Zinc electrode modified by in-situ growth passive film coating as well as preparation method and application of zinc electrode

Modifying the zinc electrode by in-situ growth passivation film coating solves the problems of dendrites growth and hydrogen evolution reaction, achieving high stability and long life of the zinc electrode, and meeting the needs of high energy density and long life.

CN118888349AActive Publication Date: 2024-11-01NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411003192.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-01
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The zinc electrode faces dendrite growth, hydrogen evolution reaction and surface passivation problems during capacitor cycle, resulting in a degradation of performance and it is difficult to meet the needs of high energy density and long life.

Method used

By soaking zinc in aqueous ammonia solution for in-situ growth passivation film coating, a thin and uniform passivation film is formed, which avoids complex coating processes and hydrothermal methods, reduces production costs, and effectively prevents hydrogen evolution and Corrosion reaction.

Benefits of technology

The long cycle and high life of zinc electrodes are achieved, the stability and electrochemical performance of zinc ion capacitors are improved, and the discharge specific capacity and stable charge and discharge cycles are maintained under high current density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888349A_ABST
    Figure CN118888349A_ABST
Patent Text Reader

Abstract

The invention provides an in-situ growth passive film coating modified zinc electrode, a preparation method and application thereof, and belongs to the technical field of zinc electrode materials. The preparation method provided by the invention comprises the following steps: soaking zinc in an ammonia water solution, and then washing and drying to obtain the zinc electrode modified by the in-situ growth passive film coating. The method provided by the invention is simple and convenient. The zinc electrode modified by an in-situ grown passive film coating can be used for assembling a zinc ion battery and a zinc ion capacitor, and compared with other alkali liquor and the treatment concentration and time, it can be seen that a symmetrical battery assembled by the zinc electrode obtained according to the ammonia water concentration and the treatment time provided by the invention has higher stability, and the service life of the symmetrical battery is prolonged. And in the application of a zinc ion capacitor, the material has better cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of zinc electrode materials, and in particular to a zinc electrode modified with an in-situ grown passivation film coating, a preparation method and application thereof. Background Art

[0002] Supercapacitors are considered to be one of the attractive devices due to their high power density, fast charging and discharging rates, long life and high safety. However, the energy density of conventional aqueous supercapacitors, especially double-layer capacitors, is difficult to meet the requirements of electronics. In order to break and solve this bottleneck, hybrid supercapacitors have been constructed due to the combination of high-energy batteries and high-power supercapacitors. In the past few decades, lithium-ion hybrid supercapacitors have been one of the promising candidates for energy storage. But the low abundance and uneven distribution of lithium resources on the earth have greatly hindered the further practical application of lithium-ion hybrid supercapacitors. [Zhiwei Li, Yufeng An, Shengyang Dong, Chaojie Chen, Langyuan Wu, Yao Sun, Xiaogang Zhang, Energy Storage Materials 31 (2020) 252-266.]

[0003] The ionic radius of zinc ions and the mechanism of ion insertion process are similar to those of lithium ions. More importantly, Zn metal has a high conductivity of 820 mA hg -1 The high theoretical capacity, low redox potential of -0.76V (relative to standard hydrogen electrode, SHE), high natural abundance, and easy operating environment have greatly reduced costs. However, the zinc anode still faces three bottleneck problems: dendrite growth, hydrogen evolution reaction, and surface passivation. In the initial stage of capacitor cycling, zinc ions are usually reduced to form small zinc bumps on the negative electrode surface at energetically favorable charge transfer sites. Due to the lower surface energy, zinc ions tend to accumulate on these bumps to form initial dendrites. The "tip effect" of dendrites enhances the local electric field, further promoting the growth of surface dendrites. When dendrites grow to a large volume, they will pierce the separator, resulting in a decrease in battery performance. Summary of the invention

[0004] In view of this, the present invention aims to provide a zinc electrode modified with an in-situ grown passivation film coating, a preparation method and its application. The present invention realizes the construction of the passivation film by simple immersion in a solution, thereby realizing the preparation of a zinc electrode with a long cycle and a high lifespan.

[0005] In order to achieve the above-mentioned purpose, the present invention provides the following technical scheme: a method for preparing a zinc electrode modified by an in-situ grown passivation film coating, wherein zinc is immersed in an ammonia solution, then washed and dried to obtain the zinc electrode modified by the in-situ grown passivation film coating.

