Preparation method of solar cell and solar cell

By forming a doped silicon glass layer during the solar cell fabrication process and using laser-processed chemical etching technology for non-grid areas, the parasitic absorption problem caused by the thickness of the doped layer was solved, improving the performance and efficiency of solar cells and reducing production costs.

CN118888643APending Publication Date: 2024-11-01JA SOLAR TECH YANGZHOU
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411139317.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The thicker the doped layer, the more severe the parasitic absorption, which limits the improvement of short-circuit current density and photoelectric conversion efficiency of solar cells.

Method used

In the fabrication process of solar cells, a doped silicon glass layer is formed on the surface of a doped polycrystalline silicon layer, and the non-gate area is treated with a laser to make its chemical etching rate higher than that of the gate area. Then, the doped silicon glass layer and part or all of the polycrystalline silicon layer in the non-gate area are removed by chemical etching, and the doped layer in the non-metallic electrode area is thinned.

Benefits of technology

It effectively reduces parasitic absorption in the doped layer, improves the short-circuit current density and photoelectric conversion efficiency of solar cells, and simplifies the process and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888643A_ABST
    Figure CN118888643A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a solar cell and the solar cell. The processing method for the doping layer of the solar cell comprises the steps that a first doped polycrystalline silicon layer is formed on the main surface of a silicon substrate, a first doped silica glass layer is formed on the surface of the first doped polycrystalline silicon layer, and doping elements in the first doped silica glass layer are the same as those in the first doped polycrystalline silicon layer; processing a non-grid line area of the first doped silica glass layer by using laser to enable the chemical etching rate of the non-grid line area in the first doped silica glass layer to be greater than that of the grid line area; and removing the first doped silica glass layer and a part or all of the first doped polycrystalline silicon layer corresponding to the non-grid line region in a chemical etching mode. According to the processing method, the doping layer in the non-metal electrode area can be thinned, parasitic absorption caused by the doping layer is reduced, and therefore the short-circuit current density and the photoelectric conversion efficiency of the solar cell are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a solar cell and the solar cell. Background Art

[0002] For solar cells, although the doping layer (such as the first doped polysilicon layer or the doped monocrystalline silicon layer) has a relatively good passivation effect, which is beneficial to improving the open circuit voltage of the solar cell, the doping layer has a relatively serious parasitic absorption, and the thicker the doping layer, the more serious the parasitic absorption. The parasitic absorption caused by the doping layer limits the improvement of the short-circuit current density and photoelectric conversion efficiency of the solar cell. Summary of the invention

[0003] In view of this, the present invention provides a method for preparing a solar cell and a solar cell, which thins the doping layer in the non-metallic electrode area and reduces the parasitic absorption caused by the doping layer, thereby effectively improving the short-circuit current density and photoelectric conversion efficiency of the solar cell.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] In a first aspect, the present invention provides a method for preparing a solar cell, comprising:

[0006] Step 1, forming a first doped polysilicon layer on the main surface of the silicon substrate, and forming a first doped silicon glass layer on the surface of the first doped polysilicon layer, wherein the doping element in the first doped silicon glass layer is the same as the doping element in the first doped polysilicon layer;

[0007] Step 2, using laser to process the non-gate line region of the first doped silicon glass layer, so that the chemical etching rate of the non-gate line region in the first doped silicon glass layer is greater than that of the gate line region;

[0008] Step 3: remove the first doped silicon glass layer and part or all of the first doped polysilicon layer corresponding to the non-gate line area by chemical etching.

[0009] In a second aspect, an embodiment of the present invention provides a solar cell prepared by the preparation method provided by the embodiment of the first aspect, comprising: a silicon substrate and a first doped polysilicon layer located on a main surface of the silicon substrate, wherein:

[0010] The first doped polysilicon layer includes: a gate line region and a non-gate line region arranged in an arranged manner, wherein:

[0011] The thickness of the gate line region is greater than the thickness of the non-gate line region.

[0012] The technical solution of the first aspect of the above invention has the following advantages or beneficial effects:

[0013] The preparation method provided by the embodiment of the present invention forms a first doped silicon glass layer on the first doped polysilicon layer after forming the first doped polysilicon layer, and processes the non-gate line area of ​​the first doped silicon glass layer by laser to modify the non-gate line area and make it easier to be etched by a chemical solution. Then, in the subsequent treatment by chemical etching, the first doped silicon glass layer in the non-gate line area is easier to remove. Then, in the process of removing the first doped silicon glass layer in the gate line area by chemical etching, the gate line area and the non-gate line area are etched at the same time, which can remove the first doped silicon glass layer in the non-gate line area more quickly. The non-gate line area lacks the protection of the first doped silicon glass layer, and part or all of the first doped polysilicon layer in the non-gate line area will also be etched and removed, thereby achieving the purpose of thinning the doped layer in the non-metallic electrode area, effectively reducing the parasitic absorption caused by the doped layer, thereby effectively improving the short-circuit current density and photoelectric conversion efficiency of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 is a schematic diagram of the main process of a method for preparing a solar cell according to an embodiment of the present invention;

[0015] Figure 2 is a method according to an embodiment of the present invention corresponding to Figure 1 Schematic diagram of the first structural change of the solar cell in the process shown;

[0016] Figure 3 is a method according to an embodiment of the present invention corresponding to Figure 1 A diagram showing a second structural change of a solar cell in the process shown;

[0017] Figure 4 is a method according to an embodiment of the present invention corresponding to Figure 1 A diagram showing the third structural variation of the solar cell in the process shown;

[0018] Figure 5 is a schematic diagram of the main process of another method for preparing a solar cell according to an embodiment of the present invention;

[0019] Figure 6 is a method according to an embodiment of the present invention corresponding to Figure 5 A schematic diagram of the change of the solar cell structure from step S501 to step S507 in the process shown;

[0020] Figure 7 is a method according to an embodiment of the present invention corresponding to Figure 5 A schematic diagram of the change of the solar cell structure from step S507 to step S510 in the process shown;

[0021] Figure 8 is a schematic diagram of a first structure of a solar cell according to an embodiment of the present invention;

[0022] Fig. 9 is a schematic diagram of a second structure of a solar cell according to an embodiment of the present invention.

