Perovskite layer preparation method, laminated solar cell and preparation method

By introducing an ion diffusion layer during the preparation of the perovskite layer, the problem of incomplete bonding of lead iodide/cesium bromide with ammonium salt film in the traditional method is solved, and the quality of the perovskite layer and the performance of solar cells are improved.

CN118890941AInactive Publication Date: 2024-11-01SHENZHEN HIKING PV TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411343141.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the traditional perovskite layer preparation method, the binding of lead iodide/cesium bromide film and ammonium salt film is incomplete, resulting in a large number of defects in the perovskite layer, affecting the performance and life of solar cells.

Method used

Lead iodide/cesium bromide film was prepared by co-evaporation, and an ion diffusion layer was formed on its surface. Then, an ammonium salt film was prepared on the surface of the ion diffusion layer and annealed to form a perovskite layer to improve the dispersion and reaction of the ammonium salt. sex.

Benefits of technology

It effectively reduces the defect density of the perovskite layer, improves the photoelectric conversion efficiency and device stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118890941A_ABST
    Figure CN118890941A_ABST
Patent Text Reader

Abstract

The invention provides a perovskite layer preparation method, a laminated solar cell and a preparation method, and belongs to the technical field of perovskite laminated solar cells. Firstly, a lead iodide / cesium bromide thin film is prepared through a co-evaporation method, after co-evaporation, an ion diffusion material is evaporated to the surface of the lead iodide / cesium bromide thin film to form an ion diffusion layer, free diffusion can be carried out in the perovskite thin film, perovskite reaction is promoted, and the perovskite performance is improved. Meanwhile, the ion diffusion layer can passivate defects in the forming process of the perovskite thin film, so that the conformal perovskite thin film with lower defect density is formed, and the performance of the device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of perovskite tandem solar cells, and in particular to a perovskite layer preparation method and a tandem solar cell and a preparation method thereof. Background Art

[0002] Perovskite tandem solar cells are a new type of solar cell with high-efficiency photoelectric conversion potential. They use perovskite as a photovoltaic material and are composed of perovskite layers combined through a stacked structure. Each stacked structure in the stacked solar cell can absorb sunlight of different wavelengths, thereby maximizing the photoelectric conversion efficiency and achieving more efficient use of light energy. The working principle of perovskite tandem solar cells is that when sunlight is irradiated on the perovskite tandem solar cell, the sunlight can be divided into several continuous parts. The light with the shortest wavelength is absorbed and utilized by the outermost wide bandgap material battery, and the light with a longer wavelength can be transmitted in to be absorbed and utilized by the narrower bandgap material battery, thereby maximizing the conversion of light energy into electrical energy. The bandgap of the perovskite material in the perovskite layer is small and can absorb sunlight with a longer wavelength. In addition, the perovskite material also exhibits a higher light absorption coefficient. Therefore, perovskite tandem solar cells have been widely used.

[0003] At present, the preparation methods of perovskite layer include evaporation, spin coating, light treatment and plasma treatment, among which the most commonly used methods are evaporation and spin coating. Usually, the perovskite layer adopts a two-step co-evaporation method, firstly preparing the lead iodide / cesium bromide film by evaporation, and then preparing the ammonium salt film on the lead iodide / cesium bromide film by evaporation, or first preparing the lead iodide / cesium bromide film by evaporation, and then preparing the ammonium salt film on the lead iodide / cesium bromide film by spin coating. However, when the ammonium salt film prepared by these two methods is combined with the lead iodide / cesium bromide film, the lead iodide / cesium bromide at the bottom of the lead iodide / cesium bromide film cannot directly contact the ammonium salt, and it is difficult to react completely, and a large amount of lead iodide residue is finally formed in the lower layer inside the perovskite layer. These free lead iodides will form a large number of defects in the perovskite layer, resulting in low quality of the formed perovskite film, thereby affecting the device performance.