[0006] In some embodiments, before immersing the zinc in the ammonia solution, the step of pre-treating the zinc is also included; the pre-treatment is: grinding and cleaning the zinc.

[0007] In some embodiments, the mass concentration of the ammonia solution is 25-40%, preferably 28-30%; and the soaking time is 1-4 hours.

[0008] In some embodiments, the washing solution is anhydrous ethanol.

[0009] In some embodiments, the drying temperature is 60-70° C.; and the drying is performed in an atmosphere containing oxygen.

[0010] The reaction process of in-situ growth of the passivation film coating on the zinc surface in the present invention is as follows:

[0011] Zn+4NH3·H2O→Zn[(NH3)4] 2+ +4H2O

[0012] Zn[(NH3)4] 2+ +O2→ZnO+4NH3

[0013] In the present invention, the surface of the zinc foil is firstly corroded by NH3·H2O solution to expose more active sites, and then the residual liquid on the surface is removed by washing with anhydrous ethanol. After that, it is easy to contact with oxygen during the drying process, and a thin and uniform passivation film modification coating is easily formed on the surface after corrosion.

[0014] The invention also provides a zinc electrode modified with an in-situ grown passivation film coating prepared by the preparation method.

[0015] The present invention also provides the use of the zinc electrode modified by the in-situ grown passivation film coating in a zinc ion battery or a zinc ion capacitor.

[0016] The present invention also provides a zinc ion battery, wherein the negative electrode material is the zinc electrode modified by the in-situ grown passivation film coating.

[0017] In some embodiments, the zinc ion battery is a symmetrical battery or an asymmetrical battery. When assembling a symmetrical battery, the zinc electrode modified by the in-situ grown passivation film coating serves as both the positive and negative electrodes of the battery, and a glass fiber is used as a separator. When assembling the symmetrical battery, a 2M ZnSO4 electrolyte is added dropwise;

[0018] When assembling an asymmetric battery (such as a Zn-I2 battery, a Zn-Br2 battery, a Zn-MnO2 battery, a Zn-V2O5 battery, a Zn-PBA battery, etc.), the carbon paper electrode coated with I2, Br2, MnO2, V2O5, PBA, etc. is used as the positive electrode of the battery, the zinc electrode modified with the in-situ grown passivation film coating is used as the negative electrode of the battery, glass fiber is used as a separator, and 2M ZnSO4 electrolyte is added dropwise when assembling the battery.

[0019] The present invention also provides a zinc ion capacitor, wherein the negative electrode material is the zinc electrode modified by the in-situ grown passivation film coating.

[0020] In some embodiments, in the zinc ion capacitor, the activated carbon-coated carbon paper electrode is used as the positive electrode, the in-situ grown passivation film coating-modified zinc electrode is used as the negative electrode, glass fiber is used as the diaphragm, and 2M ZnSO4 electrolyte is added dropwise when assembling the zinc ion capacitor.

[0021] The present invention discloses the following technical effects:

[0022] The present invention provides a method for preparing a zinc electrode modified by an in-situ growth passivation film coating, and the formation of the passivation film layer can be achieved by only soaking and rinsing in an ammonia solution. The present invention avoids the complex method of common zinc electrode surface modification, and does not require a complex coating process and a series of complex hydrothermal methods to grow other substances in situ on the surface. The modification method of the zinc electrode of the present invention is simple and convenient, greatly reducing the production cost and the high requirements for equipment.

[0023] The passivation film formed by the present invention is more uniform, and the passivation film formed within the concentration range provided by the present invention is thinner, and while playing a role, it is not easy to affect the migration and stripping process of zinc ions. It can effectively avoid direct contact between zinc and electrolyte, thereby preventing hydrogen evolution and corrosion reactions, and effectively improving the cycle life of zinc ion capacitors.

[0024] By comparing other alkaline solutions, as well as treatment concentrations and times, the present invention can be seen that the symmetrical battery assembled with the zinc electrode having the ammonia concentration and treatment time provided by the present invention under high current density has higher stability and better cycle stability in the use of zinc ion capacitors.

