Novel flexible integrated all-gel zinc-air battery and preparation method thereof
By adopting flexible integrated fully gel structure and porous polyacrylic hydrogel electrodes in zinc-air batteries, the leakage and contact impedance problems of traditional zinc-air batteries during deformation are solved, achieving high performance and low cost zinc-air battery production, suitable for commercial applications.
Patent Information
- Application Number
- CN202410801955.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-01
AI Technical Summary
Traditional zinc-air batteries are prone to fluid leakage and contact impedance problems during repeated deformation, resulting in short circuits, and the production process is complex and costly, making it difficult to meet the requirements of daily life and commercial applications.
Using a new flexible integrated fully gel zinc-air battery, polyacrylic hydrogel is prepared by using acrylic monomers to form a porous structure by combining conductive materials and carbon materials. , through the interface dry crosslink connection, simplify the process flow and reduce costs.
It realizes high performance, good flexibility and low cost production of zinc-air batteries, avoids liquid leakage and contact impedance problems, improves the stability and safety of the batteries, and is suitable for large-scale production and application.
Abstract
Description
Technical Field
[0001] The invention relates to a novel flexible integrated full-gel zinc-air battery and a preparation method thereof. Background Art
[0002] Metal-air batteries are a new type of battery between fuel cells and lithium-ion batteries, and their theoretical energy density is several times that of current lithium-ion batteries and other batteries. Lithium-air batteries have a high theoretical specific energy (up to 5200 Wh kg-1), the highest value in the metal-air battery category, and the strongest potential. However, in contrast, lithium metal electrodes are too active, which is dangerous when used, and the cost is high. Therefore, zinc-air batteries can be used as an effective alternative to lithium-air batteries. Even though their theoretical specific energy is 1084Wh kg-1, which is lower than that of lithium-air batteries, it is still 4 times that of commercial lithium-ion batteries.
[0003] Moreover, with the growing market demand for portable smart electronic products and wearable devices, higher requirements are placed on the flexibility and output capacity of advanced energy storage and conversion technologies. Zinc-air batteries (ZAB) have the characteristics of high energy density, low cost, high safety and environmental friendliness, making them one of the most promising new energy sources. Traditional zinc-air battery materials include positive electrode, negative electrode, electrolyte, diaphragm, etc. The battery is not flexible enough, which will cause short circuit problems during repeated deformation. Due to the characteristics of the electrolyte, there is a risk of leakage, and contact impedance will be formed between the positive electrode, negative electrode and diaphragm interfaces. These factors will affect the quality of zinc-air batteries.
[0004] In the existing technology, hydrogel technology has been proposed to solve the leakage and impedance problems. However, the battery performance and flexibility are different according to the different hydrogel monomers and preparation processes. Moreover, it is only in the research stage and has not been put into mass production and applied to daily life and the corresponding battery field. It can be seen that its performance, effect, operation process and cost have not met the requirements of practical application and need further improvement. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention aims to ensure the product quality of zinc-air batteries and provide a new flexible integrated all-gel zinc-air battery. After solving the problems of leakage and contact impedance between interfaces, the battery has good flexibility and avoids traditional problems such as short circuit caused by deformation. At the same time, the battery has the advantages of high performance, simpler operation, lower cost, and can form a simple process flow for production.
[0006] In order to achieve the above objectives, this experiment adopts the following technical solutions: A novel flexible integrated full-gel zinc-air battery, the battery comprises three parts: a hydrogel electrolyte, a hydrogel electrode and a zinc sheet. The hydrogel electrode and the zinc sheet are located on both sides of the hydrogel electrolyte to form a three-layer structure. The hydrogel electrolyte and the hydrogel electrode are connected to form a full gel, which is assembled and pressed in sequence with the zinc sheet. The raw materials for preparing the hydrogel electrolyte and the hydrogel electrode include acrylic acid monomers.
[0007] The hydrogel electrode and the hydrogel electrolyte are connected together through interfacial dry cross-linking.