[0004] Therefore, the perovskite film prepared by the traditional two-step method will cause incomplete deposition on the lead iodide / cesium bromide film, resulting in a large number of defects in the perovskite layer, which will shorten the life of the solar cell and reduce the absorbance during use, thereby affecting the performance of the prepared solar cell. Summary of the invention

[0005] The invention provides a perovskite layer preparation method, a laminated solar cell and a preparation method. The invention prepares a lead iodide / cesium bromide film by a co-evaporation method, then prepares an ion diffusion layer on the surface of the lead iodide / cesium bromide film, and finally prepares an ammonium salt film on the surface of the ion diffusion layer and anneals to react to form a perovskite layer, wherein the ion diffusion layer enables the ammonium salt in the ammonium salt film to be more evenly and quickly dispersed in the lead iodide and cesium bromide films, so that the prepared perovskite layer has lower defects, and the photoelectric conversion efficiency and stability of the device are effectively improved.

[0006] To achieve the above object, the specific scheme provided by the present invention is as follows:

[0007] A method for preparing a perovskite layer, the method comprising the following steps:

[0008] S1, providing a battery substrate, and co-evaporating lead iodide and cesium bromide onto the surface of the battery substrate by a co-evaporation method to obtain a lead iodide / cesium bromide thin film;

[0009] S2, on the surface of the lead iodide / cesium bromide film in S1, evaporating an ion diffusion material by an evaporation method to obtain an ion diffusion layer;

[0010] S3. Spin-coating the surface of the ion diffusion layer in S2 with an ammonium salt precursor solution, followed by annealing to obtain the perovskite layer.

[0011] Furthermore, the battery substrate includes a crystalline silicon bottom battery, a tunneling layer and a hole transport layer in sequence from bottom to top, and the lead iodide / cesium bromide film is prepared on the surface of the hole transport layer.

[0012] Furthermore, the ratio of the evaporation rate of lead iodide in the co-evaporation method to the evaporation rate of the lead iodide is (2:1)-(10:1).

[0013] Furthermore, the evaporation time of the co-evaporation method in step S1 is 1-10000s.

[0014] Furthermore, the thickness of the lead iodide / cesium bromide film in step S1 is 200-800 nm.

[0015] Furthermore, the ion diffusion material in step S2 is one or more of rubidium fluoride (RbF), potassium fluoride (KF), sodium fluoride (NaF), rubidium chloride (RbCl), potassium chloride (KCl), and sodium chloride (NACl).

[0016] Furthermore, the vacuum degree of the evaporation in the evaporation method in step S2 is 1×10 -4 Pa-5×10 -4 The evaporation temperature is 50-400°C, and the evaporation rate is 0.05-1Å / S.

[0017] Furthermore, the thickness of the ion diffusion layer in step S2 is 1-100 nm.

[0018] Furthermore, the ammonium salt precursor solution in step S3 is a mixed solution of formamidine iodide (FAI) and formamidine bromide (FABr).

[0019] Furthermore, the concentration of formamidine iodide (FAI) and formamidine bromide (FABr) in the solution is 0.5-2 mol / L, and the molar ratio of formamidine iodide (FAI) and formamidine bromide (FABr) in the solution is (1:10)-(10:1).

[0020] Furthermore, the ammonium salt precursor solution also includes an additive, the additive is methylammonium chloride (MACl), and the mass fraction of the methylammonium chloride (MACl) accounts for 0.5-50% of the ammonium salt precursor solution.

[0021] Furthermore, the spin coating speed of the spin coating method in step S3 is 1200-6000 rpm, and the spin coating time is 20-120 s.

[0022] Furthermore, the annealing temperature in step S3 is 50-150° C., and the annealing time is 5-40 min.

[0023] The present invention also provides a stacked solar cell, comprising a crystalline silicon bottom cell, a tunneling layer and a perovskite top cell, wherein the perovskite top cell comprises a hole transport layer, a perovskite layer, an electron transport layer, a second transparent electrode layer, a second metal electrode layer and an anti-reflection layer, and the perovskite layer is prepared by the above-mentioned perovskite preparation method.

[0024] Furthermore, the perovskite layer is ABX 3 Structure, where the A position is an organic cation, including CH 3 NH 3 + (MA + ), NH 2 CH=NH 2 + (FA + ), CH 3 CH 2 NH 3 + or Cs + At least one of;

[0025] The B position is a metal cation, including Pb 2+ Sn 2+ At least one of;

[0026] The X position is a halogen anion, including F - , Cl - Br - ,I - At least one of .

