Blade-coated perovskite solar cell and preparation method thereof
By depositing soil slope cylindrical dot array templates and three-stage coating technology on the scraper, the problems of uneven crystallization rate and spoiler in the preparation of perovskite solar cells are solved, and the charge transfer efficiency and stability are improved, so as to achieve Preparation of high-quality large-area films.
Patent Information
- Application Number
- CN202410936262.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The prior art In the preparation of large-area perovskite solar cells, there is uneven crystallization rate, spoiler of perovskite precursor and substrate during coating, resulting in uneven film formation and low charge transfer efficiency.
Using the scraper coating process, by depositing soil slope cylindrical dot array templates on the scraper, the spoiler phenomenon between the perovskite precursor and the substrate is reduced, the wetting property is improved, and the coating speed is adjusted through the three-stage coating process. , eliminate thickness differences and reduce wet film agglomeration.
The photoelectric conversion efficiency and stability of perovskite solar cells are significantly improved, the secondary agglomeration of the wet film is reduced, and the overall uniformity and crystallization uniformity of the film are improved.
Smart Images

Figure CN118890940A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optoelectronic functional devices, and in particular relates to a blade-coated perovskite solar cell and a preparation method thereof. Background Art
[0002] With the continuous development and innovation of photovoltaic devices and photovoltaic materials, perovskite solar cells, as a new solar energy technology, have become a strong competitor to traditional silicon cells with their advantages of high efficiency, easy preparation, and low cost, and have rapidly made remarkable progress. Small-area perovskite solar cells prepared by spin coating in the laboratory can achieve high photoelectric conversion efficiency. In industrial production, there are still deficiencies in the preparation process and coating of large-area perovskite solar cells, and there is a lot of room for improvement. The existing general coating equipment and coating process are difficult to meet the preparation of high-quality large-area perovskite films.
[0003] The present invention provides a scraper-coated perovskite solar cell and a preparation method thereof. Aiming at the preparation of a large-area high-quality perovskite film, the invention can well solve the disturbance phenomenon of the perovskite precursor solution and the substrate during the coating process, increase the contact area between the precursor solution and the substrate, reduce the contact angle between the scraper and the perovskite precursor solution, improve the coating speed, thereby improving the overall uniformity of the coating and the film-forming quality, reduce the agglomeration phenomenon of the perovskite wet film, improve the charge transfer efficiency, and thus improve the efficiency and stability of the perovskite solar cell as a whole. Summary of the invention
[0004] Technical issues solved:
[0005] The present application aims to solve the technical problems such as uneven crystallization rate caused by agglomeration in the large-area preparation of perovskites in the prior art, deficiencies in the preparation process and coating of large-area perovskite solar cells in industrial production, and turbulence between the perovskite precursor solution and the substrate during the coating process. A scraper-coated perovskite solar cell and a preparation method thereof are provided. Based on the scraper and the corresponding coating process, the turbulence between the perovskite precursor solution and different substrates can be minimized, the contact angle between the scraper and the perovskite precursor solution can be reduced, the wettability can be improved, and the problems caused by uneven film formation can be reduced, thereby improving the photoelectric conversion efficiency and stability of the perovskite solar cell.
