Lithium ion secondary battery
By using a layered structure lithium transition metal composite oxide with high Ni content and Si-containing negative electrode active material in lithium-ion secondary batteries, the problem of increasing resistance caused by the reduction of cobalt content is solved, and the initial resistance and storage resistance are suppressed is achieved. , improves battery performance and durability.
Patent Information
- Application Number
- CN202410528056.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-01
- Filing Date
- 2024-04-29
- Publication Date
- 2024-11-01
AI Technical Summary
When the cobalt content in the positive electrode active substance of the lithium-ion secondary battery is reduced, the initial resistance of the lithium-ion secondary battery and the resistance during storage are significantly increased, which affects the performance of the battery.
The layered lithium transition metal composite oxide containing Li, Ni and Mn is used as the positive electrode active material, and carbon material and Si-containing material are added to the negative electrode active material to control the Ni content and primary particles of the lithium transition metal composite oxide. The aspect ratio ensures that the content ratio of Ni to metal elements other than Li is 75 mol % or more, and the aspect ratio of primary particles is 1.9 or more, and the content ratio of Si elements in the negative electrode active material is 5 mass %~ 10 mass %.
It effectively suppresses the increase in initial resistance and during storage, improves the performance and durability of lithium-ion secondary batteries, and is suitable for various vehicle driving power supplies and small power storage devices.
Smart Images

Figure CN118888818A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a lithium ion secondary battery. Background Art
[0002] Lithium-ion secondary batteries are suitable for use as driving power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and electric vehicles (BEVs), and their demand is rapidly expanding. As positive electrode active materials used in lithium-ion secondary batteries, lithium transition metal composite oxides are used, among which lithium nickel cobalt manganese composite oxides containing Ni, Co, and Mn as shown in Japanese Patent Publication No. 2017-191662 can be cited.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Publication No. 2017-191662 Summary of the invention
[0006] On the other hand, in recent years, as the demand for lithium-ion secondary batteries has expanded, there is a concern that cobalt (Co) used in lithium-ion secondary batteries will be depleted. As such a countermeasure, it is possible to consider reducing the content of Co in the positive electrode active material. However, the inventors conducted in-depth research and found the following problem: when the content of Co in the positive electrode active material is reduced, the initial resistance of the lithium-ion secondary battery and the increase in resistance during storage become significant.
[0007] The technology disclosed herein has been accomplished in view of the above circumstances, and an object of the technology is to provide a lithium ion secondary battery in which the increase in initial resistance and resistance during storage is suppressed, although the cobalt content in the positive electrode active material is reduced.
[0008] The technology disclosed herein relates to a lithium ion secondary battery, characterized in that it comprises a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte, the positive electrode comprising a positive electrode active material layer containing a positive electrode active material, the positive electrode active material comprises a lithium transition metal composite oxide having a layered structure containing Li, Ni and Mn, the lithium transition metal composite oxide is a secondary particle formed by aggregation of primary particles, the content of the Ni relative to the total of metal elements other than the Li is 75 mol% or more, the aspect ratio of the primary particles is 1.9 or more, the negative electrode comprising a negative electrode active material layer containing a negative electrode active material, the negative electrode active material comprises a carbon material and a Si-containing material, and when the total amount of the negative electrode active material is set to 100 mass%, the content ratio of the Si element in the negative electrode active material is 5 mass% to 10 mass%.
[0009] According to this configuration, the composition in the positive electrode active material, specifically the content of Ni in the lithium transition metal composite oxide is set to a specified range. In addition, the lithium transition metal composite oxide is a secondary particle, and the aspect ratio of the primary particle of the lithium transition metal composite oxide is greater than 1.9. Furthermore, as a negative electrode active material, a specified amount of Si-containing material is also included in addition to the carbon material. Thus, a lithium ion secondary battery can be provided that suppresses the increase in initial resistance and resistance during storage while reducing the cobalt content in the positive electrode active material. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 This is a cross-sectional view schematically showing the internal structure of a lithium ion secondary battery according to one embodiment.
[0011] Figure 2 This is a schematic exploded view showing the structure of an electrode body of a lithium ion secondary battery according to one embodiment.
[0012] Figure 3 It is a schematic diagram showing the structure of a positive electrode active material according to one embodiment.
[0013] Figure 4 It is a schematic diagram showing the structure of a negative electrode sheet (negative electrode) according to one embodiment.
[0014] Figure 5 The structure of the negative electrode sheet (negative electrode) of the second embodiment is shown in FIG. Figure 4 The corresponding figure.
[0015] Explanation of symbols
[0016] 20 Electrode body
[0017] 30 Battery housing
[0018] 36 Safety valve
[0019] 42 Positive terminal
[0020] 42a Positive electrode collector plate
[0021] 44 Negative terminal
[0022] 44a Negative collector plate
[0023] 50 positive electrode sheet (positive electrode)
[0024] 52 positive electrode collector
[0025] 52a Positive electrode active material layer non-formed portion
[0026] 54 Positive electrode active material layer
[0027] 56 Positive electrode active material
[0028] 56a Lithium transition metal composite oxide
[0029] 56c covered part
[0030] 56p primary particle
[0031] 60, 160 Negative electrode sheet (negative electrode)
[0032] 62 negative electrode collector
[0033] 62a Negative electrode active material layer non-formed portion
[0034] 64, 164 Negative electrode active material layer
[0035] 164u negative electrode upper layer
[0036] 164d Negative electrode lower layer
[0037] 66 Negative electrode active material
[0038] 66c Carbon Material
[0039] 66s Si-containing materials
[0040] 70 Isolation
[0041] 80 Non-aqueous electrolyte
[0042] 100 Lithium-ion secondary battery DETAILED DESCRIPTION
[0043] Hereinafter, some preferred embodiments of the lithium ion secondary battery disclosed herein are described with appropriate reference to the accompanying drawings. Matters other than those specifically mentioned in this specification and required for the implementation of the present disclosure (for example, the general composition and manufacturing process of the lithium ion secondary battery of the present invention are not characterized) can be grasped as design matters for those skilled in the art based on the prior art in this field. The lithium ion secondary battery disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in this field.
[0044] It should be noted that in the following drawings, the same symbols are marked for components and parts that play the same role, and repeated descriptions are sometimes omitted or simplified. In addition, the expression "A to B" indicating a range in this specification includes the meaning of greater than A and less than B, as well as the meaning of "preferably greater than A" and "preferably less than B". In addition, in this specification, "lithium-ion secondary battery" (hereinafter sometimes referred to as "battery") refers to all electrical storage devices that use lithium ions as charge carriers and can be repeatedly charged and discharged by the charge transfer of lithium ions between the positive and negative electrodes.
[0045] Hereinafter, the present disclosure will be described in detail by taking a flat rectangular lithium ion secondary battery having a flat electrode body and a flat battery case as an example, but the present disclosure is not intended to be limited to the contents described in this embodiment.
[0046] Figure 1 This is a cross-sectional view schematically showing the internal structure of a lithium ion secondary battery according to one embodiment. Figure 1 The lithium-ion secondary battery 100 shown is a sealed battery constructed by accommodating a flat electrode body 20 and a non-aqueous electrolyte 80 in a flat square battery case (i.e., an outer container) 30. The battery case 30 is provided with a positive terminal 42 and a negative terminal 44 for external connection, and a thin-walled safety valve 36 that is set to release the internal pressure when the internal pressure of the battery case 30 rises to a specified level or above. In addition, the battery case 30 is provided with an injection port (not shown) for injecting the non-aqueous electrolyte 80. The positive terminal 42 is electrically connected to the positive electrode collector plate 42a. The negative terminal 44 is electrically connected to the negative electrode collector plate 44a. As the material of the battery case 30, a metal material such as aluminum, which is lightweight and has good thermal conductivity, is used.
[0047] Figure 2 1 is a schematic exploded view showing the structure of an electrode body of a lithium ion secondary battery according to one embodiment. Figure 1 and Figure 2 As shown, the electrode body 20 has a form in which a strip-shaped positive electrode sheet 50 and a strip-shaped negative electrode sheet 60 are overlapped and wound in the length direction via two strip-shaped separators 70. The positive electrode sheet 50 has a structure in which a positive electrode active material layer 54 is formed on one side or both sides (here both sides) of a long strip-shaped positive electrode collector 52 along the length direction. The negative electrode sheet 60 has a structure in which a negative electrode active material layer 64 is formed on one side or both sides (here both sides) of a long strip-shaped negative electrode collector 62 along the length direction. The positive electrode active material layer non-formed portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode collector 52 is exposed) and the negative electrode active material layer non-formed portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode collector 62 is exposed) are formed to extend outward from both ends of the winding axis direction (i.e., the sheet width direction orthogonal to the above-mentioned length direction) of the electrode body 20. The positive electrode active material layer non-formed portion 52a and the negative electrode active material layer non-formed portion 62a are joined to the positive electrode collector plate 42a and the negative electrode collector plate 44a, respectively. It should be noted that the positive electrode sheet 50 is an example of the "positive electrode" disclosed herein, and the negative electrode sheet 60 is an example of the "negative electrode" disclosed herein.
[0048] <Positive electrode>
[0049] The positive electrode (positive electrode sheet 50) disclosed herein includes a positive electrode active material layer 54. Figure 2As shown, the positive electrode (positive electrode sheet 50) includes a positive electrode collector 52 and a positive electrode active material layer 54 supported by the positive electrode collector 52. It should be noted that in this embodiment, the positive electrode active material layer 54 is illustrated only on one side of the positive electrode collector 52, but the positive electrode active material layer 54 may be provided on both sides of the positive electrode collector 52.