[0027] Furthermore, the crystalline silicon bottom cell can be selected from a crystalline silicon cell such as a pear cell, a topcon cell or a HJT cell;

[0028] Specifically, the crystalline silicon bottom cell includes, from bottom to top, a first metal electrode layer, a first transparent electrode layer, a P-type base doping layer, a base passivation layer, a textured crystalline silicon substrate, a base surface passivation layer and an N-type base doping layer.

[0029] In this embodiment, the surface of the textured crystalline silicon substrate is provided with a textured structure, which can reduce surface reflection and light escape, improve light capture efficiency, and thus improve photoelectric conversion efficiency.

[0030] The textured crystalline silicon substrate can be selected from one of intrinsic single crystal silicon, intrinsic polycrystalline silicon, N-type or P-type single crystal silicon.

[0031] In this embodiment, the hole transport layer is poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly-3-hexylthiophene (P 3 HT), nickel oxide (NiO x ), molybdenum trioxide (MoO 3 ), cuprous iodide (CuI), and cuprous thiocyanate (CuSCN);

[0032] In this embodiment, the electron transport layer is zinc oxide (ZnO), tin dioxide (SnO 2 ), titanium dioxide (TiO 2 ), [6,6] phenyl C 61 Methyl butyrate (PC 61 BM), carbon 60 (C 60 ), at least one of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP);

[0033] In this embodiment, the first transparent electrode layer and the second transparent electrode layer are composed of at least one of indium tin oxide (ITO), indium zinc oxide (IZO), and aluminum zinc oxide (AZO);

[0034] In this embodiment, the first metal electrode layer and the second metal electrode layer are composed of at least one of silver (Ag), gold (Au), copper (Cu), aluminum (Al), and carbon (C);

[0035] In this embodiment, the anti-reflection layer is magnesium fluoride, lithium fluoride (LiF), sodium fluoride (NaF), silicon oxide (SiO 2 ) is composed of at least one of the following.

[0036] Furthermore, a passivation layer is provided between the perovskite layer and the electron transport layer.

[0037] The passivation layer includes but is not limited to at least one of propylenediamine bromide (PDADBr), butylammonium chloride (BACl), butylammonium bromide (BABr), butylammonium iodide (BAI), N,N-dimethyl-1,3-propylenediamine hydrochloride (DMePDADCl), and dodecanediaminium bromide (DDDADBr); it may also be at least one of magnesium fluoride (MgF), lithium fluoride (LiF), and sodium fluoride (NaF).

[0038] Furthermore, a buffer layer is provided between the electron transport layer and the second transparent electrode layer.

[0039] The buffer layer is zinc oxide (ZnO), tin dioxide (SnO 2 ), titanium dioxide (TiO 2 ) is composed of at least one of the following.

[0040] The present invention also provides a method for preparing a stacked solar cell, comprising the following steps:

[0041] A textured crystalline silicon substrate is provided, wherein a base passivation layer is prepared on the back of the textured crystalline silicon substrate, a P-type base doping layer is prepared on the surface of the base passivation layer, a first transparent electrode layer is prepared on the surface of the P-type base doping layer, and a first metal electrode layer is prepared on the surface of the first transparent electrode layer; and a base surface passivation layer is prepared on the surface of the textured crystalline silicon substrate, an N-type base doping layer is prepared on the surface of the base surface passivation layer, a tunneling layer is prepared on the surface of the N-type base doping layer, a hole transport layer is prepared on the surface of the tunneling layer, a perovskite layer is prepared on the surface of the hole transport layer, a passivation layer is prepared on the surface of the perovskite layer, an electron transport layer is prepared on the surface of the passivation layer, a buffer layer is prepared on the surface of the electron transport layer, a second transparent electrode layer is prepared on the surface of the buffer layer, a second metal electrode layer is prepared on the surface of the second transparent electrode layer, and an anti-reflection layer is prepared on the surface of the second metal electrode layer.

[0042] In this embodiment, the perovskite layer is prepared by using the above-mentioned perovskite preparation method.