[0006] Technical solution:
[0007] To achieve the above objectives, this application is implemented through the following technical solutions:
[0008] A method for preparing a perovskite solar cell by blade coating comprises the following steps:
[0009] The first step is to immerse the blade coater in a detergent for ultrasonic cleaning, then rinse the detergent with deionized water, and then immerse it in deionized water, acetone and isopropanol for ultrasonic cleaning in sequence, dry it for later use, and deposit a layer of commercial photoresist film on the bottom surface of the blade coater;
[0010] Step 2: Place the scraper from the first step in a 100°C oven for post-baking for 10 minutes;
[0011] Step 3: After the scraper in step 2 is cooled, the bottom surface of the scraper is perpendicular to the light source and exposed through the mask with a circular pattern for 60 seconds;
[0012] Step 4: Immerse the scraper from step 3 in a 1% NaOH aqueous solution for 9-11 seconds, rinse with water, and blow dry with nitrogen;
[0013] Step 5: Use the scraper in step 4 to prepare metal on the bottom surface by physical vapor deposition (PVD) to form a metal layer on the photoresist surface and in the holes;
[0014] Step 6: Use acetone to ultrasonically remove the photoresist from the scraper in step 5, and the metal layer grown on the photoresist is removed together, while the metal layer grown in the holes is retained, thereby obtaining a cylindrical dot array template on the bottom surface of the scraper coater;
[0015] Step 7: Etch the cylindrical point array on the bottom surface of the scraper in step 6, cut off the vertical undulating edges, and obtain the soil slope cylindrical points with embankment-like edges, thus completing the scraper coater with the soil slope cylindrical point array;
[0016] Step 8: Use a doctor blade coater with a soil slope cylindrical dot array to scrape and coat the transparent conductive substrate to prepare the first carrier transport layer;
[0017] Step 9: Use a scraper coater with a soil slope cylindrical dot array to scrape the first carrier transport layer to prepare a perovskite light absorbing layer;
[0018] Step 10: Use a scraper coater with a sloped cylindrical dot array to scrape the perovskite light absorbing layer to prepare a second carrier transport layer; Step 11: Prepare a metal electrode on the second carrier transport layer to complete the preparation of the entire perovskite solar cell.
[0019] Furthermore, the material of the scraper coater is stainless steel, glass, quartz or silicon, and the metal in the fifth step is one or an alloy of gold, silver, copper, nickel and chromium.
[0020] Furthermore, the etching in the seventh step is chemical etching or physical grinding etching. The chemical etching is to seal the scraper in an iodine cylinder, allow the Ag column on the bottom surface of the scraper to react with iodine vapor for 50-70 seconds, then take it out and soak it in 1,3-propylenediamine ethanol solution to etch away the silver iodide. The physical grinding etching is to fix the scraper, apply grinding liquid on the bottom surface of the scraper, and polish and wipe it with a dust-free cloth, repeating multiple times until the etching is completed.
[0021] Furthermore, in the eighth step, the transparent conductive substrate is fluorine-doped tin oxide FTO, indium-doped tin oxide ITO or a metal grid; the first carrier transport layer is a formal structure or a trans structure, when it is a formal structure, the first carrier transport layer is an electron transport layer, and when it is a trans structure, the first carrier transport layer is a hole transport layer; the electron transport layer adopts tin dioxide SnO2, titanium dioxide TiO2, zinc oxide ZnO or a fullerene derivative PCBM; the hole transport layer adopts 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene Spiro-MeOTAD, triphenylamine polymer PTAA or PEDOT:PSS.
[0022] Furthermore, in the ninth step, a discontinuous layer of nanoparticle seeds is first deposited on the bottom surface of the scraper, and then the perovskite precursor solution is coated by three-stage scraping, followed by annealing to complete the preparation of the perovskite light absorbing layer.
[0023] Furthermore, in the tenth step, the second carrier transport layer is a formal structure or a trans structure. When it is a formal structure, the second carrier transport layer is a hole transport layer; when it is a trans structure, the second carrier transport layer is an electron transport layer.
[0024] Furthermore, in the eleventh step, the metal electrode layer is gold Au, which is prepared by evaporation.
[0025] Furthermore, the nanoparticle seeds are selected from one or more of lead iodide, lead bromide, lead chloride, methylammonium iodide, formamidine iodide, cesium iodide, methylammonium bromide, formamidine bromide, cesium bromide, methylammonium chloride, formamidine chloride, and cesium chloride nanoparticles; the solvent of the nanoparticle seeds is selected from one or more of dimethyl sulfoxide DMSO, N,N-dimethylformamide DMF, and isopropyl alcohol IPA, and the concentration of the nanoparticle seeds in the solvent of the nanoparticle seeds is less than or equal to 1 mol / L; the deposition method of the nanoparticle seeds is one of spin coating, spray coating, drip coating, scraping or printing.