[0008] A method for preparing the novel flexible integrated all-gel zinc-air battery comprises the following steps: Step 1: Acrylic acid, deionized water, sodium hydroxide, a crosslinking agent, and an initiator are mixed in a mass ratio of 1: (1-1.5): (0.4-0.6): (0.0005-0.0015): (0.005-0.010), and free radical polymerization is performed to obtain a polyacrylic acid hydrogel. The dried polyacrylic acid hydrogel is immersed in an alkaline solution to obtain a hydrogel electrolyte; Step 2: Acrylic acid, deionized water, one of (conductive polymer, carbon material, metal nanoparticles), pore-forming agent, binder, cross-linking agent, and initiator are mixed in a mass ratio of 1: (1-1.5): (0.03-0.05): (0.14-0.17): (0.03-0.05): (0.0005-0.0015): (0.005-0.010), and free radical polymerization is performed to obtain a porous polyacrylic acid / conductive material hydrogel. After dehydration, a platinum-carbon catalyst is dripped onto the surface of the conductive hydrogel and dried again to obtain a hydrogel electrode.
[0009] The crosslinking agent is one of N,N'-methylene acrylamide, N,N'-methylene bis acrylamide, divinyl benzene, diisocyanate, polyethylene glycol diacrylate and formaldehyde.
[0010] The initiator is one of potassium persulfate, ammonium persulfate, sodium bisulfite, ferrous sulfate and hydrogen peroxide.
[0011] In step 2, the conductive polymer is polypyrrole, polyaniline, polythiophene, polyacetylene, polyoxyethanol, poly(3,4-ethylenedioxythiophene); the carbon material is graphite, carbon fiber, carbon nanotube, graphene, conductive carbon black, nanographene, graphite powder; the metal nanoparticles are nickel nanoparticles, gold nanoparticles, silver nanoparticles.
[0012] The binder is carboxymethyl cellulose or sodium carboxymethyl cellulose; the pore-forming agent is one of polyethylene glycol-600, polyethylene glycol-1000 and polyethylene glycol-2000.
[0013] The hydrogel electrolyte immersion time is 48h. The alkaline solution is prepared by KOH and (CH3COO)2Zn in a molar ratio of 30:1.
[0014] Compared with the prior art, the present invention has the following beneficial effects: The preparation method of this invention uses acrylic acid monomer as a raw material to prepare hydrogel electrolyte and hydrogel electrode. Compared with the existing technology of making full gel battery with acrylamide as the matrix, polyacrylic acid hydrogel has the following advantages: Polyacrylic acid hydrogel contains a large number of carboxyl groups. Compared with other polymer hydrogels, polyacrylic acid hydrogel has strong hydrophilicity and can absorb a large amount of water. The immersion time in alkaline electrolyte is also greatly shortened.
[0015] Polyacrylic acid has excellent acid and alkali resistance and exhibits good stability when immersed in alkaline or acidic solutions, making the properties of its hydrogel electrolyte diverse.
[0016] Polyacrylic acid hydrogel is very sensitive to changes in temperature and pH. By adjusting these factors, a high-performance flexible integrated all-gel zinc-air battery can be prepared.
[0017] Acrylic acid is cheap and can save a lot of costs in the production process compared to acrylamide; at the same time, the process flow of this experiment is simple and the production is convenient, which is conducive to large-scale production and application, and has a high cost-effectiveness in the field of zinc-air batteries. DETAILED DESCRIPTION
[0018] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0019] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0020] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0021] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0022] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0023] The invention provides a method for preparing a novel flexible integrated all-gel zinc-air battery.
[0024] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0025] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0026] The present invention discloses a preparation method of a novel flexible integrated all-gel zinc-air battery, and the specific steps are as follows; Step 1: Dissolve NaOH in water and neutralize with acrylic acid in a water bath with constant temperature stirring. Slowly add crosslinker and initiator during stirring, stir for 30 minutes, pour into a mold with a diameter of 1 cm, put into a 60°C oven for drying, and soak the dried hydrogel in an alkaline solution to obtain a hydrogel electrolyte. Add deionized water, conductive polymer or carbon material to acrylic acid, stir at a constant temperature for 10 minutes to obtain a dispersion, slowly add binder and pore-forming agent to the dispersion, stir for 20 minutes, slowly add crosslinker and initiator, stir for 20 minutes, pour into a mold with a diameter of 1 cm, put into a 60°C oven for drying, obtain a porous polyacrylic acid / conductive material hydrogel, drop platinum carbon catalyst on the surface of the hydrogel and dry it to obtain a hydrogel electrode.
[0027] Step 2: The hydrogel electrode and the zinc sheet are located on both sides of the hydrogel electrolyte to form a three-layer structure. The hydrogel electrolyte and the hydrogel electrode are connected to form a full gel, which is assembled and pressed with the zinc sheet in sequence to obtain a new flexible integrated full gel zinc-air battery.