[0050] Figure 3 Schematic diagram showing the structure of a positive electrode active material 56 of one embodiment. The positive electrode active material layer 54 includes a positive electrode active material 56 capable of reversibly occluding and releasing charge carriers. The positive electrode active material 56 of this embodiment includes a lithium transition metal composite oxide 56a as a base material and a coating portion 56c disposed on at least a portion of the surface of the lithium transition metal composite oxide 56a. The coating portion 56c is typically disposed on the lithium transition metal composite oxide 56a by physical and / or chemical bonding.
[0051] The lithium transition metal composite oxide 56a of the present embodiment has a layered structure and contains lithium (Li), nickel (Ni) and manganese (Mn) as essential elements. The lithium transition metal composite oxide 56a of the present embodiment is a so-called high-Ni lithium transition metal composite oxide in which the content of Ni relative to metal elements other than Li is 75 mol% or more. It should be noted that the high-Ni lithium transition metal composite oxide is an example of the "lithium transition metal composite oxide in which the total content of Ni relative to metal elements other than Li is 75 mol% or more" disclosed herein.
[0052] The positive electrode active material may contain positive electrode active materials other than the lithium transition metal composite oxide 56a within a range that does not hinder the effects of the present disclosure (for example, less than 10% by mass, preferably less than 5% by mass relative to the total mass of the positive electrode active material). In addition, the positive electrode active material may also be composed only of the lithium transition metal composite oxide 56a.
[0053] From the viewpoint of high volume energy density of lithium ion secondary batteries, in the lithium transition metal composite oxide 56a, the content of Ni relative to the total of metal elements other than Li is preferably 80 mol% or more, and more preferably 90 mol% or more. On the other hand, from the viewpoint of high stability, the content of Ni relative to the total of metal elements other than Li is preferably 95 mol% or less, and more preferably 90 mol% or less.
[0054] As the lithium transition metal composite oxide 56a having a layered structure, for example, lithium nickel manganese composite oxides, lithium nickel cobalt manganese composite oxides, lithium nickel cobalt aluminum composite oxides, lithium iron nickel manganese composite oxides, etc. can be cited. One of them can be used alone, or two or more of them can be used in combination. The fact that the particles of the lithium transition metal composite oxide with a high Ni content have a layered structure (i.e., a layered crystal structure) can be confirmed by a known method (e.g., X-ray diffraction method, etc.).
[0055] It should be noted that in this specification, "lithium nickel cobalt manganese composite oxide" refers to a term that refers to an oxide containing one or more additional elements other than Li, Ni, Co, Mn, and O in addition to oxides containing these elements. Examples of the additional elements include transition metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, Sn, and typical metal elements. In addition, the additional elements may also be metalloid elements such as B, C, Si, and P, and non-metallic elements such as S, F, Cl, Br, and I. The same applies to the above-mentioned lithium nickel composite oxide, lithium cobalt composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.
[0056] In some preferred embodiments, the lithium transition metal composite oxide 56a preferably has a composition represented by the following general formula (i).
[0057] Li α Ni x Mn y M z O2···Formula (i)
[0058] In the above formula (i), x, y, z and α respectively satisfy 0.8≤α≤1.2, 0.75≤x≤0.95, 0.05≤y≤0.25, 0≤z≤0.2, and x+y+z=1. In the formula (i), M is at least one element selected from Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.
[0059] α in the above formula (i) preferably satisfies 0.9≤α≤1.2, and more preferably satisfies 1.0≤α≤1.1. From the viewpoint of battery characteristics (such as energy density, cycle characteristics, and thermal stability), x preferably satisfies 0.8≤x≤0.95, and more preferably satisfies 0.8≤x≤0.9. For example, from the viewpoint of energy density, thermal stability, and cost, y preferably satisfies 0.1≤y≤0.25, and more preferably satisfies 0.17≤y≤0.25. z preferably satisfies 0≤z≤0.1, and more preferably satisfies 0≤z≤0.03, and further preferably is 0. It should be noted that in the above formula (i), "x+y+z=1" includes the case where x+y+z is 1, and is substantially regarded as 1 as long as the technical effects disclosed herein can be achieved. Typically, it can be x+y+z=0.95~1.1, and preferably, it can be x+y+z=0.99~1.05.
[0060] In some preferred embodiments, the lithium transition metal composite oxide 56a preferably contains W. In other words, the lithium transition metal composite oxide 56a is preferably doped with W as an additive element. As a result, the layered structure of the lithium transition metal composite oxide 56a is stable, so in addition to better improving the initial resistance, the dissolution of Mn into the non-aqueous electrolyte is also suppressed, and the effect of suppressing the increase in resistance during storage is better obtained. In the case of doping (solid solution) W as an additive element in the lithium transition metal composite oxide 56a, it is preferably doped with 0.1 to 0.5 mol%, and more preferably doped with 0.1 to 0.3 mol%, relative to the total amount of transition metal elements of the lithium transition metal composite oxide 56a other than W.
[0061] The lithium transition metal composite oxide 56a preferably has a Co element content (mol) and a Mn element content (mol) in the following relationship:
[0062] 0≤Co / Mn≤0.42.
[0063] Thus, the content ratio of the Co element and the Mn element in the positive electrode active material can be well controlled. It should be noted that in the above relationship, the smaller the value of Co / Mn, the better it is possible to reduce the cobalt content in the lithium transition metal composite oxide 56a and suppress the increase in resistance during storage, so it is more preferably 0≤Co / Mn≤0.25, and even more preferably 0≤Co / Mn≤0.21.
[0064] In the lithium transition metal composite oxide used in the previous lithium ion secondary battery, the content ratio of the Co element relative to the metal element other than Li is typically about 10 mol% to 40 mol%. However, due to limited cobalt resources, it is preferred in this embodiment to reduce the Co content of the lithium transition metal composite oxide 56a compared to the past. Therefore, in some preferred embodiments, the content ratio of Co relative to the total of the metal elements other than Li is preferably, for example, 5 mol% or less, more preferably 3 mol% or less, and further preferably 0 mol% (i.e., no Co).
[0065] like Figure 3 As shown, the lithium transition metal composite oxide 56a is a secondary particle-like structure in which a plurality of primary particles 56p are typically aggregated by physical or chemical bonding forces. The number of primary particles 56p of the lithium transition metal composite oxide 56a constituting the secondary particles of the lithium transition metal composite oxide 56a is not particularly limited, and may be, for example, about 10 or more, preferably about 30 or more, and more preferably about 50 or more. The number of primary particles 56p is not particularly limited, and may be, for example, about 120 or less. It should be noted that, in this specification, "primary particle" refers to the smallest unit of particles constituting the positive electrode active material, specifically, refers to the smallest unit determined based on the geometric morphology of the appearance observed under an electron microscope. In addition, in this specification, a collection of more than 10 primary particles 56p is referred to as a "secondary particle".
[0066] In the present embodiment, the primary particle 56p adopts a so-called long strip shape with an aspect ratio (long diameter / short diameter ratio) of 1.9 or more. Thereby, the initial resistance is greatly improved. For the primary particle 56p of the present embodiment, typically, the long diameter extends approximately parallel to the direction (a-axis) orthogonal to the stacking direction (c-axis) of the layered lithium transition metal composite oxide. The primary particle 56p of the present embodiment typically forms a short diameter approximately parallel to the stacking direction (c-axis). The upper limit of the aspect ratio of the primary particle 56p is not particularly limited, for example, it is preferably less than 2.5, and more preferably less than 2.2.
[0067] It should be noted that in this specification, "the aspect ratio of the primary particle" means the major diameter / minor diameter ratio of the primary particle 56p constituting the lithium transition metal composite oxide 56a. The aspect ratio of the primary particle is grasped from the cross-sectional electron microscope image of the lithium transition metal composite oxide 56a, and refers to the average value of the major diameter / minor diameter ratio of a plurality of primary particles 56p selected at random. The plurality of primary particles 56p may be, for example, 20 or more. Specifically, the average particle size of the primary particle 56p can be obtained, for example, by the following operation, that is, a cross-sectional observation sample of the lithium transition metal composite oxide 56a is prepared by cross-sectional grinding, and then, a SEM image of the cross-sectional observation sample of the lithium transition metal composite oxide 56a is obtained using a scanning electron microscope (SEM), and then, an image analysis type particle size distribution measurement software (such as "Mac-View") is used to calculate the aspect ratio (ratio of the major diameter to the minor diameter) based on the major diameter and minor diameter of a plurality of primary particles 56p selected at random from the SEM image, and the arithmetic mean value thereof is obtained.
[0068] The average particle size of the primary particles 56p of the lithium transition metal composite oxide 56a is not particularly limited. For example, from the perspective of the high output characteristics and cycle characteristics of the positive electrode active material 56, the average particle size of the primary particles 56p of the lithium transition metal composite oxide 56a can be, for example, 0.1 μm to 2.5 μm, preferably 1.0 μm or more, more preferably 1.3 μm or more, and further preferably 1.9 μm or more. On the other hand, from the perspective of the higher output characteristics and cycle characteristics of the positive electrode active material 56, the average particle size of the primary particles 56p of the lithium transition metal composite oxide 56a is preferably 2.2 μm or less, more preferably 2.1 μm or less. It should be noted that "the average particle size of the primary particles of the lithium transition metal composite oxide" refers to the average particle size of the major diameter of the primary particles 56p of the lithium transition metal composite oxide 56a. The aspect ratio can be obtained by calculating the major diameters of a plurality of primary particles 56p selected arbitrarily from the SEM image and calculating the average value thereof in the same manner as the aspect ratio of the primary particles described above.