[0026] Furthermore, the three-stage scraping coating process divides the coating distance into three sections, namely, front, middle and rear sections, and adjusts the coating speed to eliminate the thickness difference between the front and rear ends of the coating, remove the liquid accumulation phenomenon, and improve the overall uniformity; the front section is 10% of the total distance from the starting point, the middle section is 80% of the total distance after the front section, and the rear section is 10% of the total distance after the middle section;
[0027] The coating speed of the front section is 8-16mm / s, the coating speed of the middle section is 10-20mm / s, and the coating speed of the back section is 12-24mm / s.
[0028] The present application also discloses a blade-coated perovskite solar cell prepared by any of the above-mentioned preparation methods, wherein the blade-coated perovskite solar cell is a formal structure or a trans structure. When the blade-coated perovskite solar cell is a formal structure, an electron transport layer, a perovskite light absorption layer, a hole transport layer and a metal electrode are sequentially arranged on a transparent conductive substrate; when the blade-coated perovskite solar cell is a trans structure, a hole transport layer, a perovskite light absorption layer, an electron transport layer and a metal electrode are sequentially arranged on a transparent conductive substrate; and the perovskite light absorption layer adopts an organic or inorganic perovskite material.
[0029] Beneficial effects:
[0030] The present application provides a blade-coated perovskite solar cell and a preparation method thereof, which has the following beneficial effects compared with the prior art:
[0031] 1. Compared with a flat surface, the soil slope cylindrical point array can reduce the flow shear stress between the precursor solution and the first carrier transport layer, avoiding secondary agglomeration. The perovskite precursor solution flows between and on the surface of the soil slope cylindrical point array. The coating process reduces the flow shear stress between the perovskite precursor solution and the first carrier transport layer. The introduction of the soil slope cylindrical point array inhibits the secondary agglomeration of the perovskite precursor solution between the scraper and the first carrier transport layer.
[0032] 2. The coating rate directly affects the thickness of the wet film. The three-stage coating process can change the situation of the traditional coating with a thin front section and a thick back section, so as to achieve an overall uniform wet film. The film coated by the general scraper is uneven, and is accompanied by problems such as secondary agglomeration of nanoparticles and precursor liquid during the coating process, and the friction between the scraper and the substrate causing discontinuity of the interface between the scraper and the film. The increase in the viscous resistance in the precursor liquid aggravates the agglomeration effect, causing the colloidal particles to aggregate at the leading edge and edge of the perovskite wet film. In addition, due to the enhanced evaporation at the fluid boundary, the viscous resistance of the migration of the colloidal particles is further increased. This application proposes a scraper with a soil slope cylindrical point array, which is used to shear perovskite colloidal particles in the process of preparing large-area perovskite. The technical effect of the soil slope cylindrical point array scraper is that shear stress and tensile flow are introduced through the arrangement of the array, which greatly reduces the generation of colloidal particle flux in the perovskite wet film state, thereby avoiding secondary agglomeration of the entire film, and further suppressing the influence of secondary agglomeration on the perovskite film. The sensitivity of colloidal particles to scale and substrate differences can be well reduced, and the uniform distribution of colloidal particles can significantly improve the overall crystallization uniformity of the perovskite film;
[0033] 3. The uniform distribution of colloidal particles in the perovskite precursor solution is a key factor in obtaining high-quality perovskite films; compared with general flat scrapers, due to the introduction of shear strain and tensile flow, the scraper with a sloped cylindrical point array can effectively shear the colloidal particles, significantly improve the mobility of the colloidal particles, and significantly shorten the lag time of the colloidal particles on the substrate. The pre-deposition of nanoparticle seeds reduces the contact angle between the solution to be deposited and the bottom surface of the scraper, improves the wettability, and then the deposited solution is spread on the surface to form a uniform thin film; the three-stage coating process divides the coating path into three sections: front, middle and back, adjusts its coating speed, eliminates the thickness difference between the front and back ends of the coating, removes the liquid accumulation phenomenon, and improves the overall uniformity. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic diagram of the blade coater of the present application;