[0043] In order to saturate the dangling bonds on the surface of the textured crystalline silicon substrate, reduce the surface activity, increase the surface cleaning process, avoid the formation of recombination centers due to the introduction of impurities in the surface layer, and thereby reduce the surface recombination rate of minority carriers, a base passivation layer and a base surface passivation layer can be formed on the two surfaces of the textured crystalline silicon substrate respectively by vapor deposition, atomic layer deposition and the like.

[0044] In one embodiment, a phosphorus source / nitrogen source is diffused on a textured crystalline silicon substrate to form a doping structure, thereby obtaining the P-type base doping layer and the N-type base doping layer.

[0045] In one embodiment, the first transparent electrode layer is prepared by a magnetron sputtering method, wherein the prepared substrate sample is placed in a magnetron sputtering device for preparation, and the magnetron sputtering power is 50-200W;

[0046] In one embodiment, the first metal electrode layer is deposited by evaporation, including placing the prepared substrate sample on a mask plate for evaporation, and the evaporation vacuum is 5×10 -5 -2×10 -4 Pa, the evaporation temperature is 500-2000℃, and the evaporation rate is 0.1-5Å / S;

[0047] In one embodiment, the tunneling layer is used to solve the problem of electrical mismatch and device instability between two series-connected batteries, and can be prepared by atomic layer deposition, magnetron sputtering or wet chemical method.

[0048] In one embodiment, the hole transport layer is formed by spin coating, which includes uniformly coating the hole transport layer dispersion on the surface of the tunnel layer, with a spin coating speed of 1000-5000 rpm and a spin coating time of 10-100 s; after the spin coating, an annealing operation is performed, with an annealing temperature of 300-600° C. and an annealing time of 10-50 min.

[0049] Optionally, the hole transport layer may also be formed by magnetron sputtering, specifically, placing the prepared substrate sample in a magnetron sputtering device with a control power of 30-90W.

[0050] In one embodiment, the passivation layer is deposited by evaporation, which includes evaporating the passivation layer material onto the surface of the perovskite layer, and the evaporation vacuum is 1×10 -4 -5×10 -4 Pa, the evaporation temperature is 50-400℃, the evaporation rate is 0.05-1Å / S, and after the evaporation, annealing operation is performed, the annealing temperature is 0-150℃, and the annealing time is 0-30min;

[0051] Alternatively, the passivation layer may also be spin-coated, including preparing a passivation layer dispersion and uniformly coating it on the surface of the perovskite layer, wherein the passivation layer dispersion is prepared by dissolving the passivation layer material in an organic solvent including but not limited to methanol, ethanol or isopropanol, ultrasonically dissolving and spin-coating, the concentration of the passivation layer dispersion is 0.1-6 mg / mL, the ultrasonic time is 0-30 min, the spin coating speed is 1000-7000 rpm, the spin coating time is 20-120 s, and after the spin coating is completed, an annealing operation is performed, the annealing temperature is 40-160° C., and the annealing time is 5-40 min;

[0052] Alternatively, the passivation layer may also be sprayed, including spraying the passivation layer dispersion on the perovskite layer at a spraying rate of 0-100 cm / s, and after spraying, performing an annealing operation at an annealing temperature of 20-170° C. for a time of 0-30 min;

[0053] In one embodiment, the electron transport layer is formed by spin coating, specifically, the electron transport layer dispersion is uniformly spin coated on the surface of the passivation layer, the spin coating speed is 500-4000 rpm, and the spin coating time is 10-80 s;

[0054] Optionally, the electron transport layer can also be deposited by evaporation to evaporate the electron transport layer material onto the surface of the passivation layer, and the evaporation vacuum degree is 5×10 -5 -5×10 -4 Pa, the evaporation temperature is 100-400℃, and the evaporation rate is 0.05-1Å / S;

[0055] In one embodiment, the buffer layer is deposited by atomic layer deposition, which includes depositing the buffer layer material onto the surface of the electron transport layer using an atomic layer deposition device, and the deposition vacuum is 0-1×10 4 Pa, the deposition pipeline temperature is between 50-150°C, and the deposition chamber temperature is 40-150°C;

[0056] Optionally, the buffer layer can also be formed by evaporation to evaporate the buffer layer material onto the surface of the electron transport layer, and the evaporation vacuum is 6×10 -5 -4×10 -4 Pa, the evaporation temperature is 100-500℃, and the evaporation rate is 0.05-1Å / S;