[0069] like Figure 3 As shown, the primary particle 56p of this embodiment is typically arranged in the lithium transition metal composite oxide 56a (secondary particle) to extend from the center C to the outer diameter OL (in a radial orientation). One end of the long side of the primary particle 56p is arranged on the outer diameter OL side, and the other end is arranged on the center C side. In other words, the a-axis of the primary particle 56p is arranged to extend from the center C to the outer diameter OL.
[0070] The primary particles 56p and secondary particles of the present embodiment can be manufactured by a conventionally known method (e.g., crystallization method, etc.). Although not particularly limited, the above-mentioned method for forming the primary particles 56p and secondary particles can be manufactured, for example, by a conventionally known crystallization method. First, a precursor of a lithium transition metal composite oxide in which the primary particles are radially oriented, i.e., a hydroxide, is prepared. The hydroxide generally contains a metal element other than lithium among the metal elements contained in the lithium transition metal composite oxide. When generating the hydroxide, a compound containing ammonium ions (e.g., ammonia) is used as an alkaline compound. At this time, by adjusting the pH, NH3 concentration, and reaction time, the aspect ratio (the major and minor diameters of the primary particles 56p) and the configuration of the primary particles 56p can be controlled. The NH3 concentration in the reaction solution is preferably less than 2wt%, for example, 1 to 2wt%. The pH in the reaction solution is preferably approximately 10.5 to 12. The reaction time is preferably approximately 20 to 40 hours. Then, the obtained hydroxide is mixed with a compound that serves as a lithium source (e.g., lithium hydroxide, etc.) and fired. At this time, by adjusting the firing temperature and firing time during firing, the morphology of the secondary particles of the lithium transition metal composite oxide 56a can be well controlled. It should be noted that the firing temperature is not particularly limited, but can be, for example, 700°C to 800°C. In addition, the firing time is not particularly limited, but can be, for example, 10 hours to 20 hours. Thus, the following can be obtained: Figure 3 The illustrated elongated primary particles 56 p are radially oriented secondary particles of the lithium transition metal composite oxide 56 a of the present embodiment.
[0071] like Figure 3As shown, in some preferred embodiments, a coating portion 56c can be configured on at least a portion of the surface of the lithium transition metal composite oxide 56a. However, the coating portion 56c is not necessary and can be omitted in some embodiments. The coating portion 56c preferably contains a boron compound. By configuring a boron compound as a coating portion 56c on the surface of the lithium transition metal composite oxide 56a, the dissolution of Mn from the lithium transition metal composite oxide 56a to the non-aqueous electrolyte 80 can be suppressed, and the increase in resistance during storage can be suppressed. In addition, in the positive electrode active material 56, by having a coating portion 56c, the binding force between the primary particles 56p is improved. As a result, the stress during expansion and contraction can be alleviated, and the particle rupture of the lithium transition metal composite oxide 56a can be suppressed. From this point of view, the increase in resistance during storage can also be well suppressed. As the above-mentioned boron compound, for example, a boron-containing oxide or an oxide containing boron and lithium is preferably used, and lithium borate is particularly preferred. As a specific example of a boron compound, there can be LiBO2, LiB(OH)4, Li3BO3, B2O3, etc., and LiBO2 is particularly preferably used. The ratio of the boron compound in the coating portion 56 c may be, for example, 0.5 to 2.0 mol %, preferably 0.7 to 1.5 mol %, calculated as boron (B) with the total amount of metal elements other than Li in the positive electrode active material being 100 mol %.
[0072] In some preferred embodiments, in addition to the boron compound, the coating 56c may further include aluminum oxide (Al2O3). In detail, aluminum oxide has the function of capturing hydrogen fluoride gas (hydrofluoric acid) generated by the decomposition of the non-aqueous electrolyte 80. As a result, the dissolution of Mn into the non-aqueous electrolyte 80 caused by the reaction of the positive electrode active material 56 (lithium transition metal composite oxide 56a) with hydrogen fluoride gas can be suppressed. Therefore, by configuring a coating 56c that further includes aluminum oxide in addition to the boron compound on the surface, the increase in resistance during storage can be better suppressed. When converted to aluminum (Al) when the total amount of metal elements other than Li in the lithium transition metal composite oxide 56a is set to 100 mol%, the proportion of aluminum oxide as the coating 56c can be, for example, 0.1 to 0.5 mol%, preferably 0.3 to 0.5 mol%.
[0073] The coating portion 56c is preferably disposed at least on the surface of the secondary particle of the lithium transition metal composite oxide 56a. In this case, the coating portion 56c may cover the positive electrode active material 56 by 60% or more. It should be noted that the coating portion 56c is disposed on the surface of the secondary particle and the ratio (coverage) of the portion covered by the coating portion 56c can be confirmed, for example, by performing XPS (X-ray Photoelectron Spectroscopy) analysis on the positive electrode active material 56.
[0074] In the case where the lithium transition metal composite oxide 56a has voids, it is preferred that the coating portion 56c exists inside the secondary particle in addition to or instead of the surface of the secondary particle. Specifically, it is preferred that the coating portion 56c exists on the surface of the primary particle 56p inside the secondary particle. The amount of the coating portion 56c existing inside the secondary particle may be more or less than the amount of the coating portion 56c existing on the surface of the secondary particle. Thus, the technical effect disclosed herein can be exerted at a high level. It should be noted that the presence of the coating portion 56c inside the secondary particle can be confirmed by LA-ICP-MS (Laser Ablation Inductively Coupled Plasma Mass Spectrometry) analysis.
[0075] The average particle size (D50) of the lithium transition metal composite oxide 56a (secondary particles) is not particularly limited. From the perspective of particularly high filling property of the positive electrode active material layer 54 and high volume energy density of the lithium ion secondary battery 100, the average particle size (D50) of the lithium transition metal composite oxide 56a (secondary particles) is preferably 5 μm to 30 μm, and more preferably 10 μm to 20 μm.
[0076] It should be noted that in this specification, "the average particle size (D50) of the lithium transition metal composite oxide (secondary particles)" refers to the median particle size (D50), which refers to the particle size corresponding to 50% by volume of the cumulative frequency from the side of the particles with a small particle size in the volume-based particle size distribution based on the laser diffraction scattering method. Therefore, the average particle size (D50) of the lithium transition metal composite oxide (secondary particles) can be obtained using a laser diffraction scattering type particle size distribution measuring device or the like.
[0077] In the present embodiment, the lithium transition metal composite oxide 56a can be a so-called solid structure in which the primary particles 56p are simply aggregated to form secondary particles. However, it is not limited to this, and the lithium transition metal composite oxide 56a can have a gap inside the secondary particle from the gap between the aggregated primary particles 56p. It should be noted that the gap can be open or not. In the case of an opening of the gap, a gap can have more than two openings. The gap is located inside the imaginary outer diameter OL of the secondary particle in the cross-sectional view, and is typically a space surrounded by multiple primary particles 56p.
[0078] In the case where the lithium transition metal composite oxide 56a (secondary particle) has voids, the void ratio is preferably 2% to 10%. The void ratio of the secondary particle is, for example, 2% or more, and may be 3% or more or 5% or more. By making the void ratio of the secondary particle be above the specified value, the initial resistance of the lithium ion secondary battery 100 can be reduced. In addition, appropriate voids can be ensured inside the secondary particle of the lithium transition metal composite oxide 56a. In addition, in the case where the lithium transition metal composite oxide 56a has a coating 56c, the coating 56c can be arranged without omission to the center C of the secondary particle. On the other hand, if the void ratio of the secondary particle is too much (typically, the void ratio exceeds 10%), the resistance increase during storage increases. Therefore, the void ratio of the secondary particle is, for example, 10% or less, and may be 9% or less or 8% or less. It should be noted that in this specification, the "average void ratio of the lithium transition metal composite oxide" is grasped from the cross-sectional electron microscope image of the lithium transition metal composite oxide, and the average value can be calculated by measuring the void ratio of a plurality of secondary particles selected arbitrarily. The number of the plurality of secondary particles may be, for example, more than 20. First, a cross-sectional observation sample of the lithium transition metal composite oxide 56a is prepared by cross-sectional grinding or the like. Next, a scanning electron microscope (SEM: Scanning Electron Microscope) is used to obtain a SEM image of the cross-sectional observation sample. From the obtained SEM image, the area of the entire secondary particle and the total area of all voids inside the secondary particle are calculated using image analysis software (e.g., "ImageJ"). Then, the porosity is calculated using the formula (ii) shown below, and the average value is calculated.
[0079] Void ratio (%) = (total area of all voids / total area of secondary particles) × 100 (ii)
[0080] The porosity of the lithium transition metal composite oxide 56a can be adjusted, for example, by changing the synthesis conditions when synthesizing a hydroxide as a precursor of the lithium transition metal composite oxide 56a by a crystallization method. Specifically, in the crystallization method, a raw material aqueous solution containing a metal element other than lithium and a pH adjusting solution are added to the reaction solution to synthesize the hydroxide. By changing the pH value and stirring speed of the reaction solution at this time, the porosity of the hydroxide can be adjusted. By mixing and firing the hydroxide and a compound that becomes a lithium source (such as lithium hydroxide, etc.), a lithium transition metal composite oxide 56a in the form of secondary particles and with adjusted porosity can be obtained.