[0035] Figure 2 is a schematic diagram of a blade coater with a cylindrical dot array of the present application;
[0036] Figure 3 This is a structural diagram of the perovskite solar cell of this application. DETAILED DESCRIPTION
[0037] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0038] Embodiment 1:
[0039] A method for preparing a perovskite solar cell by blade coating of a formal structure comprises the following steps:
[0040] The first step is to immerse the blade coater in a detergent for ultrasonic cleaning, then rinse the detergent with deionized water, and then immerse it in deionized water, acetone and isopropanol for ultrasonic cleaning in sequence, dry it for later use, and deposit a layer of commercial photoresist film on the bottom surface of the blade coater;
[0041] Step 2: Place the scraper from the first step in a 100°C oven for post-baking for 10 minutes;
[0042] Step 3: After the scraper in step 2 is cooled, the bottom surface of the scraper is perpendicular to the light source and exposed through the mask with a circular pattern for 60 seconds;
[0043] Step 4: Immerse the scraper from step 3 in a 1% NaOH aqueous solution for 9-11 seconds, rinse with water, and blow dry with nitrogen;
[0044] Step 5: Use the scraper in step 4 to prepare metal Ag on the bottom surface by physical vapor deposition (PVD) to form an Ag metal layer on the photoresist surface and in the holes;
[0045] Step 6: Use acetone to ultrasonically remove the photoresist from the scraper in step 5. The Ag metal layer grown on the photoresist is removed together, and the Ag metal layer grown in the holes is retained, thereby obtaining an Ag cylindrical dot array template on the bottom surface of the scraper coater, as shown in FIG. Figure 1 ;
[0046] Step 7: Place the knife from step 6 into an iodine cylinder and seal it. Let the Ag cylinder on the bottom surface of the scraper react with the iodine vapor for 50-70 seconds. Then take it out and soak it in 1,3-propylenediamine ethanol solution (volume ratio 1:1). Etch away the silver iodide and cut off the vertical undulating edges to obtain the soil slope-shaped cylindrical points with embankment-like edges. At this point, the scraper coater with soil slope-shaped Ag cylindrical point array is completed. Figure 2 ; Step 8: immerse the indium tin oxide ITO glass in detergent for ultrasonic cleaning, then rinse off the detergent with deionized water, and then immerse it in deionized water, acetone and isopropanol for ultrasonic cleaning in turn, dry it, prepare a SnO2 aqueous dispersion diluted with water at a volume ratio of 1:2, take 20ul between the scraper and the ITO glass, the GAP height is 30um, the coating speed is 10mm / s, heat at 150℃ for 30min, transfer it to a UV-ozone cleaner for cleaning for 10 minutes, cool it naturally to room temperature to complete annealing, and form an electron transport layer;
[0047] Step 9: PbI2 and MAI are mixed in a certain proportion and dissolved in a N,N-dimethylformamide (DMF) solvent at a concentration of 1 mol / ml, sprayed on the bottom surface of the scraper, and dried to form nanoparticle seeds; PbI2, MAI, and FAI are dissolved in a mixed solvent of dimethyl sulfoxide (DMSO) and DMF at a certain proportion. The volume ratio of SO and DMF is 1:4, and it is completely dissolved by heating at 70°C, and then scraped on the electron transport layer prepared in the previous step. The GAP height is 30um, the front scraping speed is 8mm / s, the middle scraping speed is 10mm / s, and the rear scraping speed is 12mm / s. Then the perovskite wet film is placed in a vacuum box, and the vacuum box is evacuated to 10Pa within 5s and maintained for 1 minute, and then annealed at 100°C for 10min to form a perovskite light absorption layer;
[0048] Step 10: Dissolve 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) in chlorobenzene (CB) solvent at a concentration of 72.3 mg / mL, stir vigorously to dissolve it completely, then add 28.8 μL of 4-tert-butylpyridine and 17.5 μL of bis(trifluoromethanesulfonyl)imide lithium (Li-TFSI) Li-TFSI acetonitrile solution (concentration of 520 mg / mL) to 1 mL of the solution, stir evenly, and then scrape on the perovskite light-absorbing layer prepared in the previous step, with a GAP height of 30 μm and a scraping speed of 20 mm / s to form a hole transport layer;
[0049] Step 11: Transfer to a metal evaporation chamber and use vacuum thermal evaporation with a mask to prepare an 80nm thick gold (Au) electrode to form a metal electrode, thus completing the preparation of the formal perovskite solar cell.