[0023] The reference numerals are as follows:

[0024] 10-silicon substrate; 20-first doped polysilicon layer; 30-first doped silicon glass layer; 40-tunneling oxide layer; 50-second doped polysilicon layer; 60-second doped silicon glass layer; 70-Al2O3 layer; 80-passivation anti-reflection layer. DETAILED DESCRIPTION

[0025] There are currently two main ways to obtain a thinned doped polysilicon layer. The first method is to directly deposit a polysilicon layer of the required thickness, and then perform high-temperature doping directly on the polysilicon layer. The second method is to use a mask to protect the gate line area, and the non-gate line area is thinned by cleaning. For the first method, it is necessary to perform high-temperature doping directly on the thinned polysilicon layer. For the tunneling passivation structure, the doping source can easily break through the tunneling oxide layer under the polysilicon layer, causing the tunneling effect of the solar cell to disappear. The second method requires the addition of the steps of setting a mask, cleaning the non-gate line area, and removing the mask, which increases the production steps of solar cells and increases costs.

[0026] In order to simultaneously reduce the parasitic absorption caused by the doping layer of the solar cell, avoid affecting other properties of the solar cell such as tunneling effect and passivation effect, and effectively control the production cost of the solar cell, an embodiment of the present invention provides a new method for preparing a solar cell.

[0027] The one structure stacked on another structure involved in the embodiments of the present invention generally means that the one structure is formed after the other structure, and the one structure is located on the main surface of the other structure away from the silicon substrate. It is worth noting that the one structure stacked on the other structure does not specifically mean that the one structure is located above the other structure, and it can also be located below the other structure.

[0028] The type of the doping element involved in the embodiments of the present invention is generally N-type or P-type.

[0029] The doping concentration involved in the embodiments of the present invention generally refers to the concentration of the doping element contained in the doping layer after the doping element is activated.

[0030] Regarding the formation of another structure on a structure involved in the embodiments of the present invention, the two structures may be in direct or indirect contact. That is, the other structure may be directly formed on the structure and directly contact the structure. In addition, the other structure may be first formed on the structure, and then the other structure may be formed on the other structure, that is, the structure is in indirect contact with the other structure.

[0031] It is worth noting that the terms "first", "second", etc. included in the embodiments of the present invention are used to distinguish similar objects, and are not necessarily used to describe a specific number or sequence. It should be understood that the terms used in this way can be interchangeable under appropriate circumstances, and this is merely a way of distinguishing objects with the same attributes when describing them in the embodiments of the present invention.

[0032] Embodiments of the present invention Figure 1 A schematic diagram showing the main process of the method for preparing a solar cell provided by an embodiment of the present invention is shown.

[0033] like Figure 1 As shown, the method for preparing a solar cell provided by an embodiment of the present invention may include the following steps:

[0034] Step S101: forming a first doped polysilicon layer 20 on the main surface of the silicon substrate 10, and forming a first doped silicon glass layer 30 on the surface of the first doped polysilicon layer 20, wherein the doping element in the first doped silicon glass layer 30 is the same as the doping element in the first doped polysilicon layer 20;

[0035] The silicon substrate may be an N-type silicon substrate or a P-type silicon substrate. Preferably, the silicon substrate is an N-type silicon substrate.

[0036] In this step, the main surface of the silicon substrate 10 forming the first doped polysilicon layer 20 can be the light-receiving surface of the solar cell, or can be the backlight surface of the solar cell. The light-receiving surface of the solar cell generally refers to the main surface facing the sunlight during the use of the solar cell, and the backlight surface of the solar cell generally refers to the main surface facing away from the sunlight during the use of the solar cell.

[0037] In the case where the main surface of the silicon substrate 10 is the light-receiving surface of the solar cell, the first doped polysilicon layer 20 is generally used to form the emitter of the solar cell. Therefore, the type of doping element contained in the first doped polysilicon layer 20 is generally opposite to the type of doping element of the silicon substrate. In the case where the silicon substrate 10 is an N-type silicon substrate, the type of doping element contained in the first doped polysilicon layer 20 is a P-type doping element such as boron (B); in the case where the silicon substrate 10 is a P-type silicon substrate, the type of doping element contained in the first doped polysilicon layer 20 is an N-type doping element such as phosphorus (P).

[0038] In the case where the main surface of the silicon substrate 10 is the backlight surface of the solar cell, the first doped polysilicon layer 20 is generally formed on the tunneling oxide layer 40 on the main surface of the silicon substrate 10, and it forms a passivation contact structure with the tunneling oxide layer 40. On this basis, the type of doping elements contained in the first doped polysilicon layer 20 is generally the same as the type of doping elements of the silicon substrate. In the case where the silicon substrate 10 is an N-type silicon substrate, the type of doping elements contained in the first doped polysilicon layer 20 is an N-type doping element such as phosphorus (P); in the case where the silicon substrate 10 is a P-type silicon substrate, the type of doping elements contained in the first doped polysilicon layer 20 is a P-type doping element such as boron (B). Among them, the thickness of the tunneling oxide layer 40 is generally 1 to 2nm, for example, the thickness of the tunneling oxide layer 40 can be 1nm, 1.2nm, 1.3nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, etc.

