film corresponding to different semiconductor layer thicknesses simulated by FDTD according to an exemplary embodiment. The thickness of the fixed metal layer (2) is 100nm, the thickness of the dielectric layer (3) is 180nm, and the thickness of the semiconductor layer (4) varies from 30nm to 100nm to obtain rich structural colors, which are converted into the xy coordinates of CIE1931 and the value x derived from the simulated spectrum. sim and simThe relationship is shown in Table 1:

[0044] Table 1

[0045]

[0046] Figure 5 is a chromatogram of asymmetric Fabry-Perot cavity structural color thin films corresponding to different semiconductor layer thicknesses manufactured using physical deposition technology according to an exemplary embodiment, Figure 6 FIG. 1 is a physical picture of an asymmetric Fabry-Perot cavity structural color film according to an exemplary embodiment. Figure 5 Figure 6 As shown, using high vacuum magnetron sputtering thin film deposition equipment, the thickness of the metal layer (2) is 100nm, the thickness of the dielectric layer (3) is 180nm, and the thickness of the semiconductor layer (4) varies from 30nm to 100nm. The results of FDTD simulation are restored and converted into the xy coordinates of CIE1931 and the structural color made by the experiment. The value x derived after measuring the spectrum real and real The relationship is shown in Table 2:

[0047] Table 2

[0048]

[0049] The color difference ΔE is defined using the two-norm distance. ΔE can measure the closeness between the simulated and experimental colors. The color difference corresponding to the structural colors generated by semiconductor layers (4) of different thicknesses can be obtained as shown in Table 3:

[0050] Table 3

[0051]

[0052] It can be observed from Table 3 that the color difference ΔE is basically controlled within 0.04.

[0053] like Figure 4 , Figure 5 As shown, the structural color gamut that can be displayed by the present invention is the elliptical area in the figure, and the triangular area is the sGBR full color gamut. By counting pixels and calculating the ratio of the two areas, it is obtained that the structural color gamut that can be displayed by the present invention is about 28% of the sGBR full color gamut.

[0054] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0055] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0056] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. An asymmetric Fabry-Perot cavity structural color film with a wide color gamut, characterized in that: include: A substrate (1), a metal layer (2), a dielectric layer (3) and a semiconductor layer (4); The substrate (1), the metal layer (2), the dielectric layer (3) and the semiconductor layer (4) are arranged in sequence from bottom to top; The metal layer (2), the dielectric layer (3) and the semiconductor layer (4) constitute a Fabry-Perot multi-beam interference cavity; wherein the thickness of the semiconductor layer (4) is used to selectively transmit visible light of different wavelengths.

2. The wide color gamut asymmetric Fabry-Perot cavity structural color film according to claim 1, characterized in that: The metal layer (2) is a metal with balanced reflectivity over the entire visible light band.

3. The wide color gamut asymmetric Fabry-Perot cavity structural color film according to claim 1, characterized in that: The dielectric layer (3) is a transparent dielectric material.

4. The wide color gamut asymmetric Fabry-Perot cavity structural color film according to claim 1, characterized in that: The thickness of the metal layer (2) is greater than 100 nm.

5. The wide color gamut asymmetric Fabry-Perot cavity structural color film according to claim 1, characterized in that: The thickness of the dielectric layer (3) is 160nm-240nm.

6. The wide color gamut asymmetric Fabry-Perot cavity structural color film according to claim 1, characterized in that: The thickness of the semiconductor layer (4) is 30nm-100nm.

7. The wide color gamut asymmetric Fabry-Perot cavity structural color film according to claim 1, characterized in that: The thickness of the semiconductor layer (4) is controlled by a physical deposition method or a subtractive method.