[0025] The electrode material provided by the present invention exhibits excellent electrochemical performance. The zinc foil treated with NH3·H2O is used as the electrode material to assemble a symmetrical battery that can generate an electric charge at 60 mA cm -2 At a current density of 10 mAh cm -2 The electrode can stably charge and discharge for more than 2300 hours at a capacity of 10000W, while maintaining a low charge and discharge voltage. The zinc ion capacitor assembled with the electrode matched with AC can -1At high current density, it can maintain 32mAh g -1 The discharge specific capacity is above 10,000, and the capacity does not decay after stable charge and discharge cycles for 10,000 times. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 The SEM images of the zinc electrode modified with the passivation film coating prepared in Example 1 of the present invention at different scales, wherein a is at a scale of 5 μm, and b is at a scale of 1 μm;

[0028] Figure 2 The X-ray diffraction (XRD) pattern of the zinc electrode modified with the passivation film coating prepared in Example 1 of the present invention;

[0029] Figure 3 HRTEM image (a) and SEAD image (b) of the zinc electrode modified with the passivation film coating prepared in Example 1 of the present invention;

[0030] Figure 4 The zinc ion capacitors assembled with the passivation film coating modified zinc electrode prepared in Example 1 of the present invention and the pure zinc foil electrode of Comparative Example 4 and the AC positive electrode were respectively charged at 2A g -1 SEM images after 50 cycles at a current density of, wherein a is a zinc ion capacitor assembled with a zinc electrode modified with a passivation film coating prepared in Example 1 and an AC positive electrode at a scale of 50 μm, b is a zinc ion capacitor assembled with a zinc electrode modified with a passivation film coating prepared in Example 1 and an AC positive electrode at a scale of 10 μm, c is a zinc ion capacitor assembled with a pure zinc foil electrode and an AC positive electrode of Comparative Example 4 at a scale of 50 μm, and d is a zinc ion capacitor assembled with a pure zinc foil electrode and an AC positive electrode of Comparative Example 4 at a scale of 10 μm;

[0031] Figure 5 Symmetric cells were assembled from the zinc electrode modified with the passivation film prepared by ammonia treatment in Example 1 and the zinc electrode treated with sodium hydroxide solution in Comparative Example 1 at 60 mA cm –2 At a current density of 10 mAh cm –2 Comparison diagram of charge and discharge under the capacity of; wherein, a is a symmetrical battery assembled with a zinc electrode modified with a passivation film coating prepared by ammonia water treatment in Example 1, and b is a symmetrical battery assembled with a zinc electrode treated with sodium hydroxide lye in Comparative Example 1;

[0032] Figure 6 Symmetric cells were assembled from the zinc electrode modified with ammonia solution prepared in Example 1, the zinc electrode treated with sodium hydroxide solution in Comparative Example 1, and the pure zinc foil electrode prepared in Comparative Example 4 at 20 mA cm –2 At a current density of 0.5 mAh cm –2 Comparison diagram of charge and discharge under the capacity of; wherein, a is a symmetrical battery assembled from the zinc electrode prepared by ammonia water treatment in Example 1 and the zinc electrode treated with sodium hydroxide alkali solution in Comparative Example 1, and b is a symmetrical battery assembled from the zinc electrode treated with ammonia water in Example 1 and the pure zinc foil electrode in Comparative Example 4;

[0033] Figure 7 Symmetric cells were assembled from the zinc electrode prepared by treating with 28 wt % ammonia water for 1 h in Example 1, the zinc electrode prepared by treating with 5 wt % ammonia water for 1 h in Comparative Example 2, and the zinc electrode prepared by treating with 28 wt % ammonia water for 5 h in Comparative Example 3 at 20 mA cm –2 At a current density of 0.5 mAh cm –2 The charge-discharge diagram under the capacity of; where a is the zinc electrode treated with different ammonia concentrations, and b is the zinc electrode treated with the same concentration of ammonia for different time periods;

[0034] Figure 8 A comparison chart of the rate performance of symmetrical batteries respectively assembled with the zinc electrode modified with the passivation film coating prepared in Example 1 of the present invention and the pure zinc foil electrode of Comparative Example 4;