[0028] As a further improvement of the present invention, the mass ratio of the acrylic acid, deionized water, conductive polymer or carbon material, pore-forming agent, binder, cross-linking agent and initiator is 1: (1-1.5): (0.03-0.05): (0.14-0.17): (0.03-0.05): (0.0005-0.0015): (0.005-0.010).
[0029] As a further improvement of the present invention, the crosslinking agent is one of N,N'-methylene acrylamide, N,N'-methylene bis acrylamide, divinyl benzene, diisocyanate, polyethylene glycol diacrylate, and formaldehyde. The initiator is one of potassium persulfate, ammonium persulfate, sodium bisulfite, ferrous sulfate, and hydrogen peroxide.
[0030] As a further improvement of the present invention, in step 2, the conductive polymer, carbon material, and metal nanoparticles are polypyrrole, polyaniline, polythiophene, polyacetylene, polyoxyethanol, poly(3,4-ethylenedioxythiophene), graphite, carbon fiber, carbon nanotubes, graphene, conductive carbon black, nanographene, graphite powder, nickel nanoparticles, gold nanoparticles, and silver nanoparticles; the binder is carboxymethyl cellulose or sodium carboxymethyl cellulose; and the pore-forming agent is one of polyethylene glycol-600, polyethylene glycol-1000, and polyethylene glycol-2000.
[0031] As a further improvement of the present invention, the hydrogel electrolyte immersion time is 48h. As a further improvement of the present invention, the alkaline solution is prepared by KOH and (CH3COO)2Zn in a molar ratio of 30:1.
[0032] Example 1 (1) Take 0.8g NaOH and dissolve it in 2g deionized water at a constant temperature. Pour the NaOH solution into 2g acrylic acid for neutralization. Under the action of magnetic stirring, slowly add 0.001g N,N'-methylenebisacrylamide and 0.010g potassium persulfate. Stir for 30min. Pour the mixed solution into a mold with a diameter of 1cm and put it in an oven for drying. Then soak the dried hydrogel in 6M KOH+0.2M (CH3COO)2Zn solution for 48h to obtain a hydrogel electrolyte.
[0033] (2) Take 2 g of acrylic acid and stir at a constant temperature, slowly add 2 g of deionized water and 0.06 g of carbon nanotubes and stir for 10 minutes to obtain a dispersion, slowly add 0.28 g of polyethylene glycol-1000 and 0.06 g of carboxymethyl cellulose to the dispersion, stir for 20 minutes, then slowly add 0.001 g of N,N'-methylenebisacrylamide and 0.010 g of potassium persulfate and stir for 20 minutes. Pour the mixed solution into a mold with a diameter of 1 cm and put it in an oven to dry to obtain a porous polyacrylic acid / conductive material hydrogel, drop a platinum-carbon catalyst on the surface of the hydrogel and dry it to obtain a hydrogel electrode.
[0034] (3) The hydrogel electrode and the zinc sheet are located on both sides of the hydrogel electrolyte to form a three-layer structure. The hydrogel electrolyte and the hydrogel electrode interface are dry-crosslinked to form a full gel, which is then assembled and pressed with the zinc sheet in sequence to obtain a new flexible integrated full-gel zinc-air battery.
[0035] Example 2 (1) Take 1.5g NaOH and dissolve it in 4g deionized water at a constant temperature. Pour the NaOH solution into 3g acrylic acid for neutralization. Under the action of magnetic stirring, slowly add 0.003g N,N'-methylene acrylamide and 0.015g ammonium persulfate. Stir for 30min. Pour the mixed solution into a mold with a diameter of 1cm and put it in an oven for drying. Then soak the dried hydrogel in 6M KOH+0.2M (CH3COO)2Zn solution for 48h to obtain a hydrogel electrolyte.
[0036] (2) Take 3 g of acrylic acid and stir at a constant temperature, slowly add 4 g of deionized water and 0.1 g of poly(3,4-ethylenedioxythiophene) and stir for 10 minutes to obtain a dispersion, slowly add 0.45 g of polyethylene glycol-1000 and 0.1 g of sodium carboxymethyl cellulose to the dispersion, stir for 20 minutes, then slowly add 0.003 g of N,N'-methylene acrylamide and 0.015 g of ammonium persulfate and stir for 20 minutes. Pour the mixed solution into a mold with a diameter of 1 cm and put it in an oven to dry to obtain a porous polyacrylic acid / conductive material hydrogel, drop a platinum-carbon catalyst on the surface of the hydrogel and dry it to obtain a hydrogel electrode.