[0057] In one embodiment, the second transparent electrode layer is formed by a magnetron sputtering method, including sputtering a transparent electrode material onto the surface of the buffer layer, with a control power of 30-200W;

[0058] Alternatively, the second transparent electrode layer may also be formed by a vapor deposition method, characterized in that the transparent electrode material is evaporated onto the surface of the buffer layer, and the vacuum degree of the vapor deposition is 1×10 -5-5×10 -4 Pa, the evaporation temperature is 1000-2000℃, and the evaporation rate is 0.05-3Å / S.

[0059] In one embodiment, the anti-reflection layer can be prepared by magnetron sputtering or evaporation.

[0060] The present invention provides a method for preparing a perovskite layer, a laminated solar cell and a preparation method. By preparing an ion diffusion layer between a lead iodide / cesium bromide film and an ammonium salt film, the deposition effect of the ammonium salt in the lead iodide / cesium bromide film is improved, and the traditional two-step method for preparing the perovskite layer is changed. First, the lead iodide / cesium bromide film is prepared by a co-evaporation method. After the first co-evaporation, the ion diffusion material is evaporated onto the surface of the lead iodide / cesium bromide film to form an ion diffusion layer. The ion diffusion layer is a halogen ion material such as rubidium fluoride and rubidium chloride, which has a high ionic conductivity under high temperature conditions. Secondly, the ion radius of the ion diffusion layer material is smaller than the perovskite lattice radius, and can diffuse freely inside the film during the perovskite formation process, which allows the ammonium salt in the ammonium salt film to react more completely with the lead iodide / cesium bromide film. At the same time, the ion diffusion layer can also passivate defects in the process of forming the perovskite film, thereby forming a high-quality, low-defect-density conformal perovskite film and improving device performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 is a schematic structural diagram of the stacked solar cell described in the present invention;

[0062] Figure 2 is a flow chart for preparing the perovskite layer of the present invention;

[0063] The numbers in the figure are: 1, battery substrate; 10, crystalline silicon bottom battery; 20, tunneling layer; 30, perovskite top battery; 101, first metal electrode layer; 102, first transparent electrode layer; 103, P-type base doping layer; 104, base passivation layer; 105, velvet crystalline silicon substrate; 106, base surface passivation layer; 107, N-type base doping layer; 301, hole transport layer; 302, perovskite layer; 303, passivation layer; 304, electron transport layer; 305, buffer layer; 306, second transparent electrode layer; 307, second metal electrode layer; 308, anti-reflection layer; L1, lead iodide / cesium bromide film; L2, ion diffusion layer; L3, ammonium salt film. DETAILED DESCRIPTION

[0064] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0065] In the description of the present invention, unless otherwise specified, "multiple" means two or more; the terms "center", "longitudinal", "lateral", "up", "down", "left", "right", "inside", "outside", "front end", "rear end", "head", "tail", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate the orientation or position relationship based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third" and the like are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0066] Example 1

[0067] See also Figure 1~2 This embodiment provides a method for preparing a perovskite layer, comprising the following steps:

[0068] S1, providing a battery substrate 1, and co-evaporating lead iodide and cesium bromide onto the surface of the battery substrate 1 by a co-evaporation method to obtain a 440nm lead iodide / cesium bromide film L1, wherein the evaporation rate of the lead iodide is 8A / s, the evaporation rate of the cesium bromide is 0.8A / s, and the total evaporation time is 1000s;

[0069] S2, on the surface of the lead iodide / cesium bromide film L1 in S1, rubidium fluoride is evaporated by evaporation to obtain a 1 nm ion diffusion layer L2, the vacuum degree of the evaporation is 1×10 -4 Pa, the evaporation temperature is 400 °C, and the evaporation rate is 0.05 Å / S;

[0070] S3. On the surface of the ion diffusion layer L2 in S2, an ammonium salt precursor solution is coated by spin coating, and annealed to obtain the perovskite layer L3; the spin coating speed is 5000 rpm, the spin coating time is 30 s, the annealing temperature is 150° C., the annealing time is 10 min, the molar ratio of formamidine iodide (FAI) to formamidine bromide (FABr) in the ammonium salt precursor solution is 1:4.7, the ammonium salt precursor solution also includes an additive, the additive is methylamine chloride (MACl), the mass fraction of the methylamine chloride (MACl) accounts for 10% of the formamidine iodide (FAI) and formamidine bromide (FABr) solutions, and the concentrations of formamidine iodide (FAI) and formamidine bromide (FABr) in the ammonium salt precursor solution are both 1 mol / L.