[0050] Embodiment 2:
[0051] A method for preparing a perovskite solar cell with a reverse structure by blade coating comprises the following steps:
[0052] The first step is to immerse the blade coater in a detergent for ultrasonic cleaning, then rinse the detergent with deionized water, and then immerse it in deionized water, acetone and isopropanol for ultrasonic cleaning in sequence, dry it for later use, and deposit a layer of commercial photoresist film on the bottom surface of the blade coater;
[0053] Step 2: Place the scraper from the first step in a 100°C oven for post-baking for 10 minutes;
[0054] Step 3: After the scraper in step 2 is cooled, the bottom surface of the scraper is perpendicular to the light source and exposed through the mask with a circular pattern for 60 seconds;
[0055] Step 4: Immerse the scraper from step 3 in a 1% NaOH aqueous solution for 9-11 seconds, rinse with water, and blow dry with nitrogen;
[0056] Step 5: Use the scraper in step 4 to prepare metal Cu on the bottom surface by physical vapor deposition (PVD) to form a Cu metal layer on the photoresist surface and in the holes;
[0057] Step 6: The scraper in step 5 is used to remove the photoresist by ultrasonic acetone, and the Cu metal layer grown on the photoresist is removed together, and the Cu metal layer grown in the holes is retained, thereby obtaining a Cu cylindrical dot array template on the bottom surface of the scraper coater;
[0058] Step 7: Fix the scraper in step 6, apply abrasive liquid on the bottom surface of the scraper, and polish and wipe it with a dust-free cloth, reciprocating for many times until a soil slope-shaped Cu cylindrical point with a bank-like edge is obtained, and the scraper coater with a soil slope-shaped Cu cylindrical point array is completed;
[0059] Step 8: Immerse the indium tin oxide ITO glass in detergent for ultrasonic cleaning, then rinse off the detergent with deionized water, and then immerse it in deionized water, acetone and isopropanol for ultrasonic cleaning in turn, dry it, dissolve poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine (PTAA) in chlorobenzene (CB) at a concentration of 5 mg / mL, and apply at a scraping speed of 10 mm / s. The GAP height is 30 um, and the temperature is heated at 120°C for 10 minutes, and then naturally cooled to room temperature for annealing to form a hole transport layer;
[0060] Step 9: Mix lead iodide (PbI2) and methylamine iodide (MAI) in proportion and dissolve them in N,N-dimethylformamide (DMF) solvent at a concentration of 1 mol / ml, spray them on the bottom surface of the scraper, and dry them to form nanoparticle seeds; weigh five powders of lead iodide (PbI2), lead bromide (PbBr2), formamidine iodine (FAI), methylamine bromide (MABr), and cesium iodide (CsI) in the same reagent bottle, add a mixed solvent of DMSO and DMF at a volume ratio of 1:4, and control The concentration of lead ions in the final precursor solution is 1.5 mol / L. The solution is placed on a hot plate at 90°C and heated to fully dissolve. The solution is then scraped on the hole transport layer prepared in the previous step. The GAP height is 30 um. The scraping speeds of the front section, the middle section, and the rear section are 14 mm / s. The perovskite wet film is then placed in a vacuum box. The vacuum box is evacuated to 10 Pa within 5 seconds and maintained for 1 minute. The solution is then annealed at 100°C for 10 minutes to form a perovskite light-absorbing layer.