[0035] Fig. 9 A comparison chart of the zinc electrode modified with the passive film coating prepared in Example 1 of the present invention and the pure zinc foil electrode of Comparative Example 4 respectively subjected to Tafel test in 1M Na2SO4 solution using a three-electrode system;

[0036] Fig.10 The rate diagrams of zinc ion capacitors assembled with the passivation film coating modified zinc electrode prepared in Example 1 of the present invention and the pure zinc foil electrode of Comparative Example 4 respectively matched with AC; wherein a is the zinc electrode modified with the passivation film coating prepared in Example 1, and b is the pure zinc foil electrode of Comparative Example 4;

[0037] Fig.11 The zinc electrode modified with the passivation film coating prepared in Example 1 of the present invention and the pure zinc foil electrode of Comparative Example 4 were respectively matched with AC to assemble zinc ion capacitors at 2A g –1 The charge-discharge cycle diagram under current density, wherein a is a zinc ion capacitor assembled with a zinc electrode modified with a passivation film coating prepared in Example 1 and matched with AC, and b is a zinc ion capacitor assembled with a pure zinc foil electrode and matched with AC in Comparative Example 4;

[0038] Fig.12The zinc electrode modified with the passivation film coating prepared in Example 1 of the present invention and the pure zinc foil electrode of Comparative Example 4 were respectively matched with AC to assemble zinc ion capacitors at 8A g –1 The charge and discharge cycle diagram under current density, wherein a is the zinc electrode modified with the passivation film coating prepared in Example 1 and the AC matched assembled zinc ion capacitor, and b is the pure zinc foil electrode and AC matched assembled zinc ion capacitor of Comparative Example 4. DETAILED DESCRIPTION

[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0040] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0044] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0045] Unless otherwise specified, the reagents used in the examples can be obtained from commercial sources.

[0046] Example 1

[0047] The preparation method of the zinc electrode modified by in-situ growth of the passivation film coating in this embodiment is as follows:

[0048] A zinc foil of 100 cm×20 cm and 0.1 nm in thickness was polished with 600-mesh and 3000-mesh sandpapers, respectively, and then cut into small discs with a diameter of 0.1 cm by a cutting machine, which were used as samples for large-scale treatment in Example 1. Then, a certain amount of 28 wt% NH3·H2O solution was taken out in a watch glass (the amount of ammonia water was sufficient to completely immerse the zinc foil), and the treated zinc foil was immersed in the solution, kept for 1 hour, and then taken out, and then washed with anhydrous ethanol for 3 times, and finally placed in a 60°C forced air drying oven for drying, and then the in-situ grown passivation film coating modified zinc electrode was obtained.

[0049] Comparative Example 1

[0050] The preparation method of the zinc electrode in this comparative example is as follows:

[0051] A zinc foil of 100 cm×20 cm and a thickness of 0.1 nm was polished with 600-mesh and 3000-mesh sandpapers respectively, and then cut into small discs with a diameter of 0.1 cm using a sheet cutter as the sample for large-scale treatment in Example 1. Then, a certain amount of 8M NaOH solution was taken out in a watch glass (the amount of NaOH solution was sufficient to completely immerse the zinc foil), and the treated zinc foil was immersed in the solution for 1.5 minutes, then taken out, and then rinsed with deionized water for 2 minutes, and finally placed in a vacuum oven at 60°C for drying to obtain a zinc electrode.

[0052] Comparative Example 2

[0053] The preparation method of the zinc electrode in this comparative example is the same as that in Example 1, except that the 28 wt % NH 3 · H 2 O solution is replaced by a 5 wt % NH 3 · H 2 O solution.

[0054] Comparative Example 3

[0055] The preparation method of the zinc electrode in this comparative example is the same as that in Example 1, except that the time for immersing the zinc foil in the solution is replaced by 5 hours from 1 hour.

[0056] Comparative Example 4

[0057] The preparation method of the zinc electrode in this comparative example is the same as that in Example 1, except that the step of soaking the zinc foil in the NH3·H2O solution is omitted.

[0058] Effect test example

[0059] The zinc electrodes obtained in Example 1 and Comparative Examples 1-4 were assembled into zinc ion batteries and capacitors, respectively, and electrochemical performance tests were performed.