[0039] For this step to make an emitter for a solar cell, the corresponding structural changes are as follows: Figure 2 As shown. For this step applied to making a passivation contact structure for a solar cell, the corresponding structural changes are as follows Figure 3 shown.

[0040] The doping element included in the first doped silicon glass layer 30 is the same as the doping element included in the first doped polysilicon layer 20 . In addition, the main component of the first doped silicon glass layer 30 is silicon oxide.

[0041] The first doped silicon glass layer 30 can be formed during the high-temperature activation of the doping elements in the first doped polysilicon layer 20, or can be formed in a cooling stage after the doping elements are activated, or can be formed independently of the high-temperature activation of the doping elements. Preferably, the first doped silicon glass layer 30 is formed in a cooling stage after the doping elements are activated, which will be described in detail later and will not be repeated here.

[0042] Step S102: using laser to process the non-gate line region of the first doped silicon glass layer 30, so that the chemical etching rate of the non-gate line region in the first doped silicon glass layer 30 is greater than that of the gate line region;

[0043] Wherein, the gate line area refers to the gate line setting area, and the non-gate line area is other areas outside the gate line area. The non-gate line area and the gate line area are arranged side by side. Preferably, the non-gate line area and the gate line area are arranged alternately.

[0044] In this step, laser processing is performed to make the first doped silicon glass layer 30 easier to be chemically etched.

[0045] The laser wavelength used in the laser treatment in this step is generally 500nm to 550nm, for example, the laser wavelength may be 500nm, 510nm, 515nm, 520nm, 530nm, 540nm or 550nm, etc. By selecting the laser wavelength, it can be ensured that the first doped silicon glass layer 30 can be completely modified by the laser to meet the requirement of subsequent chemical etching for thickness control of the first doped polysilicon layer 20.

[0046] In this step, the side length of the laser spot used for laser processing is smaller than the spacing between two adjacent grid lines to ensure that the grid line area is not processed by the laser. The side length of the laser spot can be determined according to the spacing of the grid lines set in the solar cell. Here, there is no restriction on the side length of the laser spot.

[0047] For the light-receiving surface of the solar cell, the structure after this step is as follows Figure 2 As shown, for the backlight side of the solar cell, the structure after this step is as follows Figure 3 shown.

[0048] Step S103: removing the first doped silicon glass layer 30 and part or all of the first doped polysilicon layer 20 corresponding to the non-gate line region by chemical etching.

[0049] In a preferred embodiment, after the processing in step S103 , the thinned first doped polysilicon layer 20 still exists in the non-gate line region, so as to protect the tunneling oxide layer and ensure the passivation effect of the first doped polysilicon layer 20 .

[0050] For the light-receiving surface of the solar cell, the structure after this step is as follows Figure 2 As shown, for the backlight side of the solar cell, the structure after this step is as follows Figure 3 shown.

[0051] Specifically, the first doped polysilicon layer 20 is formed on the tunneling oxide layer 40 formed on the first main surface of the silicon substrate 10. After step S103, the first doped polysilicon layer 20 and the tunneling oxide layer 40 constitute a passivation contact structure on the back side of the solar cell. The first main surface of the silicon substrate 10 is the backlight surface.

[0052] The chemical solution used for chemical etching in this step may contain at least one of KOH, NaOH, TMAH and an etching additive.

[0053] The preparation method provided by the embodiment of the present invention forms a first doped silicon glass layer on the first doped polysilicon layer after forming the first doped polysilicon layer, and processes the non-gate line area of ​​the first doped silicon glass layer by laser to modify the non-gate line area and make it easier to be etched by a chemical solution. Then, in the subsequent treatment by chemical etching, the first doped silicon glass layer in the non-gate line area is easier to remove. Then, in the process of removing the first doped silicon glass layer in the gate line area by chemical etching, the gate line area and the non-gate line area are etched at the same time, which can remove the first doped silicon glass layer in the non-gate line area more quickly. The non-gate line area lacks the protection of the first doped silicon glass layer, and part or all of the first doped polysilicon layer in the non-gate line area will also be etched and removed, thereby achieving the purpose of thinning the doped layer in the non-metallic electrode area, effectively reducing the parasitic absorption caused by the doped layer, thereby effectively improving the short-circuit current density and photoelectric conversion efficiency of the solar cell.

[0054] In addition, the preparation method provided by the embodiment of the present invention replaces the laser processing with the mask setting, without adding any additional steps, and without the need to specially set up a mask or remove the mask. Compared with the mask setting and mask removal processes, the laser processing has relatively low requirements for alignment accuracy. The desired structure can be obtained by laser processing and one-step chemical etching. The process is relatively simple and easy to control, which is conducive to industrial production and can effectively control costs. The technical solution provided by the present invention can ensure that the existing process route remains unchanged and is conducive to the upgrading of the existing route.

[0055] Furthermore, due to the presence of the first doped silicon glass layer 30, it can block the laser, so that the above-mentioned laser processing process will not damage the tunneling oxide layer, ensuring that the tunneling oxide layer in the passivation contact structure formed by the above-mentioned method has a complete tunneling effect, so that the preparation process has a relatively wide process window, which is conducive to mass production and effectively reduces the mass production cost while effectively ensuring the yield rate of solar cells.

[0056] In addition to the above embodiments exemplarily providing the doped polysilicon layer required for preparing the emitter on the front side of the solar cell or the doped polysilicon layer required for preparing the passivation contact structure on the back side of the solar cell, steps S101 to S103 provided in the embodiments of the present invention can also be used to prepare the doped polysilicon layer required for the emitter on the front side of the solar cell and the passivation contact structure on the back side of the solar cell.