[0081] The BET specific surface area of the lithium transition metal composite oxide 56a is not particularly limited. From the viewpoint of providing the lithium ion secondary battery 100 with excellent output characteristics, the BET specific surface area of the lithium transition metal composite oxide 56a is preferably 0.50 m 2 / g~0.85m 2 / g, more preferably 0.55m 2 / g~0.80m 2 / g. The BET specific surface area of the lithium transition metal composite oxide 56a can be measured by a nitrogen adsorption method using a commercially available specific surface area measuring apparatus.
[0082] The content of the positive electrode active material 56 in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material 56 relative to the total mass of the positive electrode active material layer 54) is not particularly limited, and is, for example, 80 mass % or more, preferably 87 mass % or more, more preferably 90 mass % or more, further preferably 95 mass % or more, and most preferably 97 mass % or more.
[0083] The positive electrode current collector 52 may be a known material used in the lithium ion secondary battery 100, and examples thereof include a sheet or foil made of a metal having good conductivity (such as aluminum, nickel, titanium, stainless steel, etc.). The positive electrode current collector 52 of this embodiment is preferably an aluminum foil.
[0084] The size of the positive electrode current collector 52 is not particularly limited and can be appropriately determined according to the battery design. When aluminum foil is used as the positive electrode current collector 52, the thickness of the positive electrode current collector 52 is not particularly limited, and is, for example, 5 μm to 35 μm, preferably 7 μm to 20 μm.
[0085] <Negative electrode>
[0086] The negative electrode (negative electrode sheet 60) disclosed herein includes a negative electrode active material layer 64. Figure 2 As shown, the negative electrode (negative electrode sheet 60) includes a negative electrode collector 62 and a negative electrode active material layer 64 supported on the negative electrode collector 62. It should be noted that in this embodiment, the negative electrode active material layer 64 is illustrated only on one side of the negative electrode collector 62, but the negative electrode active material layer 64 may be provided on both sides of the negative electrode collector 62.
[0087] The negative electrode active material layer 64 contains a negative electrode active material 66 capable of reversibly occluding and releasing charge carriers. Figure 4 Schematic diagram showing the structure of a negative electrode sheet 60 (negative electrode) of one embodiment. The negative electrode active material 66 of this embodiment must include a carbon material 66c and a Si-containing material 66s. However, the negative electrode active material 66 may further include other negative electrode active materials in addition to the carbon material 66c and the Si-containing material 66s. In addition, for ease of explanation, although not shown here, the negative electrode active material layer 64 may include a conductive material, a binder, a thickener, etc. in addition to the negative electrode active material 66.
[0088] As the carbon material 66c, for example, graphite, hard carbon, soft carbon, etc. can be used, among which graphite can be preferably used. The graphite may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material.
[0089] The average particle size of the carbon material 66c is not particularly limited, and is, for example, 0.1 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 5 μm to 20 μm. The average particle size (D50) of the carbon material can be determined, for example, by a laser diffraction scattering method.
[0090] Examples of the Si-containing material 66s include silicon (Si), SiO x Silicon oxide represented by (0.05<x<1.95), Si-C composite containing Si particles in carbon particles, lithium silicate (Li x Si y O z ) and the like. The Si-containing material 66s can preferably use silicon, silicon oxide, or Si-C composite. In addition, the Si-containing material 66s can use an alloy composed of Si and elements other than Si. Examples of elements other than Si include Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn, and Ti. By including the Si-containing material 66s in the negative electrode active material 66, the formation of a coating layer starting from Mn dissolved from the positive electrode active material on the surface of the negative electrode active material layer 64 can be suppressed. Therefore, the increase in resistance during storage can be well suppressed.
[0091] The average particle size of the Si-containing material 66s is not particularly limited, and is, for example, 0.1 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 5 μm to 20 μm. The average particle size (D50) of the carbon material can be determined, for example, by a laser diffraction scattering method.
[0092] In the present embodiment, from the viewpoint of taking into account both the resistance increase suppression effect and the capacity retention rate during storage, the content ratio of the Si element in the negative electrode active material 66 is 5% to 10% by mass when the total amount of the negative electrode active material 66 is 100% by mass. When the content ratio of the Si element is small (typically less than 5% by mass), the effect of suppressing the formation of the film layer starting from Mn dissolved from the positive electrode active material on the surface of the negative electrode active material layer 64 cannot be well obtained, and the storage resistance suppression effect cannot be smoothly obtained. On the other hand, when the content ratio of the Si element is too high (typically more than 10% by mass), the capacity retention rate during storage decreases, so it is not preferred.
[0093] There is no particular limitation on the distribution of the Si-containing material 66s in the negative electrode active material layer 64. The Si-containing material may be dispersed throughout the negative electrode active material layer 64, concentrated in the upper layer of the negative electrode active material layer 64 (the surface side of the negative electrode active material layer 64), or concentrated in the lower layer of the negative electrode active material layer 64 (the negative electrode current collector 62 side). In some preferred embodiments, as described in the second embodiment ( Figure 5 ), the Si-containing material 66s is preferably dispersed in the upper layer of the negative electrode active material layer 64 (equivalent to Figure 5 The negative electrode upper layer 164u). Figure 4 As shown, in the present embodiment, the Si-containing material 66s is substantially uniformly dispersed throughout the negative electrode active material layer 64. It should be noted that "concentratedly dispersed in the upper layer of the negative electrode active material layer 64" is an example of "the content ratio of the Si element in the negative electrode upper layer is 90% by mass or more when the Si element in the entire negative electrode active material is 100% by mass" disclosed herein.
[0094] The negative electrode active material layer 64 may contain components other than the negative electrode active material 66, such as a conductive material, a binder, a thickener, etc. As the binder, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF) and other binders conventionally used in lithium secondary batteries may be used without particular limitation. As the thickener, for example, carboxymethyl cellulose (CMC) may be used.
[0095] The negative electrode active material layer 64 preferably further includes a conductive material. As a conductive material, for example, carbon black (CB) such as acetylene black (AB), ketjen black, carbon black (CB), carbon nanotubes (CNT), carbon fibers such as vapor-grown carbon fibers (VGCF), activated carbon, graphite and other carbon materials can be used well, among which CNT is preferably included. By including CNT as a conductive material, the capacity retention rate can be well maintained. As CNT, any one of single-layer carbon nanotubes (SWCNT), double-layer carbon nanotubes (DWCNT), and multi-layer carbon nanotubes (MWCNT) can be used, and they can be used alone or in combination of more than two. When using CNT as a conductive material for the negative electrode active material layer 64, SWCNT is preferably used. When CNT is used as a conductive material for the negative electrode active material layer 64, it is preferably included in an amount of 0.5% by mass or less of CNT relative to the entire negative electrode active material layer.
[0096] The content of the negative electrode active material 66 in the negative electrode active material layer 64 is preferably 90% by mass or more, and more preferably 95% by mass to 99% by mass. The content of the binder in the negative electrode active material layer 64 is preferably 0.1% by mass to 8% by mass, and more preferably 0.5% by mass to 3% by mass. The content of the thickener in the negative electrode active material layer 64 is preferably 0.3% by mass to 3% by mass, and more preferably 0.5% by mass to 2% by mass.
[0097] The thickness of the negative electrode active material layer 64 is not particularly limited, and is, for example, 10 μm to 200 μm, preferably 20 μm to 100 μm, when the negative electrode active material layer 64 is provided on only one surface of the negative electrode current collector 62. In addition, when the negative electrode active material layer 64 is provided on both surfaces of the negative electrode current collector 62, the thickness of one surface (the thickness of each of one surface and the other surface) is, for example, 10 μm to 200 μm, preferably 20 μm to 100 μm.
[0098] A known negative electrode current collector used in lithium ion secondary batteries can be used as the negative electrode current collector 62 , and examples thereof include sheets or foils made of metals with good conductivity (such as copper, nickel, titanium, stainless steel, etc.). The negative electrode current collector 62 is preferably copper foil.
[0099] The size of the negative electrode current collector 62 is not particularly limited and can be appropriately determined according to the battery design. When copper foil is used as the negative electrode current collector 62, the thickness of the negative electrode current collector 62 is not particularly limited, and is, for example, 5 μm to 35 μm, preferably 7 μm to 20 μm.
[0100] As the separator 70, various porous sheets similar to those used in lithium-ion secondary batteries can be used, and examples thereof include porous resin sheets made of resins such as polyethylene (PE) and polypropylene (PP). The porous resin sheet can be a single-layer structure or a multi-layer structure of two or more layers (for example, a three-layer structure in which PP layers are stacked on both sides of a PE layer). The separator 70 can also have a heat-resistant layer (HRL).
[0101] As the non-aqueous electrolyte 80, the same non-aqueous electrolyte as that of the conventional lithium-ion secondary battery can be used, and typically a non-aqueous electrolyte containing a supporting salt in an organic solvent (non-aqueous solvent) can be used. As the non-aqueous solvent, aprotic solvents such as carbonates, esters, and ethers can be used. Among them, carbonates are preferred because the effect of reducing the low-temperature resistance of the positive electrode material becomes particularly high. Examples of carbonates include ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), trifluorodimethyl carbonate (TFDMC), etc. Such non-aqueous solvents can be used alone or in appropriate combinations of two or more. As a supporting salt, for example, lithium salts such as LiPF6, LiBF4, and lithium bis(fluorosulfonyl)imide (LiFSI) can be used well. The concentration of the supporting salt is preferably 0.7 mol / L to 1.3 mol / L.