[0060] Preparation of activated carbon AC positive electrode: Specifically, activated carbon, conductive acetylene black and PVDF are mixed in a ratio of 8:1:1, NMP is used as solvent to form a uniform slurry, which is coated on the surface of carbon paper, and the electrode is placed in a vacuum oven at 60°C for 12 hours to obtain the positive electrode material (AC). The carbon paper before and after coating is weighed respectively, and the difference in mass between the two is the loading of the coating material. By calculation, it can be obtained that the loading of activated carbon on each electrode is about 2 mg.

[0061] When assembling a symmetrical battery, the activated carbon AC pole piece was used as the positive electrode, the zinc electrode modified with the in-situ grown passivation film coating prepared in Example 1 was used as the negative electrode, an appropriate amount of 2M ZnSO4 electrolyte was added, and glass fiber was used as a separator to test the electrochemical performance of the assembled symmetrical battery.

[0062] When assembling a zinc ion capacitor, the activated carbon AC pole piece is used as the capacitor positive electrode, the zinc electrode modified with the in-situ grown passivation film coating prepared in Example 1 is used as the negative electrode, an appropriate amount of 2M ZnSO4 electrolyte is added, and glass fiber is used as a diaphragm to test the electrochemical performance of the assembled zinc ion capacitor.

[0063] The SEM image of the zinc electrode surface obtained in Example 1 is as follows Figure 1 As shown, Figure 1 In the figure a and b are SEM images of the zinc electrode surface modified with the passivation film coating at a scale of 5 μm and 1 μm, respectively. It can be seen that the passivation film coating was successfully prepared to form a thin membrane on the surface of the zinc foil to prevent direct contact between the electrolyte and the zinc foil.

[0064] Figure 2 This is the X-ray diffraction (XRD) pattern of the zinc electrode prepared in Example 1. Figure 2 The three curves in the figure are the XRD spectrum of ZnO@Zn (i.e. ZnO-Zn in the figure), the standard PDF card of zinc and the standard PDF card of zinc oxide. From the XRD spectrum, it can be concluded that the passivation film coating is successfully prepared, and the main component of the passivation film is zinc oxide.

[0065] Figure 3 The high-resolution transmission electron microscopy (HRTEM) image (a) and selected area electron diffraction (SEAD) image (b) of the passivation film scraped off the surface of the zinc electrode prepared in Example 1. Obvious lattice fringes can be seen in the electron microscopy image, and the selected area electron diffraction shows symmetrical spots, indicating that the main component of the prepared passivation film coating is zinc oxide.

[0066] Figure 4The zinc ion capacitors assembled with the zinc electrode prepared in Example 1 and the pure zinc foil electrode in Comparative Example 4 and the AC positive electrode were 2Ag -1 SEM image after 50 cycles at a current density of Figure 4 In the figure, a and b are ZnO@Zn-AC capacitors at 2Ag -1 SEM images of Zn-AC capacitors after 50 cycles at a current density of 2A. -1 SEM image after 50 cycles at a current density of . It can be seen that only a small amount of zinc dendrites on the surface of the zinc electrode modified by the passivation film coating grow vertically, while almost all dendrites on the surface of the zinc foil grow vertically to the surface of the zinc foil. This shows that the zinc electrode modified by the passivation film coating can inhibit the vertical growth of zinc dendrites along the electrode surface, thereby reducing the possibility of zinc dendrites piercing the diaphragm and improving the cycling stability of the electrode.

[0067] Figure 5 Symmetric cells were assembled from the zinc electrode prepared by ammonia treatment in Example 1 and the zinc electrode treated with sodium hydroxide solution in Comparative Example 1 at 60 mA cm -2 At a current density of 10 mAh cm -2 Charge and discharge diagram under capacity. Figure 5 In the figure, a is the zinc electrode assembled symmetrical battery of Example 1 at 60 mA cm -2 At a current density of 10 mAh cm -2 The charge and discharge diagram of the symmetrical battery at a capacity of , b is the charge and discharge diagram of the symmetrical battery assembled with zinc electrode of comparative example 1 at 60 mA cm -2 At a current density of 10 mAh cm -2 Symmetrical battery charge and discharge diagram under the capacity of. Figure 5 It can be seen that at 60mA cm -2 At high current densities and 10 mAh cm -2 At a capacity of 1.34 W, the symmetrical battery assembled with zinc electrodes treated with ammonia has better stability than that with zinc electrodes treated with sodium hydroxide, and can cycle for 2300 h at a high current density with a lower overpotential. However, the symmetrical battery assembled with zinc electrodes treated with sodium hydroxide can only cycle for 150 h and is prone to short circuit.