[0037] (3) The hydrogel electrode and the zinc sheet are located on both sides of the hydrogel electrolyte to form a three-layer structure. The hydrogel electrolyte and the hydrogel electrode interface are dry-crosslinked to form a full gel, which is then assembled and pressed with the zinc sheet in sequence to obtain a new flexible integrated full-gel zinc-air battery.
[0038] Example 3 (1) Take 2.5g NaOH and dissolve it in 7g deionized water at a constant temperature. Pour the NaOH solution into 5g acrylic acid for neutralization. Under the action of magnetic stirring, slowly add 0.005g polyethylene glycol diacrylate and 0.025g potassium persulfate. Stir for 30min. Pour the mixed solution into a mold with a diameter of 1cm and put it in an oven for drying. Then soak the dried hydrogel in 6M KOH+0.2M (CH3COO)2Zn solution for 48h to obtain a hydrogel electrolyte.
[0039] (2) Take 5 g of acrylic acid and stir at a constant temperature, slowly add 7 g of deionized water and 0.2 g of polypyrrole and stir for 10 minutes to obtain a dispersion, slowly add 0.75 g of polyethylene glycol-600 and 0.2 g of carboxymethyl cellulose to the dispersion, stir for 20 minutes, then slowly add 0.005 g of polyethylene glycol diacrylate and 0.025 g of potassium persulfate and stir for 20 minutes. Pour the mixed solution into a mold with a diameter of 1 cm and put it in an oven to dry to obtain a porous polyacrylic acid / conductive material hydrogel, drop a platinum-carbon catalyst on the surface of the hydrogel and dry it to obtain a hydrogel electrode.
[0040] (3) The hydrogel electrode and the zinc sheet are located on both sides of the hydrogel electrolyte to form a three-layer structure. The hydrogel electrolyte and the hydrogel electrode interface are dry-crosslinked to form a full gel, which is then assembled and pressed with the zinc sheet in sequence to obtain a new flexible integrated full-gel zinc-air battery.
[0041] Example 4 (1) Take 2.8g NaOH and dissolve it in 10.5g deionized water at a constant temperature. Pour the NaOH solution into 7g acrylic acid for neutralization. Under the action of magnetic stirring, slowly add 0.007g N,N'-methylenebisacrylamide and 0.035g ammonium persulfate. Stir for 30min. Pour the mixed solution into a mold with a diameter of 1cm and put it in an oven for drying. Then soak the dried hydrogel in 6M KOH+0.2M (CH3COO)2Zn solution for 48h to obtain a hydrogel electrolyte.
[0042] (2) Take 7 g of acrylic acid and stir at a constant temperature, slowly add 10.5 g of deionized water and 0.28 g of graphene and stir for 10 minutes to obtain a dispersion, slowly add 1.05 g of polyethylene glycol-1000 and 0.28 g of carboxymethyl cellulose to the dispersion, stir for 20 minutes, then slowly add 0.007 g of N,N'-methylenebisacrylamide and 0.035 g of ammonium persulfate and stir for 20 minutes. Pour the mixed solution into a mold with a diameter of 1 cm and put it in an oven to dry to obtain a porous polyacrylic acid / conductive material hydrogel, drop a platinum-carbon catalyst on the surface of the hydrogel and dry it to obtain a hydrogel electrode.
[0043] (3) The hydrogel electrode and the zinc sheet are located on both sides of the hydrogel electrolyte to form a three-layer structure. The hydrogel electrolyte and the hydrogel electrode interface are dry-crosslinked to form a full gel, which is then assembled and pressed with the zinc sheet in sequence to obtain a new flexible integrated full-gel zinc-air battery.
[0044] Example 5 (1) Take 5.4g NaOH and dissolve it in 13.5g deionized water at a constant temperature. Pour the NaOH solution into 9g acrylic acid for neutralization. Under the action of magnetic stirring, slowly add 0.0135g N,N'-methylenebisacrylamide and 0.09g ammonium persulfate. Stir for 30min. Pour the mixed solution into a mold with a diameter of 1cm and put it in an oven for drying. Then soak the dried hydrogel in 6M KOH+0.2M (CH3COO)2Zn solution for 48h to obtain a hydrogel electrolyte.