[0057] Specifically, Figure 4The structure change shown in the figure is that first, a stacked first doped polysilicon layer 20 (the first doped polysilicon layer 20 is a part of the emitter) and a first doped silicon glass layer 30 are prepared on the second main surface of the silicon substrate 10 (i.e., the light-receiving surface of the silicon substrate 10) through the processing procedure of step S101; then, the first doped silicon glass layer 30 on the second main surface of the silicon substrate 10 is processed by laser; further, a tunneling oxide layer 40 is formed on the first main surface of the silicon substrate 10 (i.e., the backlight surface of the silicon substrate 10); and then, the processing procedure of step S101 is performed again to form a tunneling oxide layer 40 on the tunneling oxide layer 40. A first doped polysilicon layer 20 (the first doped polysilicon layer 20 is a part of the passivation contact structure) and a first doped silicon glass layer 30 are stacked on the passivation layer 40; further, through the processing procedure of step S102, the first doped silicon glass layer 30 on the first main surface of the silicon substrate 10 is removed; finally, through step S103, the first doped silicon glass layer 30 and a part of the first doped polysilicon layer 20 on the first main surface of the silicon substrate 10 are removed by etching together, and the first doped silicon glass layer 30 and a part of the first doped polysilicon layer 20 on the first main surface of the silicon substrate 10 are removed, Figure 4 The structure shown.

[0058] Furthermore, the specific implementation of the above step S101 may include the following steps:

[0059] Step S1011: depositing a doping layer on the main surface of the silicon substrate 10 by PECVD (plasma enhanced chemical vapor deposition);

[0060] In this step, the first reaction gas containing the doping element is generally used in H2 or Ar atmosphere to in-situ deposit the doping layer on the main surface of the silicon substrate 10. When the doping element is phosphorus, the first reaction gas is a mixed gas of SiH4 and PH3. When the doping element is boron, the first reaction gas can be a mixed gas of SiH4 and TMB (trimethyl boron).

[0061] Specifically, the thickness of the doping layer deposited in this step is generally 100 nm to 150 nm. For example, the thickness of the doping layer may be 100 nm, 110 nm, 120 nm, 123 nm, 125 nm, 130 nm, 140 nm, 145 nm or 150 nm.

[0062] Deposition conditions of this step: deposition temperature can be 380℃~450℃; deposition power can be 4000W~13000W; duty cycle can be 1:8~1:24; deposition time can be 600s~1200s; pressure can be 200~350Pa. For example, the deposition temperature can be 380℃, 390℃, 400℃, 420℃, 430℃, 440℃, 450℃, etc. For example, the deposition power can be 4000W, 5000W, 6000W, 7000W, 8000W, 90000W, 10000W, 11000W, 12000W, 13000W, etc. For example, the duty cycle can be 1:8, 1:9, 1:10, 1:11, 1:12, etc. For example, the deposition time may be 600s, 700s, 800s, 900s, 1000s, 1200s, etc. For another example, the pressure may be 200Pa, 220Pa, 230Pa, 240Pa, 250Pa, 270Pa, 290Pa, 300Pa, 320Pa, 330Pa, 340Pa, 350Pa, etc. By controlling the deposition conditions within the above range, the formation of the required doping layer is ensured while minimizing energy consumption. Among them, the above deposition temperature, deposition power, duty cycle, deposition time and pressure can be arbitrarily combined within the above numerical range. Preferably, the above deposition condition combination is: deposition temperature is 400°C; power is 10000W, duty cycle is 1:10, deposition time is 900s, and pressure is 250Pa.

[0063] Step S1012: performing high temperature annealing on the deposited doped layer to form a first doped polysilicon layer 20;

[0064] In this step, the temperature of the high temperature annealing treatment is 860°C to 950°C, and the time of the high temperature annealing treatment is 10 minutes to 40 minutes. For example, the temperature of the high temperature annealing treatment can be 860°C, 870°C, 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C or 950°C.

[0065] Step S1013 : in the cooling stage after the high temperature annealing treatment, depositing a first doped silicon glass layer 30 on the first doped polysilicon layer 20 .

[0066] For step S1013, after the temperature of the high temperature annealing is reduced to 650°C to 780°C, the first doped polysilicon layer 20 is passed through a second reaction gas containing doping elements and oxygen for a duration of 10 minutes to 50 minutes. For example, the temperature of the high temperature annealing is reduced to 650°C, 660°C, 680°C, 690°C, 700°C, 720°C, 730°C, 750°C, 770°C or 780°C, and the duration can be 10 minutes, 20 minutes, 25 minutes, 30 minutes, 33 minutes, 40 minutes, 45 minutes or 50 minutes. The first doped silicon glass layer 30 deposited in the cooling stage after the high temperature annealing treatment is conducive to laser treatment modification. Compared with the area not treated by the laser, the first doped silicon glass layer 30 after the laser treatment is convenient to be removed by chemical etching.

[0067] The flow rate of the second reaction gas is generally 1000 sccm / min to 2000 sccm / min, and the flow rate of oxygen is 500 sccm / min to 1500 sccm / min. For example, the flow rate of the second reaction gas can be 1000 sccm / min, 1200 sccm / min, 1300 sccm / min, 1500 sccm / min, 1600 sccm / min, 1700 sccm / min, 1800 sccm / min or 2000 sccm / min.

[0068] For an N-type silicon substrate, the first doped polysilicon layer 20 is a part of the passivation contact structure on the back of the solar cell, and the second reaction gas containing doping elements used to form the first doped silicon glass layer 30 is generally POCl3. That is, in the process of forming the first doped silicon glass layer 30, the first doped polysilicon layer 20 is further doped to form a highly doped polysilicon layer to enhance the passivation effect.