[0068] Figure 6 Symmetric cells were assembled from the zinc electrode prepared by ammonia treatment in Example 1, the zinc electrode treated with sodium hydroxide solution in Comparative Example 1, and the pure zinc foil electrode in Comparative Example 4. -2 At a current density of 0.5 mAh cm -2 Comparison chart of charge and discharge at capacity. Figure 6In the figure, a is a symmetrical battery composed of a zinc electrode prepared by ammonia treatment in Example 1 and a zinc electrode treated by sodium hydroxide solution in Comparative Example 1 at 20 mA cm -2 At a current density of 0.5 mAh cm -2 The charge and discharge comparison diagram of the symmetrical battery at a capacity of 20 mA cm-1 is shown in Figure 2. ... -2 At a current density of 0.5 mAh cm -2 Comparison chart of symmetrical battery charge and discharge under the capacity of. Figure 6 It can be seen that the symmetrical battery assembled from the zinc electrode treated with ammonia water has a more stable voltage overall at a relatively small current density compared to the zinc electrode treated with sodium hydroxide and the untreated zinc electrode, and can maintain a lower overpotential even after 5000 cycles.

[0069] Figure 7 Symmetric cells were assembled from the zinc electrode prepared by treating with 28 wt % NH 3 · H 2 O for 1 h in Example 1, the zinc electrode prepared by treating with 5 wt % NH 3 · H 2 O for 1 h in Comparative Example 2, and the zinc electrode prepared by treating with 28 wt % NH 3 · H 2 O for 5 h in Comparative Example 3 at 20 mA cm -2 At a current density of 0.5 mAh cm -2 Charge and discharge diagram under capacity. Figure 7 In the figure, a is the Zn electrode treated with different ammonia concentrations at 20 mA cm -2 At a current density of 0.5 mAh cm -2 The charge and discharge comparison diagram of the symmetric battery under the capacity of b is the zinc electrode treated with the same concentration of ammonia for different time at 20mA cm -2 At a current density of 0.5 mAh cm -2 Comparison of symmetrical battery charge and discharge under the capacity of. Figure 7 It can be found from the comparison of a and b that the symmetrical battery assembled with the zinc electrode prepared by the specific ammonia concentration and time selected in Example 1 of the present invention has better cycle stability and lower overpotential. Therefore, the ammonia concentration and time in the present invention are the optimal selection range for improving the performance of the zinc electrode.

[0070] Figure 8 The rate performance comparison diagram of the symmetrical battery assembled with the zinc electrode prepared in Example 1 and the pure zinc foil electrode of Comparative Example 4 (in the figure, ZnO@Zn represents Example 1 and Zn represents Comparative Example 4) is shown in FIG. Figure 8It can be seen that the zinc electrode modified by the passivation film coating has a smaller nucleation overpotential and a lower polarization potential than the unmodified zinc electrode, which means that the electrode modified by the passivation film coating can reduce the energy barrier of metal nucleation, thereby promoting uniform zinc metal deposition. It can be seen that the presence of the in-situ grown passivation film coating reduces the charge transfer resistance on the surface of the zinc electrode, showing excellent electroplating and stripping energy, and has better rate performance.

[0071] Fig. 9 The comparison diagram of the zinc electrode prepared in Example 1 and the pure zinc foil electrode in Comparative Example 4 in Tafel test using a three-electrode system in 1M Na2SO4 solution (ZnO@Zn in the figure represents Example 1, and Bare-Zn represents Comparative Example 4). Fig. 9 It can be seen that the zinc electrode modified with the passivation film coating prepared in Example 1 has a higher corrosion potential than the unmodified zinc foil electrode of Comparative Example 4 (the corrosion potential of the ZnO@Zn electrode is -1.036 V, and the corrosion potential of the zinc foil electrode is -1.122 V).