[0045] (2) Take 9 g of acrylic acid and stir at a constant temperature, slowly add 13.5 g of deionized water and 0.45 g of graphene and stir for 10 minutes to obtain a dispersion, slowly add 1.53 g of polyethylene glycol-1000 and 0.45 g of carboxymethyl cellulose to the dispersion, stir for 20 minutes, then slowly add 0.0135 g of N,N'-methylenebisacrylamide and 0.09 g of ammonium persulfate and stir for 20 minutes. Pour the mixed solution into a mold with a diameter of 1 cm and put it in an oven to dry to obtain a porous polyacrylic acid / conductive material hydrogel, drop a platinum-carbon catalyst on the surface of the hydrogel and dry it to obtain a hydrogel electrode.
[0046] (3) The hydrogel electrode and the zinc sheet are located on both sides of the hydrogel electrolyte to form a three-layer structure. The hydrogel electrolyte and the hydrogel electrode interface are dry-crosslinked to form a full gel, which is then assembled and pressed with the zinc sheet in sequence to obtain a new flexible integrated full-gel zinc-air battery.
[0047] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A new type of flexible integrated all-gel zinc-air battery, It is characterized in that The battery comprises three parts: a hydrogel electrolyte, a hydrogel electrode and a zinc sheet. The hydrogel electrode and the zinc sheet are located on both sides of the hydrogel electrolyte to form a three-layer structure. The hydrogel electrolyte and the hydrogel electrode are connected to form a full gel, which is assembled and pressed in sequence with the zinc sheet. The raw materials for preparing the hydrogel electrolyte and the hydrogel electrode include acrylic acid monomers.
2. A novel flexible integrated all-gel zinc-air battery according to claim 1, It is characterized in that The hydrogel electrode and the hydrogel electrolyte are connected together through interfacial dry cross-linking.
3. A method for preparing the novel flexible integrated all-gel zinc-air battery as claimed in claim 1, It is characterized in that The following steps are involved: Step 1: Acrylic acid, deionized water, sodium hydroxide, a crosslinking agent, and an initiator are mixed in a mass ratio of 1: (1-1.5): (0.4-0.6): (0.0005-0.0015): (0.005-0.010), and free radical polymerization is performed to obtain a polyacrylic acid hydrogel. The dried polyacrylic acid hydrogel is immersed in an alkaline solution to obtain a hydrogel electrolyte; Step 2: Acrylic acid, deionized water, one of (conductive polymer, carbon material, metal nanoparticles), pore-forming agent, binder, cross-linking agent, and initiator are mixed in a mass ratio of 1: (1-1.5): (0.03-0.05): (0.14-0.17): (0.03-0.05): (0.0005-0.0015): (0.005-0.010), and free radical polymerization is performed to obtain a porous polyacrylic acid / conductive material hydrogel. After dehydration, a platinum-carbon catalyst is dripped onto the surface of the conductive hydrogel and dried again to obtain a hydrogel electrode.
4. A method for preparing a novel flexible integrated all-gel zinc-air battery according to claim 3, It is characterized in that The crosslinking agent is one of N,N'-methylene acrylamide, N,N'-methylene bis acrylamide, divinyl benzene, diisocyanate, polyethylene glycol diacrylate and formaldehyde.
5. A method for preparing a novel flexible integrated all-gel zinc-air battery according to claim 3, It is characterized in that The initiator is one of potassium persulfate, ammonium persulfate, sodium bisulfite, ferrous sulfate and hydrogen peroxide.
6. A method for preparing a novel flexible integrated all-gel zinc-air battery according to claim 3, It is characterized in that In step 2, the conductive polymer is polypyrrole, polyaniline, polythiophene, polyacetylene, polyoxyethanol, poly(3,4-ethylenedioxythiophene); the carbon material is graphite, carbon fiber, carbon nanotube, graphene, conductive carbon black, nanographene, graphite powder; the metal nanoparticles are nickel nanoparticles, gold nanoparticles, silver nanoparticles.
7. A method for preparing a novel flexible integrated all-gel zinc-air battery according to claim 3, It is characterized in that The binder is carboxymethyl cellulose or sodium carboxymethyl cellulose; the pore-forming agent is one of polyethylene glycol-600, polyethylene glycol-1000 and polyethylene glycol-2000.
8. A method for preparing a novel flexible integrated all-gel zinc-air battery according to claim 3, It is characterized in that The hydrogel electrolyte immersion time is 48 hours.
9. The method for preparing a novel flexible integrated all-gel zinc-air battery according to claim 3, It is characterized in that The alkaline solution is KOH and (CH 3 COO 2 Zn is made in a molar ratio of 30:1.