[0069] The thickness of the first doped silicon glass layer 30 deposited by the above process is generally 10 nm to 70 nm. For example, the thickness of the first doped silicon glass layer 30 can be 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, etc.

[0070] In addition, for an N-type silicon substrate, when the first doped polysilicon layer 20 is a part of the emitter on the front side of a solar cell, the second reaction gas containing doping elements used to form the first doped silicon glass layer 30 is generally BCl 3 or BBr 3 .

[0071] Furthermore, in the case where the above steps S101 to S103 are for preparing a doped polysilicon layer in a passivation contact structure on the back side of a solar cell, before the above step S101, the following may be further included:

[0072] Step 01: forming a second doped polysilicon layer 50 and a second doped silicon glass layer 60 by in-situ diffusion on a second main surface of a silicon substrate 10 with a double textured surface, wherein the type of doping elements included in the second doped polysilicon layer is opposite to the type of doping elements included in the first doped polysilicon layer 20;

[0073] For example, if the doping type of the first doped polysilicon layer 20 is N-type, the doping type of the second doped polysilicon layer 50 is P-type.

[0074] Step 02: Clean the second doped polysilicon layer 50 and the second doped silicon glass layer 60 coated on the first main surface of the silicon substrate 10, and polish the first main surface of the silicon substrate 10.

[0075] Through the above process, a velvet structure is formed on the light-receiving surface of the silicon substrate 10 to increase the light trapping performance of the light-receiving surface of the silicon substrate 10. The backlight surface of the silicon substrate 10 is a polished surface to ensure that the tunneling oxide layer and the doped polysilicon layer can be evenly formed on the backlight surface of the silicon substrate 10 to ensure the passivation contact effect.

[0076] Preferably, the light-receiving surface of the silicon substrate 10 adopts a velvet structure, whose light-trapping performance can not only compensate for the parasitic absorption of the second doped polysilicon layer 50 formed by in-situ diffusion on the second main surface of the silicon substrate 10, but also improve the light absorption rate of the front side of the solar cell.

[0077] Further, based on the above step 01 and step 02, the above step S103 may further include: simultaneously removing the second doped silicon glass layer 60 on the second main surface of the silicon substrate 10 .

[0078] Furthermore, after the second doped polycrystalline layer on the front side of the solar cell and the tunneling oxide layer and the first doped polycrystalline silicon layer on the back side are prepared, the method for preparing the solar cell may further include the following steps:

[0079] Step 4: forming an Al2O3 layer 70 on the second doped polysilicon layer 50;

[0080] This step is generally achieved by depositing an Al2O3 thin film by ALD (atomic layer deposition).

[0081] Step 5: forming a passivation anti-reflection layer 80 on the Al2O3 layer 70 and the first doped silicon glass layer 30 respectively;

[0082] This step is achieved by depositing a nitride film or a nitride oxide film using PECVD equipment.

[0083] Step 6: Print metal grid lines on the passivation anti-reflection layer 80 on the two main surfaces and sinter them, wherein the metal grid lines printed on the first main surface of the silicon substrate 10 are in contact with the grid line area, and the metal grid lines printed on the second main surface of the silicon substrate 10 are in contact with the Al2O3 layer 70.

[0084] The above processing can be completed by using the existing solar cell production process.

[0085] Furthermore, another embodiment of the present invention provides a method for preparing a solar cell. Figure 5 As shown, the method for preparing the solar cell may include the following steps:

[0086] Step S501: forming a second doped polysilicon layer 50 and a second doped silicon glass layer 60 by in-situ diffusion on the second main surface of the silicon substrate 10 with a double textured surface, wherein the type of doping elements included in the second doped polysilicon layer is opposite to the type of doping elements included in the first doped polysilicon layer 20;

[0087] For this Figure 5 In the embodiment shown, the structure of the corresponding solar cell changes as shown in FIG. Figure 6 and Figure 7 shown.

[0088] In this embodiment, an N-type silicon substrate is selected, the first doping element is phosphorus, and the second doping element is boron.

[0089] In this step, the second doped silicon glass layer 60 is formed in the process of forming the second doped polysilicon layer 50 , that is, the process of forming the second doped silicon glass layer 60 in this step is different from the subsequent process of forming the first doped silicon glass layer 30 .

[0090] Step S502: cleaning the second doped polysilicon layer 50 and the second doped silicon glass layer 60 coated on the first main surface of the silicon substrate 10, and polishing the first main surface of the silicon substrate 10;

[0091] The first main surface of the silicon substrate 10 is the backlight surface of the solar cell. The polishing process in this step can ensure that the tunneling oxide layer formed subsequently is relatively uniform, so as to ensure the tunneling effect.

[0092] Step S503: in an H2 or Ar atmosphere, a first reaction gas containing a doping element in-situ deposits a doping layer with a thickness of 100 nm to 150 nm on the main surface of the silicon substrate 10 by PECVD;

[0093] For an N-type silicon substrate, the first doping element is phosphorus, and the first reaction gas is a mixed gas of SiH4 and PH3.