[0061] Step 10: Dissolve the fullerene derivative PC61BM in CB solvent at a concentration of 20 mg / mL, stir on a hot plate at 60°C for 2 hours, and scrape on the previously prepared perovskite light-absorbing layer at a scraping speed of 10 mm / s and a GAP height of 30 um to obtain an electron transport layer; scrape a saturated isopropanol solution of bathocuproin (BCP) on the electron transport layer to form a buffer layer at a scraping speed of 20 mm / s and a GAP height of 30 um;
[0062] Step 11: Transfer to a metal evaporation chamber and use vacuum thermal evaporation with a mask to prepare an 80nm thick silver (Ag) electrode to form a metal electrode, thus completing the preparation of the inverse perovskite solar cell.
[0063] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A method for preparing a perovskite solar cell by blade coating, characterized in that: The specific steps include: The first step is to immerse the blade coater in a detergent for ultrasonic cleaning, then rinse the detergent with deionized water, and then immerse it in deionized water, acetone and isopropanol for ultrasonic cleaning in sequence, dry it for later use, and deposit a layer of commercial photoresist film on the bottom surface of the blade coater; Step 2: Place the scraper from the first step in a 100°C oven for post-baking for 10 minutes; Step 3: After the scraper in step 2 is cooled, the bottom surface of the scraper is perpendicular to the light source and exposed through the mask with a circular pattern for 60 seconds; Step 4: Immerse the scraper from step 3 in a 1% NaOH aqueous solution for 9-11 seconds, rinse with water, and blow dry with nitrogen; Step 5: Use the scraper in step 4 to prepare metal on the bottom surface by physical vapor deposition (PVD) to form a metal layer on the photoresist surface and in the holes; Step 6: Use acetone to ultrasonically remove the photoresist from the scraper in step 5, and the metal layer grown on the photoresist is removed together, while the metal layer grown in the holes is retained, thereby obtaining a cylindrical dot array template on the bottom surface of the scraper coater; Step 7: Etch the cylindrical point array on the bottom surface of the scraper in step 6, cut off the vertical undulating edges, and obtain the soil slope cylindrical points with embankment-like edges, thus completing the scraper coater with the soil slope cylindrical point array; Step 8: Use a doctor blade coater with a soil slope cylindrical dot array to scrape and coat the transparent conductive substrate to prepare the first carrier transport layer; Step 9: Use a scraper coater with a soil slope cylindrical dot array to scrape and coat the first carrier transport layer to prepare a perovskite light absorbing layer; Step 10: Use a doctor blade coater with a soil slope cylindrical dot array to scrape the perovskite light absorption layer to prepare a second carrier transport layer; Step 11: Prepare a metal electrode on the second carrier transport layer to complete the preparation of the entire perovskite solar cell.
2. The method for preparing a perovskite solar cell by blade coating according to claim 1, characterized in that: The material of the scraper coater is stainless steel, glass, quartz or silicon, and the metal in the fifth step is one or an alloy of gold, silver, copper, nickel and chromium.
3. The method for preparing a perovskite solar cell by blade coating according to claim 1, characterized in that: The etching in the seventh step is chemical etching or physical grinding etching. The chemical etching is to put the scraper into an iodine cylinder and seal it, allowing the Ag column on the bottom surface of the scraper to react with iodine vapor for 50-70 seconds, then take it out and soak it in 1,3-propylenediamine ethanol solution to etch away the silver iodide. The physical grinding etching is to fix the scraper, apply grinding liquid on the bottom surface of the scraper, and polish and wipe it with a dust-free cloth, repeating multiple times until the etching is completed.