[0102] It should be noted that, as long as the effects of the present disclosure are not significantly impaired, the non-aqueous electrolyte 80 may contain components other than the above-mentioned non-aqueous solvent and supporting salt, such as various additives such as a gas generator, a film former, a dispersant, and a thickener. As additives used in the non-aqueous electrolyte 80, for example, positive and negative electrode film formers such as vinylene carbonate (VC), fluoroethylene carbonate (FEC), and 1,3-propane sultone (PS); overcharge preventers such as biphenyl (BP), cyclohexylbenzene (CHB), tert-butylbenzene, and tert-amylbenzene, etc. can be cited. Among them, the non-aqueous electrolyte 80 preferably contains FEC. In the case where FEC is included as an additive in the non-aqueous electrolyte 80, it is preferred that FEC be included in a ratio of 20 vol% or less relative to the non-aqueous electrolyte 80.
[0103] The positive electrode active material of the lithium ion secondary battery 100 constructed as described above includes a lithium transition metal composite oxide as a high-Ni lithium transition metal composite oxide, and a positive electrode active material having a primary particle of the lithium transition metal composite oxide with an aspect ratio of 1.9 or more. In addition, the negative electrode active material of the lithium ion secondary battery 100 includes a negative electrode active material comprising a carbon material and a Si-containing material, and when the total amount of the negative electrode active material is set to 100% by mass, the content ratio of the Si element in the negative electrode active material is 5% to 10% by mass. Thus, although the cobalt content in the positive electrode active material is reduced, the increase in initial resistance can be suppressed, and the increase in resistance during storage can be suppressed.
[0104] In detail, the lithium transition metal composite oxide with a layered structure typically has a stacked structure in which a lithium layer, an oxygen layer, a transition metal layer, and an oxygen layer are repeatedly overlapped. The above-mentioned lithium transition metal composite oxide occludes and releases Li ions from a direction (a axis) orthogonal to the stacking direction (c axis). When a lithium transition metal composite oxide with a layered structure containing Mn is used as a positive electrode active material, if the Co content in the lithium transition metal composite oxide is reduced, the stability of the lithium transition metal composite oxide is reduced. Typically, the interlayer of the lithium transition metal composite oxide narrows, so the conductivity of the Li ion decreases, thereby increasing the initial resistance. In addition, due to the reduced stability of the lithium transition metal composite oxide, Mn dissolution from the positive electrode active material layer (specifically, the lithium transition metal composite oxide) becomes significant during storage. For example, Mn dissolved from the positive electrode active material layer is precipitated on the surface of the negative electrode active material layer (typically the graphite surface), and then a film growth starting from the precipitated Mn occurs. Due to the film, the durability of the lithium ion secondary battery deteriorates. Therefore, conventionally, lithium ion secondary batteries using a layered lithium transition metal composite oxide containing Mn and having a reduced Co content as a positive electrode active material have problems such as degradation of initial resistance and a large increase in resistance during storage.
[0105] In contrast, in the lithium ion secondary battery 100 of the present embodiment, in the lithium transition metal composite oxide 56a, the content of Ni relative to the total of metal elements other than Li is 75 mol% or more, so the Mn ratio in the lithium transition metal composite oxide 56a can be suppressed. Moreover, the primary particle 56p of the present embodiment has a strip shape with an aspect ratio of 1.9 or more. According to the primary particle 56p having this structure, in the lithium transition metal composite oxide 56a, a plurality of primary particles 56p are arranged in a manner such that the long diameter extends from the outer diameter OL to the center C, thereby constituting a secondary particle. An effective diffusion path of Li ions from the surface (outer diameter OL side) of the lithium transition metal composite oxide 56a to the center C is constituted, and the diffusion curve length is reduced. As a result, the Li ion diffusivity of the lithium transition metal composite oxide 56a is improved. Therefore, the initial resistance can be reduced. Furthermore, according to the Si-containing material 66s contained in the negative electrode active material 66, the precipitation of Mn on the surface of the negative electrode active material layer 64 is suppressed. As a result, the formation of a Mn film can be suppressed on the surface of the negative electrode active material layer 64. Therefore, even when the Co content in the lithium transition metal composite oxide is reduced, it is possible to provide a lithium ion secondary battery 100 in which an increase in initial resistance and an increase in resistance during storage are suppressed.
[0106] The lithium-ion secondary battery 100 can be used for various purposes. Suitable uses include a driving power source mounted on a vehicle such as an electric vehicle (BEV), a hybrid electric vehicle (HEV), and a plug-in hybrid electric vehicle (PHEV). In addition, the lithium-ion secondary battery 100 can be used as a storage battery for a small power storage device, etc. The lithium-ion secondary battery 100 can also be typically used in the form of a battery pack formed by connecting a plurality of batteries in series and / or in parallel.
[0107] It should be noted that, as an example, a square lithium-ion secondary battery 100 having an electrode body 20 with a winding structure having a flat shape is described. However, the lithium-ion secondary battery disclosed herein may also be configured as a lithium-ion secondary battery having a stacked electrode body (i.e., an electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked). The stacked electrode body may include a plurality of separators in a manner in which one separator is sandwiched between the positive electrode and the negative electrode, respectively, or the positive electrode and the negative electrode may be alternately stacked while folding one separator. In addition, the lithium-ion secondary battery of the present embodiment may also be constructed in the form of a cylindrical lithium-ion secondary battery, a coin-type lithium-ion secondary battery, a laminated lithium-ion secondary battery, and the like. Furthermore, an all-solid secondary battery in which the electrolyte is a solid electrolyte may also be constructed.
[0108] <Second embodiment>
[0109] Figure 5 The negative electrode sheet 160 (negative electrode) of the second embodiment is Figure 4 The corresponding figure. Figure 5 In the embodiment, the negative electrode active material layer 164 is provided in place of the negative electrode active material layer 64, and other than that, the above-mentioned lithium ion secondary battery 100 can be the same. Figure 5 As shown, the negative electrode active material layer 164 has a so-called multilayer structure including a negative electrode upper layer 164 u and a negative electrode lower layer 164 d .
[0110] In some preferred embodiments, when viewed from the thickness direction, the negative electrode active material layer 164 may include a negative electrode lower layer 164d in contact with the negative electrode current collector 62 and a negative electrode upper layer 164u further away from the negative electrode current collector 62 than the negative electrode lower layer 164d. However, the negative electrode active material layer 164 may also be a multilayer structure of three or more layers. For example, a layer having a different composition from the negative electrode upper layer 164u and the negative electrode lower layer 164d may be further formed between the negative electrode upper layer 164u and the negative electrode lower layer 164d.
[0111] The negative electrode upper layer 164u is a layer located on the surface side of the negative electrode lower layer 164d when viewed from the thickness direction of the negative electrode active material layer 164. The negative electrode upper layer 164u is located farther from the negative electrode collector 62 than the negative electrode lower layer 164d. The negative electrode upper layer 164u constitutes the outermost layer of the negative electrode active material layer 164. In other words, the negative electrode upper layer 164u is located on the positive electrode (positive electrode sheet 50) side than the negative electrode lower layer 164d.
[0112] The negative electrode active material 66 of the negative electrode upper layer 164u must contain a Si-containing material 66s. When the Si element content of the entire negative electrode active material layer 164 is set to 100 mass%, the content ratio of the Si element contained in the negative electrode upper layer 164u is preferably 90 mass% or more, more preferably 95 mass% or more, and further preferably 98 mass% or more. Typically, the content of the Si element contained in the negative electrode upper layer 164u is greater than the content of the Si element contained in the negative electrode lower layer 164d. In other words, in the negative electrode active material layer 164, the Si element is concentrated and dispersed on the positive electrode (positive electrode sheet 50) side.
[0113] As described above, Mn dissolved from the positive electrode active material layer 54 (typically, the lithium transition metal composite oxide 56a) precipitates from the positive electrode (positive electrode sheet 50) side of the negative electrode active material layer 64, in other words, the surface layer of the negative electrode active material layer 164, to form a film. Here, by adopting a structure in which the Si-containing material is concentratedly dispersed on the positive electrode (positive electrode sheet 50) side of the negative electrode active material layer 164, that is, on the negative electrode upper layer 164u side, the effect of suppressing the formation of a film of Mn on the surface of the negative electrode active material layer 164 is more effectively exhibited. Therefore, the increase in resistance during storage can be well suppressed.
[0114] It should be noted that the "content ratio (mass %) of the Si element contained in the negative electrode upper layer when the Si element amount of the entire negative electrode active material layer is set to 100%" in this specification can be calculated as follows. First, the thickness of the negative electrode upper layer is obtained by observing the cross-sectional SEM image of the negative electrode active material layer 164. Next, for a specified area of the negative electrode active material layer, the negative electrode active material layer of the thickness portion of the negative electrode upper layer obtained above is scraped to recover the sample, and an ICP (Inductively Coupled Plasma) analysis is performed to calculate the Si element amount in the negative electrode upper layer. Similarly for the negative electrode lower layer, the sample is recovered by scraping a specified area of the negative electrode active material layer, and the Si element amount in the negative electrode lower layer is calculated by ICP analysis. Then, based on the values of the Si element amount of the negative electrode upper layer and the negative electrode lower layer respectively obtained, the content ratio of the Si element in the negative electrode upper layer relative to the Si element amount of the entire negative electrode active material layer can be calculated.