[0094] Step S504: performing high temperature annealing treatment on the deposited doped layer at a temperature of 860° C. to 950° C. for 10 min to 40 min to form a first doped polysilicon layer 20;

[0095] Step S505: after the temperature is reduced to 650°C to 780°C after the high temperature annealing treatment, POCl3 with a flow rate of 1000sccm / min to 2000sccm / min and oxygen with a flow rate of 500sccm / min to 1500sccm / min are introduced into the first doped polysilicon layer 20 for 10min to 50min, and a first doped silicon glass layer 30 with a thickness of 10nm to 70nm is deposited on the first doped polysilicon layer 20;

[0096] Step S506: using a laser with a wavelength of 500-550 nm to process the non-gate line region of the first doped silicon glass layer 30, so that the chemical etching rate of the non-gate line region in the first doped silicon glass layer 30 is greater than that of the gate line region;

[0097] Step S507: removing the first doped silicon glass layer 30 and part or all of the first doped polysilicon layer 20 corresponding to the non-gate line region by chemical etching, and simultaneously removing the second doped silicon glass layer 60 on the second main surface of the silicon substrate 10;

[0098] Step S508: forming an Al2O3 layer 70 on the second doped polysilicon layer 50;

[0099] Step S509: forming a passivation anti-reflection layer 80 on the Al2O3 layer 70 and the first doped silicon glass layer 30 respectively;

[0100] Step S510: Printing metal grid lines on the passivation anti-reflection layer 80 on the two main surfaces and sintering, wherein the metal grid lines printed on the first main surface of the silicon substrate 10 are in contact with the grid line area, and the metal grid lines printed on the second main surface of the silicon substrate 10 are in contact with the Al2O3 layer 70.

[0101] Furthermore, an embodiment of the present invention provides a solar cell. The solar cell is prepared by the preparation method provided in the above embodiment. Specifically, Figure 8 and Fig. 9 As shown, the solar cell may include: a silicon substrate 10 and a first doped polysilicon layer 20 located on a main surface of the silicon substrate 10, wherein:

[0102] The first doped polysilicon layer 20 includes: a gate line region and a non-gate line region arranged in an arranged manner, wherein:

[0103] The thickness of the gate line region is greater than the thickness of the non-gate line region.

[0104] Specifically, the solar cell can be Figure 8 In the structure shown in FIG. 1 , the first doped polysilicon layer 20 exists on two main surfaces of the silicon substrate 10. The solar cell may also be as shown in FIG. Fig. 9 In the structure shown, the first doped polysilicon layer 20 is present on the backlight side of the silicon substrate 10 .

[0105] Furthermore, if Figure 8 and Fig. 9 As shown, the solar cell may further include: a tunneling passivation layer 40 disposed on one main surface of the silicon substrate 10 , wherein the first doped polysilicon layer 20 is stacked on the tunneling passivation layer 40 .

[0106] The doping concentration of the gate line region is greater than the doping concentration of the non-gate line region.

[0107] The gate line area refers to the gate line setting area, and the non-gate line area refers to other areas outside the gate line area.

[0108] Furthermore, if Figure 8 and Fig. 9 As shown, the solar cell may further include: a doped polysilicon layer ( Figure 8 The first doped polysilicon layer 20 or Fig. 9 The Al2O3 layer 70 and the passivation anti-reflection layer 80 on the second doped polysilicon layer 50 shown in the figure, the passivation anti-reflection layer 80 stacked on the first doped polysilicon layer 20 on the backlight surface of the silicon substrate 10, and the metal gate line arranged on the light-receiving surface of the silicon substrate 10 and electrically connected to the Al2O370, and the metal gate line arranged on the backlight surface of the silicon substrate 10 and electrically connected to the first doped polysilicon layer 20.

[0109] The above solar cell structure can reduce parasitic absorption of light, since the non-gate line region in the doped polysilicon layer is relatively thin, thereby effectively improving the light utilization rate of the solar cell.

[0110] Example:

[0111] S1: Double-sided texturing is performed on an N-type single-crystal silicon wafer with a resistivity of 1.0Ω, and boron is diffused on the light-receiving side of the single-crystal silicon wafer to form a boron-doped polysilicon layer and a borosilicate glass layer. The boron-doped polysilicon layer and the borosilicate glass layer coated on the backlight side of the single-crystal silicon wafer are removed, and then polished to obtain a silicon wafer with a polished backlight side.

[0112] S2: Using PECVD equipment, power 10000W, duty cycle 5:90, at a deposition temperature of 400℃, N2O was introduced to react with the backlight surface of the silicon wafer, the deposition time was controlled to be 60s, the pressure was 200Pa, and a 1-2nm tunneling oxide layer (SiO x ).

[0113] S3: Continue in the PECVD equipment, introduce SiH4, PH3 and H2 on the tunnel oxide layer to deposit in-situ doped amorphous silicon with a thickness of 150nm, control the deposition temperature to 400℃; power 10000W, duty cycle 5:50, deposition time 900s, pressure 250Pa, and obtain SiO x - Amorphous silicon doped layer.

[0114] S4: Annealing temperature is, time is to prepare SiO x -The silicon wafer with the amorphous silicon doped layer is subjected to high temperature annealing at 900°C for 20 minutes to form a phosphorus-doped polysilicon layer.

[0115] S5: After the annealing temperature reaches 750°C, POCl3 and O2 are introduced, and the deposition time is controlled to be 10 minutes, and a phosphosilicate glass layer with a thickness of 20 nm is deposited on the phosphorus-doped polysilicon layer.

[0116] S6: Then, a laser with a wavelength of 532 nanometers and a laser spot side length of 150 um is used to perform graphic local processing, and the laser processing area is a non-grid line area.

[0117] S7: Etching the silicon wafer processed in step 6 in an alkaline solution to remove the phosphorus-silicate glass layer on the backlight side and the phosphorus-silicate glass layer on the light-receiving side, thereby obtaining a phosphorus-doped polysilicon layer with a thickness of 60 nm in the non-gate line area.

[0118] S8: Perform coating passivation treatment on the light-receiving surface of the silicon wafer.

[0119] S9: depositing a passivation film on the backlight side of the silicon wafer.