4. The method for preparing a perovskite solar cell by blade coating according to claim 1, characterized in that: In the eighth step, the transparent conductive substrate is fluorine-doped tin oxide FTO, indium-doped tin oxide ITO or a metal grid; the first carrier transport layer is a formal structure or a trans structure, and when it is a formal structure, the first carrier transport layer is an electron transport layer, and when it is a trans structure, the first carrier transport layer is a hole transport layer; The electron transport layer uses tin dioxide SnO2, titanium dioxide TiO2, zinc oxide ZnO or fullerene derivative PCBM; The hole transport layer adopts 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene Spiro-MeOTAD, triphenylamine polymer PTAA or PEDOT:PSS.
5. The method for preparing a perovskite solar cell by blade coating according to claim 1, characterized in that: In the ninth step, a discontinuous layer of nanoparticle seeds is first deposited on the bottom surface of the scraper, and then the perovskite precursor solution is coated by three-stage scraping, followed by annealing to complete the preparation of the perovskite light absorbing layer.
6. The method for preparing a perovskite solar cell by blade coating according to claim 1, characterized in that: In the tenth step, the second carrier transport layer is a regular structure or a trans structure. When it is a regular structure, the second carrier transport layer is a hole transport layer; when it is a trans structure, the second carrier transport layer is an electron transport layer.
7. The method for preparing a perovskite solar cell by blade coating according to claim 1, characterized in that: In the eleventh step, the metal electrode layer is gold Au, which is prepared by evaporation.
8. The method for preparing a perovskite solar cell by blade coating according to claim 5, characterized in that: The nanoparticle seeds are selected from one or more of lead iodide, lead bromide, lead chloride, methylammonium iodide, formamidine iodide, cesium iodide, methylammonium bromide, formamidine bromide, cesium bromide, methylammonium chloride, formamidine chloride, and cesium chloride nanoparticles; the solvent of the nanoparticle seeds is selected from one or more of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), and isopropyl alcohol (IPA); the concentration of the nanoparticle seeds in the solvent of the nanoparticle seeds is less than or equal to 1 mol / L; the deposition method of the nanoparticle seeds is one of spin coating, spray coating, drip coating, scraping, or printing.
9. The method for preparing a perovskite solar cell by blade coating according to claim 5, characterized in that: The three-stage scraping coating process divides the coating distance into three sections, namely, front, middle and rear sections, and adjusts the coating speed to eliminate the thickness difference between the front and rear ends of the coating, remove the liquid accumulation phenomenon, and improve the overall uniformity; the front section is 10% of the total distance traveled from the starting point, the middle end is 80% of the total distance traveled after the front section, and the rear section is 10% of the total distance traveled after the middle section; the coating speed of the front section is 8-16 mm / s, the coating speed of the middle section is 10-20 mm / s, and the coating speed of the rear section is 12-24 mm / s.
10. A blade-coated perovskite solar cell prepared by any preparation method of claims 1-9, characterized in that: The blade-coated perovskite solar cell is a formal structure or a trans structure. When the blade-coated perovskite solar cell is a formal structure, an electron transport layer, a perovskite light absorption layer, a hole transport layer and a metal electrode are sequentially arranged on a transparent conductive substrate; when the blade-coated perovskite solar cell is a trans structure, a hole transport layer, a perovskite light absorption layer, an electron transport layer and a metal electrode are sequentially arranged on a transparent conductive substrate; the perovskite light absorption layer adopts an organic or inorganic perovskite material.
Citation Information
Patent Citations
A preparation method of large-area perovskite thin film and a battery module thereof
CN109103338A
Solvent system for perovskite solar cell and preparation method of perovskite solar cell
CN114203912A
Method for preparing large-scale perovskite array through screen printing
CN115377299A
Perovskite solar cell and preparation method thereof
CN115835741A
A method for preparing a flexible perovskite solar cell by blade coating
WO2019000642A1