[0072] Fig.10 The rate diagram of zinc ion capacitors assembled with the zinc electrode prepared in Example 1 and the pure zinc foil electrode of Comparative Example 4 respectively matched with AC, Fig.10 In the figure, a is the rate diagram of zinc ion capacitor assembled with AC matched by zinc electrode modified by passivation film coating prepared in Example 1, and b is the rate diagram of zinc ion capacitor assembled with AC matched by pure zinc foil electrode in Comparative Example 4. Fig.10 It can be seen that when the current density increases from 0.2A g -1 , 0.5A g -1 , 1A g -1 , 2A g -1 , 3A g -1 When gradually increasing, the ZnO@Zn-AC capacitors have 54.4 mAh g -1 , 46.8mAh g -1 , 41.5mAh g -1 、38.9mAh g -1 、36.1mAh g -1 The discharge capacity of Zn-AC capacitors is only 46.3 mAh g at the same current density. -1 、38.2mAh g -1 、32.7mAh g -1 , 28.3mAh g -1 , 26.1mAh g -1 Therefore, the ZnO@Zn-AC capacitor has a higher specific capacitance than the Zn-AC capacitor at a low current, -1 Up to 3A g-1 At each current density, the ZnO@Zn-AC capacitor has a higher specific capacity, indicating that it has better rate performance. The reason why the zinc electrode modified by the passivation film coating prepared by the present invention has better rate performance is that the electrode avoids direct contact with the electrolyte, reduces the occurrence of corrosion and hydrogen evolution reaction, and its electrochemical performance is better than that of the zinc foil electrode.

[0073] Fig.11 The zinc electrode modified with the passivation film coating prepared in Example 1 and the pure zinc foil electrode of Comparative Example 4 were respectively matched with AC to assemble zinc ion capacitors at 2A g -1 Figure 1 shows the charge-discharge cycle diagram under current density. Figure a shows the zinc electrode modified with the passivation film coating prepared in Example 1 and the AC matched zinc ion capacitor assembled at 2A g -1 The charge and discharge cycle diagram under current density, Figure b is the pure zinc foil electrode and AC matching assembled zinc ion capacitor in comparative example 4 at 2A g -1 The charge and discharge cycle diagram under current density. Fig.11 It can be seen that the capacity of the Zn-AC capacitor decayed dramatically after 4,000 charge and discharge cycles, indicating that the cycle stability of the Zn-AC capacitor is poor. However, the capacity of the ZnO@Zn-AC capacitor did not decay after 10,000 stable charge and discharge cycles, indicating that this ZnO@Zn-AC capacitor has good cycle stability and cycle life.

[0074] Fig.12 The zinc electrode modified with the passivation film coating prepared in Example 1 and the pure zinc foil electrode of Comparative Example 4 were respectively matched with AC to assemble zinc ion capacitors at 8A g -1 Figure 1 shows the charge-discharge cycle diagram under current density. Figure a shows the zinc electrode modified with the passivation film coating prepared in Example 1 and the AC matched zinc ion capacitor assembled at 8A g -1 The charge and discharge cycle diagram under current density, Figure b is the pure zinc foil electrode and AC matching assembled zinc ion capacitor in comparative example 4 at 8A g -1 The charge and discharge cycle diagram under current density. Fig.12 It can be seen that the overall capacity of the Zn-AC capacitor is relatively low and the cycle stability is poor during the charge and discharge cycle. However, the capacity of the ZnO@Zn-AC capacitor remains at 32 mAh g after 10,000 stable charge and discharge cycles. -1 , which shows that this ZnO@Zn-AC capacitor has good cycle stability and cycle life.

[0075] The present invention also tests the electrochemical performance of zinc ion batteries assembled by using the zinc electrode modified with the in-situ grown passivation film coating prepared in Example 1 as the negative electrode and the carbon paper coated with MnO2, V2O5 powder or PBA powder as the positive electrode. The results show that when the zinc electrode modified with the in-situ grown passivation film coating provided by the present invention is selected as the negative electrode material, the assembled different zinc ion batteries all have excellent electrochemical performance.

[0076] Example 2

[0077] The preparation method of the zinc electrode modified with the in-situ grown passivation film coating in this embodiment is the same as that in Embodiment 1, except that the time for immersing the zinc foil in the solution is replaced by 4 hours from 1 hour.