[0120] S10: printing silver aluminum grid lines on the light-receiving side of the silicon wafer; overprinting silver metal grid lines on the backlight side of the silicon wafer and sintering them simultaneously with the silver aluminum grid lines on the front side to obtain a solar cell.

[0121] Comparative Example:

[0122] The only difference from the above embodiment is that step S6 is omitted, and a phosphorus-doped polysilicon layer with uniform thickness is obtained.

[0123] The solar cells obtained in the above embodiment and the comparative example were subjected to performance tests, and the test results are shown in Table 1. As can be seen from Table 1, compared with the comparative example, the current density (Jsc (mA / cm 2 )) increased by about 0.2mA / cm 2 , the battery efficiency (Eta(%)) increased by about 0.1%.

[0124] Table 1

[0125] project <![CDATA[Jsc(mA / cm 2 )]]> Voc(V) FF(%) Eta(%) Comparative Example 41.248 0.7372 84.18 25.596 Example 41.487 0.7374 83.98 25.690

[0126] In summary, the embodiments of the present invention provide the following technical solutions:

[0127] Technical solution 1, a method for preparing a solar cell, comprising:

[0128] Step 1, forming a first doped polysilicon layer 20 on the main surface of the silicon substrate 10, and forming a first doped silicon glass layer 30 on the surface of the first doped polysilicon layer 20, wherein the doping element in the first doped silicon glass layer 30 is the same as the doping element in the first doped polysilicon layer 20;

[0129] Step 2, using laser to process the non-gate line region of the first doped silicon glass layer 30, so that the chemical etching rate of the non-gate line region in the first doped silicon glass layer 30 is greater than that of the gate line region;

[0130] Step 3: remove the first doped silicon glass layer 30 and part or all of the first doped polysilicon layer 20 corresponding to the non-gate line area by chemical etching.

[0131] Technical solution 2: According to the method for preparing a solar cell according to technical solution 1, step 1 comprises:

[0132] Step 11, depositing a doping layer on the main surface of the silicon substrate 10 by PECVD;

[0133] Step 12: performing high temperature annealing on the deposited doped layer to form a first doped polysilicon layer 20;

[0134] Step 13: in a cooling stage after the high temperature annealing treatment, depositing a first doped silicon glass layer 30 on the first doped polysilicon layer 20 .

[0135] Technical solution 3: A method for preparing a solar cell according to technical solution 2,

[0136] Step 11: In an H2 or Ar atmosphere, a first reaction gas containing a doping element in-situ deposits a doping layer on the main surface of the silicon substrate 10;

[0137] and / or,

[0138] The thickness of the doping layer formed in step 11 is 100nm to 150nm;

[0139] and / or,

[0140] The temperature of the high temperature annealing treatment in step 12 is 860° C. to 950° C., and the time of the high temperature annealing treatment is 10 min to 40 min.

[0141] Technical solution 4: According to the method for preparing a solar cell according to technical solution 2 or 3, step 13 comprises:

[0142] After the temperature of the high temperature annealing is reduced to 650° C. to 780° C., a second reaction gas containing doping elements and oxygen are introduced into the first doped polysilicon layer 20 for a duration of 10 min to 50 min.

[0143] Technical solution 5: The method for preparing a solar cell according to technical solution 4,

[0144] The flow rate of the second reaction gas is 1000 sccm / min to 2000 sccm / min, and the flow rate of the oxygen is 500 sccm / min to 1500 sccm / min;

[0145] and / or,

[0146] The thickness of the deposited first doped silicon glass layer 30 is 10 nm to 70 nm.

[0147] Technical solution 6: A method for preparing a solar cell according to any one of technical solutions 1 to 3 and 5,

[0148] The first doped polysilicon layer 20 is formed on the tunneling oxide layer 40 formed on the first main surface of the silicon substrate 10, wherein the first doped polysilicon layer 20 processed in step 3 and the tunneling oxide layer 40 constitute a passivation contact structure on the back side of the solar cell.

[0149] Technical solution 7: The method for preparing a solar cell according to technical solution 6,

[0150] The silicon substrate is an N-type silicon substrate, and the first doped polysilicon layer 20 is a phosphorus first doped polysilicon layer.

[0151] Technical solution 8: The method for preparing a solar cell according to technical solution 7,

[0152] The second reaction gas containing doping elements used to form the first doped silicon glass layer 30 is POCl 3 .

[0153] Technical solution 9. The method for preparing a solar cell according to technical solution 7 or 8,

[0154] The laser wavelength used in step 2 laser treatment is 500-550nm;

[0155] and / or,

[0156] Step 2: The side length of the laser spot used for laser processing is smaller than the spacing between two adjacent grid lines;

[0157] and / or,

[0158] The chemical solution used for chemical etching in step 3 includes at least one of KOH, NaOH, TMAH and an etching additive.

[0159] Technical solution 10: The method for preparing a solar cell according to technical solution 6, further comprising:

[0160] Step 01, forming a second doped polysilicon layer 50 and a second doped silicon glass layer 60 by in-situ diffusion on a second main surface of a silicon substrate 10 with a double textured surface, wherein the type of doping elements contained in the second doped polysilicon layer is opposite to the type of doping elements contained in the first doped polysilicon layer 20;

[0161] Step 02: clean the second doped polysilicon layer 50 and the second doped silicon glass layer 60 coated on the first main surface of the silicon substrate 10, and polish the first main surface of the silicon substrate 10.