[0115] When the total amount of the negative electrode active material 66 in the negative electrode upper layer 164 u is 100 mass %, the content of the Si element contained in the negative electrode upper layer 164 u is preferably 2 mass % or more, and more preferably 5 mass % or more.
[0116] The negative electrode lower layer 164d is a layer located closer to the negative electrode collector 62 than the negative electrode upper layer 164u when viewed in the thickness direction of the negative electrode active material layer 64. Here, the negative electrode lower layer 164d is in contact with the negative electrode collector 62.
[0117] The negative electrode active material 66 of the negative electrode lower layer 164d must contain the carbon material 66c. The negative electrode lower layer 164d may contain the Si-containing material 66s, or may not contain the Si-containing material 66s. The content of the Si element contained in the negative electrode lower layer 164d is not particularly limited. When the negative electrode active material of the negative electrode lower layer 164d is set to 100 mass%, it can be, for example, 2 mass% or less, preferably 1 mass% or less. The content of the C element contained in the negative electrode lower layer 164d is not particularly limited. When the negative electrode active material of the negative electrode lower layer 164d is set to 100 mass%, it is preferably 98 mass% or more, and more preferably 99 mass% or more.
[0118] The ratio (Tu / Ta) of the thickness Tu of the negative electrode upper layer 164u to the overall thickness Ta of the negative electrode active material layer 164 can be, for example, less than 0.8, preferably less than 0.7. Thus, the Si-containing material 66s (in other words, Si element) in the negative electrode active material layer 164 can be dispersed on the positive electrode (positive electrode sheet 50) side, thereby more effectively showing the effect of suppressing the formation of a film by Mn. Therefore, the increase in resistance during storage can be well suppressed. In addition, from the perspective of filling, the ratio of the thickness Tu of the negative electrode upper layer 164u to the overall thickness Ta of the negative electrode active material layer 164 can be, for example, more than 0.4, preferably more than 0.5. It should be noted that the "ratio of the thickness of the negative electrode upper layer to the overall thickness of the negative electrode active material layer" in the specification is measured in the cross-sectional SEM image of the negative electrode active material layer 164.
[0119] It should be noted that the negative electrode upper layer 164u and the negative electrode lower layer 164d described above can be made by a conventionally known method. Although not limited thereto, for example, a negative electrode active material layer forming slurry can be prepared using two or more negative electrode active materials 66 having different compositions (typically, the content ratio of the Si-containing material) and the negative electrode active material layer can be formed by applying the negative electrode active material layer forming slurry.
[0120] Hereinafter, examples according to the technology disclosed herein will be described, but the technology disclosed herein is not intended to be limited to the contents shown in the examples.
[0121] <Test Example 1: Study on the structure of positive electrode active material and the presence or absence of Si in negative electrode active material>
[0122] (Example 1)
[0123] [Production of positive electrode sheet]
[0124] First, prepare the positive electrode active material of Example 1. Specifically, a hydroxide as a precursor is generated by a crystallization method. At this time, a compound containing ammonium ions is used as an alkaline compound, the pH of the reaction solution is set to 11, the NH3 concentration is set to 1.0-1.5wt%, the reaction time is 40 hours, and a hydroxide is generated. Then, when the obtained hydroxide and the lithium source are mixed and fired, the firing temperature is set to 770°C and the firing time is set to 15 hours. Thus, a lithium transition metal composite oxide (Li1Ni2O3) with a layered structure having a secondary particle shape and a primary particle aspect ratio of 1.9 is obtained. 0.83 Mn 0.17 O2) (corresponding to 83 / 0 / 17 in the "Ni / Co / Mn" column of Table 1). The aspect ratio of the primary particles was measured by the above-mentioned method.
[0125] The prepared positive electrode active material, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder are mixed at a solid content mass ratio of positive electrode active material: AB: PVDF = 100: 1: 1. Add an appropriate amount of N-methyl-2-pyrrolidone (NMP) to the obtained mixture, knead it, and prepare a slurry for forming a positive electrode active material layer. The obtained slurry for forming a positive electrode active material layer is applied to both sides of a positive electrode collector made of aluminum foil with a thickness of 15 μm, and dried to form a positive electrode active material layer. After rolling the obtained positive electrode active material layer using a rolling roller, cut it into a specified size to produce the positive electrode sheet of Example 1.
[0126] [Production of negative electrode sheet]
[0127] First, the negative electrode active material of Example 1 was prepared by mixing graphite as a carbon material and Si-C composite as a Si-containing material so that the content of Si element was 10 mass % and the content of C element was 90 mass % when the total amount of the negative electrode active material was 100 mass %.
[0128] The negative electrode active material prepared above, styrene butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and single-layer carbon nanotubes (SWCNT) as a conductive material are mixed in ion exchange water at a solid content mass ratio of negative electrode active material: SBR: CMC: SWCNT = 100: 1: 1: 0.5 to prepare a slurry for forming a negative electrode active material layer. The obtained slurry for forming a negative electrode active material layer is applied to a negative electrode collector made of copper foil with a thickness of 10 μm, dried, and a negative electrode active material layer is formed. The obtained negative electrode active material layer is rolled using a rolling roller and then cut into a specified size. Thus, a negative electrode sheet of Example 1 in which the Si-containing material is roughly uniformly dispersed throughout the negative electrode active material is prepared.
[0129] [Preparation of spacers]
[0130] As a separator, a porous polyolefin sheet having a three-layer structure of PP / PE / PE and a thickness of 20 μm was prepared.
[0131] [Preparation of non-aqueous electrolyte]
[0132] As a non-aqueous electrolyte, a non-aqueous electrolyte was prepared in which LiPF6 as a supporting salt was dissolved at a concentration of 1 mol / L in a mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC) and fluoroethylene carbonate (FEC) in a volume ratio of EC:EMC:DMC:FEC=25:40:30:5.
[0133] [Preparation of lithium-ion secondary battery for evaluation]
[0134] The positive electrode sheet and the negative electrode sheet are overlapped in a manner of sandwiching a separator to obtain a laminate. Next, the laminate is wound to obtain a wound body, which is pressed into a flat shape to obtain a flat electrode body. A collector terminal is installed on the electrode body, which is inserted into a battery case and welded, and then a non-aqueous electrolyte is injected. Then, the battery case is sealed to produce a lithium ion secondary battery for evaluation.
[0135] [Initial charging process]
[0136] The obtained lithium ion secondary battery for evaluation of Example 1 was charged at a constant current of 0.1 C to a voltage of 4.2 V at a temperature of 25° C. as an initial charge treatment, and then charged at a constant voltage until the current value reached 1 / 20 C. Then, the battery was discharged at a constant current of 0.1 C to a voltage of 3.0 V.
[0137] (Example 2)
[0138] Used in Li1Ni 0.83 Mn 0.17 A lithium ion secondary battery for evaluation of Example 2 was prepared in the same manner as in Example 1 except that O 2 was doped with 0.3 mol % of W (tungsten) as a lithium transition metal composite oxide additive element, and an initial charge treatment was performed.
[0139] (Example 3)
[0140] The lithium ion secondary battery for evaluation of Example 3 was prepared and initially charged in the same manner as in Example 1 except that the aspect ratio of the primary particles of the lithium transition metal composite oxide was 1.5. The aspect ratio of the primary particles was adjusted by controlling the pH of the reaction solution, the NH3 concentration, and the reaction time during the precursor preparation.
[0141] (Example 4)
[0142] A lithium ion secondary battery for evaluation of Example 4 was prepared in the same manner as in Example 1 except that the negative electrode active material was graphite alone (ie, no Si-containing material was included), and an initial charge treatment was performed.
[0143] (Example 5)
[0144] A lithium ion secondary battery for evaluation of Example 5 was prepared in the same manner as in Example 1 except that the aspect ratio of the primary particles of the lithium transition metal composite oxide was 1.5 and that the negative electrode active material was only graphite (ie, not containing Si-containing material), and was subjected to initial charge treatment.
[0145] [Evaluation of initial resistance]
[0146] For the evaluation lithium-ion secondary batteries of Examples 1 to 5, first, in a constant temperature chamber at 25°C, each evaluation lithium-ion secondary battery was charged with a constant current constant voltage (CCCV) at a current value of 0.3C, and adjusted to a state of SOC (State of Charge) of 50%. Then, a 10-second pulse discharge was performed at a current value of 5C. The voltage change (ΔV) during the pulse discharge was obtained, and the resistance value (initial resistance value) before storage was calculated using the formula (I) shown below. The results are shown in Table 1.
[0147] Resistance value = voltage change (ΔV) / current value (5C)…(I)
[0148] [Evaluation of Storage Resistance Increase Rate]
[0149] After the initial resistance value was measured, the evaluation lithium ion secondary batteries of Examples 1 to 5 were adjusted to SOC 100% under a temperature environment of 25°C. Each evaluation lithium ion secondary battery was placed in a constant temperature layer at 60°C and stored for 14 days. Then, the resistance value after storage was calculated by the same method as the initial resistance. Then, the resistance increase rate (%) was calculated according to the formula (II) shown below. The results are shown in Table 1.