[0078] The present invention also conducted an electrochemical test on the zinc electrode obtained in Example 2, and the test method was similar to the test method of the zinc electrode obtained in Example 1. The results showed that the zinc electrode modified with the in-situ grown passivation film coating prepared in this example had excellent electrochemical properties.

[0079] Example 3

[0080] The preparation method of the zinc electrode modified with the in-situ grown passivation film coating in this embodiment is the same as that in Embodiment 1, except that the 28 wt % NH 3 · H 2 O solution is replaced by a 30 wt % NH 3 · H 2 O solution.

[0081] The present invention also conducted an electrochemical test on the zinc electrode obtained in Example 3, and the test method was similar to the test method of the zinc electrode obtained in Example 1. The results showed that the zinc electrode modified with the in-situ grown passivation film coating prepared in this example had excellent electrochemical properties.

[0082] Example 4

[0083] The preparation method of the zinc electrode modified with the in-situ grown passivation film coating in this embodiment is the same as that in Embodiment 1, except that the 28 wt % NH 3 · H 2 O solution is replaced by a 25 wt % NH 3 · H 2 O solution.

[0084] The present invention also conducted an electrochemical test on the zinc electrode obtained in Example 4, and the test method was similar to the test method of the zinc electrode obtained in Example 1. The results showed that the zinc electrode modified with the in-situ grown passivation film coating prepared in this example had excellent electrochemical properties.

[0085] Example 5

[0086] The preparation method of the zinc electrode modified with the in-situ grown passivation film coating in this embodiment is the same as that in Embodiment 1, except that the 28 wt % NH 3 · H 2 O solution is replaced by a 40 wt % NH 3 · H 2 O solution.

[0087] The present invention also conducted an electrochemical test on the zinc electrode obtained in Example 5, and the test method was similar to the test method of the zinc electrode obtained in Example 1. The results showed that the zinc electrode modified with the in-situ grown passivation film coating prepared in this example had excellent electrochemical properties.

[0088] In summary, the zinc electrode modified with the passivation film coating provided by the present invention can be used as an electrode, applied in zinc ion batteries or zinc ion capacitors, and has excellent electrochemical properties.

[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a zinc electrode modified with an in-situ grown passivation film coating, characterized in that: The zinc electrode modified with the in-situ grown passivation film coating can be obtained by immersing zinc in an ammonia solution, then washing and drying.

2. The method for preparing a zinc electrode modified with an in-situ grown passivation film coating according to claim 1, characterized in that: Before immersing the zinc in the ammonia solution, the method further includes a step of pre-treating the zinc; the pre-treatment includes grinding and cleaning the zinc.

3. The method for preparing a zinc electrode modified with an in-situ grown passivation film coating according to claim 1, characterized in that: The mass concentration of the ammonia solution is 25-40%; and the soaking time is 1-4 hours.

4. The method for preparing a zinc electrode modified with an in-situ grown passivation film coating according to claim 1, characterized in that: The solution used for the washing is anhydrous ethanol.

5. The method for preparing a zinc electrode modified with an in-situ grown passivation film coating according to claim 1, characterized in that: The drying temperature is 60-70° C.; the drying is carried out in an atmosphere containing oxygen.

6. A zinc electrode modified with an in-situ grown passivation film coating prepared by the preparation method according to any one of claims 1 to 5.

7. Use of a zinc electrode modified with an in-situ grown passivation film coating as claimed in claim 6 in a zinc ion battery or a zinc ion capacitor.

8. A zinc ion battery, characterized in that: The negative electrode material is the zinc electrode modified by the in-situ grown passivation film coating as described in claim 6.

9. A zinc ion capacitor, characterized in that: The negative electrode material is the zinc electrode modified by the in-situ grown passivation film coating as described in claim 6.

Citation Information

Patent Citations

  • Method for inhibiting zinc dendritic crystal growth by using polydopamine film

    CN112349893A

  • Copper-based current collector for inducing preferential transverse deposition of lithium metal negative electrode as well as preparation method and application of copper-based current collector

    CN113036153A

  • Deep chargeable battery systems and methods

    CN115004447A

  • Negative pole piece as well as preparation method and application thereof

    CN115101715A

  • Zinc negative electrode modified by amorphous zinc oxide coating as well as preparation method and application of zinc negative electrode

    CN116504911A