[0162] Technical solution 11. The method for preparing a solar cell according to technical solution 10,

[0163] Step 3 also includes: simultaneously removing the second doped silicon glass layer 60 on the second main surface of the silicon substrate 10;

[0164] Preferably,

[0165] The preparation method further comprises:

[0166] Step 4, forming an Al2O3 layer 70 on the second doped polysilicon layer 50;

[0167] Step 5, forming a passivation anti-reflection layer 80 on the Al2O3 layer 70 and the first doped silicon glass layer 30 respectively;

[0168] Step 6: Print metal grid lines on the passivation anti-reflection layer 80 on the two main surfaces and sinter them, wherein the metal grid lines printed on the first main surface of the silicon substrate 10 are in contact with the grid line area, and the metal grid lines printed on the second main surface of the silicon substrate 10 are in contact with the Al2O3 layer 70.

[0169] Technical solution 12, a solar cell prepared by the preparation method according to any one of technical solutions 1 to 11, comprising: a silicon substrate 10 and a first doped polysilicon layer 20 located on a main surface of the silicon substrate 10, wherein:

[0170] The first doped polysilicon layer 20 includes: a gate line region and a non-gate line region arranged in an arranged manner, wherein:

[0171] The thickness of the gate line region is greater than the thickness of the non-gate line region.

[0172] Technical solution 13: The solar cell according to technical solution 12 further comprises: a tunnel passivation layer 40 disposed on a main surface of the silicon substrate 10, wherein:

[0173] The first doped polysilicon layer 20 is stacked on the tunnel passivation layer 40 .

[0174] Technical solution 14. The solar cell according to technical solution 11 or 12,

[0175] The doping concentration of the gate line region is greater than the doping concentration of the non-gate line region.

[0176] The introduction provided in the above steps is only used to help understand the method, structure and core idea of ​​the present invention. For ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also belong to the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a solar cell, characterized in that: include: Step 1: forming a first doped polysilicon layer (20) on the main surface of a silicon substrate (10), and forming a first doped silicon glass layer (30) on the surface of the first doped polysilicon layer (20), wherein the doping element in the first doped silicon glass layer (30) is the same as the doping element in the first doped polysilicon layer (20); Step 2: Processing the non-gate line region of the first doped silicon glass layer (30) with a laser, so that the chemical etching rate of the non-gate line region in the first doped silicon glass layer (30) is greater than that of the gate line region; Step 3: removing the first doped silicon glass layer (30) and part or all of the first doped polysilicon layer (20) corresponding to the non-gate line region by chemical etching.

2. The method for preparing a solar cell according to claim 1, characterized in that: Step 1 includes: Step 11, depositing a doping layer on the main surface of the silicon substrate (10) by PECVD; Step 12: performing high temperature annealing on the deposited doped layer to form a first doped polysilicon layer (20); Step 13: in a cooling stage after the high temperature annealing treatment, depositing a first doped silicon glass layer (30) on the first doped polysilicon layer (20).

3. The method for preparing a solar cell according to claim 2, characterized in that: Step 11, in an H2 or Ar atmosphere, a first reaction gas containing a doping element in-situ deposits a doping layer on the main surface of the silicon substrate (10); and / or, The thickness of the doping layer formed in step 11 is 100nm to 150nm; and / or, The temperature of the high temperature annealing treatment in step 12 is 860° C. to 950° C., and the time of the high temperature annealing treatment is 10 min to 40 min.

4. The method for preparing a solar cell according to claim 2 or 3, characterized in that: Step 13 includes: After the temperature of the high temperature annealing is reduced to 650° C. to 780° C., a second reaction gas containing doping elements and oxygen are introduced into the first doped polysilicon layer (20) for a duration of 10 minutes to 50 minutes.

5. The method for preparing a solar cell according to claim 4, characterized in that: The flow rate of the second reaction gas is 1000 sccm / min to 2000 sccm / min, and the flow rate of the oxygen is 500 sccm / min to 1500 sccm / min; and / or, The thickness of the deposited first doped silicon glass layer (30) is 10 nm to 70 nm.

6. The method for preparing a solar cell according to any one of claims 1 to 3 and 5, characterized in that: The first doped polysilicon layer (20) is formed on a tunneling oxide layer (40) formed on a first main surface of a silicon substrate (10), wherein the first doped polysilicon layer (20) processed in step 3 and the tunneling oxide layer (40) constitute a passivation contact structure on the back side of a solar cell.

7. The method for preparing a solar cell according to claim 6, characterized in that: The silicon substrate is an N-type silicon substrate, and the first doped polysilicon layer (20) is a phosphorus first doped polysilicon layer.

8. The method for preparing a solar cell according to claim 7, characterized in that: The second reaction gas containing doping elements used to form the first doped silicon glass layer (30) is POCl3.

9. The method for preparing a solar cell according to claim 7 or 8, characterized in that: The laser wavelength used in step 2 laser treatment is 500-550nm; and / or, Step 2: The side length of the laser spot used for laser processing is smaller than the spacing between two adjacent grid lines; and / or, The chemical solution used for chemical etching in step 3 includes at least one of KOH, NaOH, TMAH and an etching additive.

10. A solar cell prepared by the preparation method according to any one of claims 1 to 9, characterized in that it comprises: A silicon substrate (10) and a first doped polysilicon layer (20) located on a main surface of the silicon substrate (10), wherein: The first doped polysilicon layer (20) comprises: a gate line region and a non-gate line region arranged in an arranged manner, wherein: The thickness of the gate line region is greater than the thickness of the non-gate line region.

Citation Information

Cited By

  • Photovoltaic cell and manufacturing method thereof

    CN119789584A

  • Preparation method of thin grid side edge morphology of solar cell and solar cell

    CN120568906A

  • Solar cell and its manufacturing method

    JP7769834B1

  • Solar cell manufacturing methods

    JP7830756B1