[0150] Resistance increase rate (%) = (resistance value after storage / resistance value before storage) × 100 (II)
[0151] [Capacity maintenance rate]
[0152] The evaluation of the capacity retention rate is carried out in parallel with the evaluation of the above-mentioned storage resistance increase rate. Specifically, for the evaluation lithium ion secondary batteries of Examples 1 to 5, the discharge capacity measured during the resistance increase rate evaluation is taken as the initial capacity. Then, the discharge capacity of the evaluation lithium ion secondary battery stored in the above-mentioned storage resistance increase rate evaluation (i.e., after being stored at 60°C for 14 days) is calculated by the same method as the initial capacity. Then, the capacity retention rate (%) of each example is calculated using the formula (III) shown below. The results are shown in Table 1.
[0153] Capacity retention rate (%) = discharge capacity after 14 days storage / initial capacity × 100…(III)
[0154] [Table 1]
[0155]
[0156] According to the results of Examples 1 and 5, in Example 1 in which the aspect ratio of the primary particles of the lithium transition metal composite oxide is 1.9 and the negative electrode active material containing carbon material and Si-containing material is used, the reduction of the initial resistance and the increase of the resistance during storage are well observed compared with Example 5. On the other hand, in Example 3 in which the aspect ratio of the primary particles of the lithium transition metal composite oxide is 1.5, the reduction of the initial resistance is not observed compared with Example 1. It is thus believed that by using a lithium transition metal composite oxide having an aspect ratio of more than 1.9 of the primary particles, the effect of reducing the initial resistance can be obtained. In addition, in Example 4 in which the negative electrode active material is only graphite (i.e., not containing Si-containing material), the reduction of the resistance increase rate during storage is not observed compared with Example 1. It can be seen that by satisfying the aspect ratio of the primary particles of the lithium transition metal composite oxide being more than 1.9 and using the negative electrode active material containing carbon material and Si-containing material, the inhibitory effect of the increase of the resistance during storage can be well obtained.
[0157] In addition, in Example 2, in which W is doped as an additive element in the lithium transition metal composite oxide in addition to the composition of Example 1, better results were obtained in terms of suppressing the initial resistance and the resistance increase during storage. As a reason for this, it is believed that the layered structure of the lithium transition metal composite oxide is stabilized by doping W, thereby further improving the conductivity of Li ions and suppressing the dissolution of Mn into the non-aqueous electrolyte.
[0158] <Test Example 2: Study of Si Ratio>
[0159] (Examples 6~8)
[0160] Except that the content ratio of the Si element when the total amount of the negative electrode active material is set to 100 mass % is changed as shown in the "Si content ratio" column of Table 2, the evaluation lithium ion secondary batteries of Examples 6 to 8 are prepared in the same manner as in Example 1 and the initial charging treatment is performed. The evaluation lithium ion secondary batteries of Examples 6 to 8 are evaluated in the same manner as in Test Example 1 by the above method. The results are shown in Table 2.
[0161] [Table 2]
[0162]
[0163] As shown in the results of Table 2, for Example 7 and Example 1 in which the content ratio of Si element in the negative electrode active material is 5% by mass or 10% by mass, the resistance increase during storage is well suppressed, and no decrease in capacity retention rate is observed. In Example 6 in which the content ratio of Si element is 2% by mass, the effect of suppressing the increase in resistance during storage is not very good. As a reason for this, it is believed that in Example 6, the negative electrode does not contain Si-containing materials that can fully suppress the precipitation of Mn on the surface of the negative electrode active material. In addition, the higher the content ratio of Si element, the better the effect of suppressing the increase in battery resistance is shown. On the other hand, in Example 8 in which the content ratio of Si element is 13% by mass, it is observed that the capacity retention rate is lower than that of other examples. Therefore, from the viewpoint of taking into account both the resistance increase suppression effect during storage and the capacity retention rate, it is believed that the content ratio of Si element in the negative electrode active material is 5 to 10% by mass, which is a more suitable range.
[0164] <Test Example 3: Study on the Aspect Ratio of Primary Particles>
[0165] (Examples 9~10)
[0166] The aspect ratio of the primary particles of the lithium transition metal composite oxide is set as shown in the "Aspect Ratio of Primary Particles" of Table 3. In addition, the lithium ion secondary batteries for evaluation of Examples 9 to 10 are prepared in the same manner as in Example 1 and subjected to initial charging treatment. It should be noted that the aspect ratio of the primary particles is adjusted by controlling the pH, NH3 concentration, and reaction time of the reaction solution during precursor preparation. In addition, the aspect ratio of the primary particles is determined by the above method. For the lithium ion secondary batteries for evaluation of Examples 9 to 10, the same evaluation as in Test Example 1 is implemented by the above method. The results are shown in Table 3.
[0167] [Table 3]
[0168]
[0169] According to the results of Table 3, compared with Example 3 in which the aspect ratio of the primary particles of the lithium transition metal composite oxide is 1.5, in Examples 1, 9 and 10 in which the aspect ratio of the primary particles is 1.9 or more, good results were obtained for the initial resistance for any of the examples. As a reason for this, it is believed that by making the aspect ratio 1.9 or more, an effective diffusion path of Li ions is formed in the secondary particle form, and the diffusion curve length is reduced, thereby improving the Li ion diffusivity of the lithium transition metal composite oxide 56a. In addition, according to the results of Examples 1, 9 and 10, it was observed that the larger the aspect ratio of the primary particles, the better the initial resistance.
[0170] <Test Example 4: Study of Covering Part>
[0171] (Example 11)
[0172] A lithium transition metal composite oxide having the same composition as in Example 1 is used, and a positive electrode active material of LiBO2 having a boron conversion ratio of 100 mol % relative to the total amount of metal elements other than Li in the lithium transition metal composite oxide is configured on the surface of the lithium transition metal composite oxide. In addition, a lithium ion secondary battery for evaluation of Example 11 is prepared in the same manner as in Example 1 and an initial charging treatment is performed.
[0173] (Example 12)
[0174] A lithium ion secondary battery for evaluation of Example 12 was prepared in the same manner as Example 1 except that a positive electrode active material having LiBO2 and Al2O3 as a coating portion was arranged on the surface of the lithium transition metal composite oxide, and an initial charge treatment was performed. It should be noted that the ratio of LiBO2 and Al2O3 was converted to Li and Al, respectively, and the molar ratio of LiBO2:Al2O3 = 1:0.5 was set to 100 mol% relative to the total amount of metal elements other than Li in the lithium transition metal composite oxide.
[0175] The lithium ion secondary batteries for evaluation of Examples 11 and 12 were evaluated in the same manner as in Test Example 1 by the above-mentioned method.
[0176] [Table 4]
[0177]
[0178] As shown in the results of Table 4, in Example 11 in which LiBO2 is configured as a coating portion on the surface of the lithium transition metal composite oxide, better results were obtained in terms of suppressing the increase in resistance during storage. In addition, in Example 12 in which Al2O3 is also contained as a coating portion in addition to LiBO2, further good results were obtained in terms of suppressing the increase in resistance during storage. As a reason for this, it is believed that the boron compound has the following effects: by being configured on the surface of the lithium transition metal composite oxide, the reaction area between the non-aqueous electrolyte and the lithium transition metal composite oxide is suppressed, and the dissolution of Mn is suppressed. In addition, aluminum oxide has the effect of capturing hydrogen fluoride gas generated by the decomposition of the non-aqueous electrolyte. Therefore, it is believed that in Examples 11 and 12, better results were obtained in terms of suppressing the increase in resistance during storage.
[0179] <Test Example 5: Study on Ni Mixing Ratio in Positive Electrode Active Material>
[0180] (Examples 13~19)
[0181] Except that the composition (molar ratio) of Ni, Co and Mn in the lithium transition metal composite oxide was changed as shown in the "Ni / Co / Mn" column of Table 5, the lithium ion secondary batteries for evaluation of Examples 13 to 19 were prepared in the same manner as in Example 1, and the initial charging treatment was performed. It should be noted that the molar ratio (Li / (Ni+Co+Mn)) of Li to the total of the transition metal elements (Ni+Co+Mn) in the lithium transition metal composite oxides of Examples 13 to 19 was 1.0 mol%. The lithium ion secondary batteries for evaluation of Examples 13 to 19 were evaluated in the same manner as in Test Example 1 by the above method. The results are shown in Table 5.
[0182] [Table 5]
[0183]
[0184] As shown in the results of Table 5, in Example 1 and Examples 13 to 15 in which the Ni ratio of the lithium transition metal composite oxide is 83 mol%, even when the Co content of the lithium transition metal composite oxide is reduced, the resistance suppression effect and the capacity maintenance rate during storage are stably taken into account. In addition, for Examples 16 to 17 in which the Ni ratio of the lithium transition metal composite oxide is 95 mol% and Examples 18 to 19 in which the Ni ratio of the lithium transition metal composite oxide is 75 mol%, the resistance suppression effect and the capacity maintenance rate during storage are also observed to be taken into account. In addition, when observing the Co / Mn ratio of the lithium transition metal composite oxide, for Example 15 in which the Co / Mn ratio is 0.42, the resistance suppression effect and the capacity maintenance rate during storage are also well taken into account.
[0185] <Test Example 6: Study on the Distribution of Si-Containing Material in Negative Electrode Active Material Layer>
[0186] (Examples 20~21)
[0187] A slurry for forming a first negative electrode active material layer was prepared in the same manner as in Example 1 except that the negative electrode active material was made to be only graphite (i.e., the content of Si element was 0 mass% and the content of C element was 100 mass% when the total amount of the negative electrode active material was set to 100 mass%).
[0188] Similarly, a second negative electrode active material layer forming slurry was prepared in the same manner as in Example 1 except that the content of Si element in graphite and Si—C composite was 20 mass % and 80 mass % respectively, based on 100 mass % of the total amount of the negative electrode active material.
[0189] The first negative electrode active material layer forming slurry is applied to the negative electrode collector made of copper foil which is the same as the negative electrode collector used in Example 1, dried, and rolled using a rolling roller in a manner to obtain a specified density. Next, the second negative electrode active material layer forming slurry is applied to the dried coating film of the first negative electrode active material layer forming slurry, dried, and rolled using a rolling roller in a manner to obtain a specified density. At this time, the thickness of the second negative electrode active material layer forming slurry is 0.5 relative to the overall thickness of the negative electrode active material layer. Thus, a negative electrode sheet of Example 20 is obtained, in which a negative electrode lower layer formed by the first negative electrode active material layer forming slurry and a negative electrode upper layer formed by the second negative electrode active material layer forming slurry are supported on the negative electrode collector. It should be noted that in the negative electrode sheet of Example 20, the content ratio of the Si element in the negative electrode upper layer when the Si element of the entire negative electrode active material is set to 100% by mass is 99% by mass.
[0190] Similarly, a second negative electrode active material layer forming slurry is applied to a negative electrode collector made of the same copper foil as the negative electrode collector used in Example 1, dried, and rolled using a rolling roller in a manner to obtain a specified density. Next, a first negative electrode active material layer forming slurry is applied to the dried coating of the second negative electrode active material layer forming slurry, dried, and rolled using a rolling roller in a manner to obtain a specified density. At this time, the thickness of the first negative electrode active material layer forming slurry is 0.5 relative to the overall thickness of the negative electrode active material layer. Thus, a negative electrode sheet of Example 21 is obtained, in which a negative electrode lower layer formed by a second negative electrode active material layer forming slurry and a negative electrode upper layer formed by a first negative electrode active material layer forming slurry are supported on the negative electrode collector. It should be noted that in the negative electrode sheet of Example 21, the content ratio of the Si element in the negative electrode upper layer when the Si element of the entire negative electrode active material is set to 100% by mass is 1% by mass.
[0191] The evaluation batteries of Examples 20 and 21 were prepared in the same manner as in Example 1 except that the negative electrode sheet was used, and the initial charge treatment was performed. The evaluation lithium ion secondary batteries of Examples 20 and 21 were evaluated in the same manner as in Test Example 1 by the above method. The results are shown in Table 6.
[0192] [Table 6]
[0193]
[0194] As shown in the results of Table 6, Examples 1, 20 and 21 all observed an effect of suppressing the increase in resistance during storage compared to Example 4 in which only graphite was used as the negative electrode active material. In Examples 1, 20 and 21 in which the Si ratio was 10% by mass, almost no difference was observed in the capacity retention rate during storage caused by the distribution of the Si-containing material. In addition, comparing Examples 1, 20 and 21, in Example 1 in which the Si-C composite was uniformly dispersed throughout the negative electrode active material layer, the effect of suppressing the increase in resistance during storage was good, and in Example 20 in which the Si-containing material was concentrated in the upper layer, further good results were obtained in suppressing the increase in resistance during storage. It is believed that this is because by concentrating the Si-containing material in the upper layer of the negative electrode active material, the effect of the Si-containing material in suppressing the precipitation of Mn is more effectively manifested on the surface of the negative electrode active material.
[0195] The preferred embodiment of the present disclosure has been described above, but the above embodiment is only an example. The present disclosure can be implemented in various other forms. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the scope of the claim includes the technology obtained by various deformations and changes to the above-mentioned exemplified embodiments. For example, part of the above-mentioned embodiment can be replaced by other variations, and other variations can be added to the above-mentioned embodiment. In addition, if the technical feature is not described as a necessary feature, it can also be deleted appropriately.
[0196] As described above, specific aspects of the technology disclosed herein include the following items.
[0197] Item 1: A lithium-ion secondary battery, comprising a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte, the positive electrode comprising a positive electrode active material layer containing a positive electrode active material, the positive electrode active material comprising a lithium transition metal composite oxide having a layered structure containing Li, Ni and Mn, the lithium transition metal composite oxide being a secondary particle formed by aggregation of primary particles, the content of Ni relative to the total of metal elements other than Li being 75 mol% or more, the aspect ratio of the primary particles being 1.9 or more, the negative electrode comprising a negative electrode active material layer containing a negative electrode active material, the negative electrode active material comprising a carbon material and a Si-containing material, and when the total amount of the negative electrode active material is set to 100 mass %, the content ratio of the Si element in the negative electrode active material is 5 mass % to 10 mass %.
[0198] Item 2: The lithium-ion secondary battery according to Item 1, wherein the lithium transition metal composite oxide is represented by the following general formula: Li α Ni x Mn y M zO2 (it should be noted that 0.8≤α≤1.2, 0.75≤x≤0.95, 0.05≤y≤0.25, 0≤z≤0.2, x+y+z=1, and M is one or more selected from Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W).
[0199] Item 3: The lithium ion secondary battery according to Item 1 or 2, wherein in the lithium transition metal composite oxide, the content (mol) of the Co element and the content (mol) of the Mn element satisfy the following relationship: 0≤Co / Mn≤0.42.
[0200] Item 4: The lithium ion secondary battery according to any one of Items 1 to 3, wherein the lithium-transition metal composite oxide contains W.
[0201] Item 5: The lithium ion secondary battery according to any one of Items 1 to 4, wherein the aspect ratio of the primary particles is 2.5 or less.
[0202] Item 6: The lithium ion secondary battery according to any one of Items 1 to 5, further comprising a coating portion disposed on at least a portion of a surface of the lithium transition metal composite oxide, wherein the coating portion contains a boron compound.
[0203] Item 7: The lithium ion secondary battery according to Item 6, wherein the coating portion further comprises aluminum oxide.
[0204] Item 8: A lithium-ion secondary battery according to any one of Items 1 to 7, wherein the negative electrode further comprises a negative electrode collector, and when observed in the thickness direction, the negative electrode active material layer comprises a negative electrode lower layer in contact with the negative electrode collector and a negative electrode upper layer farther away from the negative electrode collector than the negative electrode lower layer, and when the Si element of the entire negative electrode active material is set to 100 mass %, the content ratio of the Si element in the negative electrode upper layer is greater than 90 mass %.
[0205] Item 9: The lithium ion secondary battery according to Item 8, wherein a ratio of a thickness of the negative electrode upper layer to a total thickness of the negative electrode active material layer is 0.4 to 0.8.
[0206] Item 10: The lithium ion secondary battery according to any one of Items 1 to 9, wherein the Si-containing material includes one or more selected from the group consisting of Si, silicon oxide, and a Si—C composite.
Claims
1. A lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte, The positive electrode comprises a positive electrode active material layer containing a positive electrode active material. The positive electrode active material comprises a lithium transition metal composite oxide having a layered structure containing Li, Ni and Mn. The lithium transition metal composite oxide is a secondary particle formed by aggregation of primary particles, the content of Ni relative to the total of metal elements other than Li is 75 mol % or more, and the aspect ratio of the primary particles is 1.9 or more, The negative electrode comprises a negative electrode active material layer containing a negative electrode active material. The negative electrode active material comprises a carbon material and a Si-containing material, When the total amount of the negative electrode active material is 100 mass %, the content ratio of the Si element in the negative electrode active material is 5 mass % to 10 mass %.
2. The lithium ion secondary battery according to claim 1, wherein The lithium transition metal composite oxide is represented by the following general formula: Li α Ni x Mr y M z O2 Among them, 0.8≤α≤1.2, 0.75≤x≤0.95, 0.05≤y≤0.25, 0≤z≤0.2, x+y+z=1, and M is one or more selected from Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.
3. The lithium ion secondary battery according to claim 1 or 2, wherein: In the lithium transition metal composite oxide, the content of the Co element and the content of the Mn element satisfy the following relationship, and the unit of the content is mole, 0≤Co / Mn≤0.
42.
4. The lithium ion secondary battery according to claim 1 or 2, wherein: The lithium transition metal composite oxide contains W.
5. The lithium ion secondary battery according to claim 1 or 2, wherein: The aspect ratio of the primary particles is 2.5 or less.
6. The lithium ion secondary battery according to claim 1 or 2, wherein: further comprising a coating portion disposed on at least a portion of the surface of the lithium transition metal composite oxide, The coating portion includes a boron compound.
7. The lithium ion secondary battery according to claim 6, wherein: The coating portion further includes aluminum oxide.
8. The lithium ion secondary battery according to claim 1 or 2, wherein: The negative electrode further comprises a negative electrode current collector, The negative electrode active material layer includes a negative electrode lower layer in contact with the negative electrode current collector and a negative electrode upper layer farther from the negative electrode current collector than the negative electrode lower layer when viewed in the thickness direction. The content ratio of the Si element in the negative electrode upper layer is 90 mass % or more when the Si element in the entire negative electrode active material is 100 mass %.
9. The lithium ion secondary battery according to claim 8, wherein: The ratio of the thickness of the negative electrode upper layer to the entire thickness of the negative electrode active material layer is 0.4 to 0.
8.