[0071] The present embodiment also provides a stacked solar cell, comprising a crystalline silicon bottom cell 10, a tunneling layer 20 and a perovskite top cell 30, wherein the crystalline silicon bottom cell 10 comprises, from bottom to top, a first metal electrode layer 101, a first transparent electrode layer 102, a P-type base doping layer 103, a base passivation layer 104, a velvet crystalline silicon substrate 105, a base surface passivation layer 106, and an N-type base doping layer 107, and the perovskite top cell 30 comprises, from bottom to top, a hole transport layer 301, a perovskite layer 302, a passivation layer 303, an electron transport layer 304, a buffer layer 305, a second transparent electrode layer 306, a second metal electrode layer 307, and an anti-reflection layer 308, and the perovskite layer is prepared by the above-mentioned perovskite preparation method.

[0072] This embodiment also provides a method for preparing the stacked solar cell, comprising the following steps:

[0073] S (1) providing a textured crystalline silicon substrate 105, preparing a base passivation layer 104 on the back side of the textured crystalline silicon substrate 105, and diffusing a phosphorus source into the base passivation layer 104 to form a P-type base doping layer 103; preparing a base surface passivation layer 106 on the surface of the textured crystalline silicon substrate 105, and diffusing a nitrogen source into the base surface passivation layer 106 to form an N-type base doping layer 107;

[0074] S(2), preparation of the first transparent electrode layer 102:

[0075] The first transparent electrode layer 102 is prepared on the surface of the P-type base doping layer 103 by magnetron sputtering. The thickness of the first transparent electrode layer 102 is 100 nm. The target material of the magnetron sputtering is indium tin oxide (ITO). The power of the magnetron sputtering is 60 W. The operation time of the magnetron sputtering is 1.5 hours.

[0076] S (3), preparation of the first metal electrode layer 101:

[0077] The substrate sample prepared in the previous step is placed on a mask, and silver (Ag) is evaporated onto the surface of the first transparent electrode layer 102 by evaporation to prepare the first metal electrode layer 101. The thickness of the first metal electrode layer 101 is 200 nm, wherein the vacuum degree of the evaporation method is 2×10 -4 Pa, temperature is 800°C, evaporation rate is 2.5Å / S;

[0078] S (4), preparation of tunneling layer 20:

[0079] A tunneling layer 20 is prepared on the surface of the N-type base doping layer 107, wherein the thickness of the tunneling layer 20 is 40 nm, wherein the power of the magnetron sputtering is 60 W, and the operation time is 1 hour;

[0080] S (5), preparation of hole transport layer 301:

[0081] The tunneling layer 20 is cleaned with an ultraviolet ozone cleaner (UV-Ozone) for 15 minutes, 0.05 mol NiOx powder is dissolved in 1 mL ultrapure water, ultrasonically shaken for 20 minutes, and a hole transport layer dispersion is prepared. The hole transport layer dispersion is ultrasonically shaken for 20 minutes and then uniformly coated on the surface of the tunneling layer 20, and then spin-coated by a spin coating method, and then annealed to prepare the hole transport layer 301, wherein the spin coating speed of the spin coating method is 2000 rpm, the spin coating time is 40 seconds, the spin coating solution amount is 100 ul, the annealing temperature is 450° C., and the annealing time is 30 minutes;

[0082] S (6), preparation of perovskite layer 302:

[0083] Lead iodide and cesium bromide are co-evaporated onto the surface of the hole transport layer 301 to obtain a lead iodide / cesium bromide film L1, and then rubidium fluoride is evaporated onto the surface of the lead iodide / cesium bromide film L1 by evaporation to form an ion diffusion layer L2. Finally, the ammonium salt precursor solution is spin-coated onto the surface of the ion diffusion layer L2 to prepare an ammonium salt film L3 on the surface of the ion diffusion layer L2. After the preparation is completed, annealing is performed to obtain the perovskite layer 302, and the thickness of the perovskite layer 302 is 440 nm. The evaporation rate of lead iodide in the co-evaporation method is 8 A / s, the evaporation rate of lead iodide in the co-evaporation method is 0.8 A / s, the ratio of the evaporation rate of lead iodide in the co-evaporation method to the evaporation rate of lead iodide is 10:1, the evaporation time of the co-evaporation method is 1000 s, and the vacuum degree of the evaporation method is 1×10 -4 Pa, the evaporation temperature is 400°C, the evaporation rate is 0.05Å / S, the thickness of the ion diffusion layer L2 is 1nm, the spin coating speed of the spin coating method is 5000rpm, the spin coating time is 30s, the annealing temperature is 150°C, the annealing time is 10 min, the molar ratio of formamidine iodide (FAI) to formamidine bromide (FABr) in the formamidine iodide (FAI) and formamidine bromide (FABr) solutions is 1:4.7, the formamidine iodide (FAI) and formamidine bromide (FABr) solutions also include additives, the additive is methylammonium chloride (MACl), the mass fraction of the methylammonium chloride (MACl) accounts for 10% of the formamidine iodide (FAI) and formamidine bromide (FABr) solutions, and the concentrations of the formamidine iodide (FAI) and formamidine bromide (FABr) solutions are both 1mol / L;

[0084] S (7), preparation of passivation layer 303:

[0085] The substrate sample prepared in the previous step is placed on the mask, and 3 mg of propylene diamine iodide is evaporated onto the surface of the perovskite layer 302 by evaporation, and annealed to prepare the passivation layer 302. The thickness of the passivation layer 302 is 4 nm, wherein the evaporation vacuum degree is 2×10 -4 Pa, evaporation temperature is 80℃, evaporation rate is 0.1Å / S, annealing temperature is 100℃, and annealing time is 8min;

[0086] S (8), preparation of electron transport layer 304:

[0087] C 60 The electron transport layer 304 is prepared by evaporation to the surface of the passivation layer 303. The thickness of the electron transport layer 304 is 20 nm. The vacuum degree of the evaporation is 1×10 -4 Pa, the evaporation temperature is 200 °C, and the evaporation rate is 0.1 Å / S;

[0088] S (9), preparation of buffer layer 305:

[0089] SnO 2 The buffer layer 305 is prepared by atomic layer deposition on the surface of the electron transport layer 304 using an atomic layer deposition device. The thickness of the buffer layer 305 is 15 nm. The vacuum degree of the deposition is 0.5×10 4 Pa, the temperature of the deposition pipeline is 70°C, and the temperature of the deposition chamber is 60°C;

[0090] S (10), preparation of the second transparent electrode layer 306:

[0091] The second transparent electrode layer 306 is prepared on the surface of the buffer layer 305 by magnetron sputtering, and the thickness of the second transparent electrode layer 306 is 100 nm, wherein the target material of the magnetron sputtering method is indium tin oxide (ITO), the power of the magnetron sputtering method is 50 W, and the operation time of the magnetron sputtering method is 1 hour;

[0092] S (11), preparation of the second metal electrode layer 307:

[0093] The substrate sample prepared in the previous step is placed on the mask, and silver (Ag) is evaporated on the surface of the second transparent electrode layer 306 by evaporation to prepare the second metal electrode layer 307. The thickness of the second metal electrode layer 307 is 100 nm, wherein the vacuum degree of the evaporation is 2×10 -4 Pa, temperature is 800°C, evaporation rate is 0.1Å / S;

[0094] S (12), preparation of anti-reflection layer 308:

[0095] The substrate sample prepared in the previous step is placed on the mask, and magnesium fluoride is evaporated onto the surface of the second metal electrode layer 307 by evaporation, and annealed to prepare the anti-reflection layer 308. The thickness of the anti-reflection layer 308 is 100 nm. The vacuum degree of the evaporation is 2×10 -4 Pa, the evaporation temperature is 80°C, the evaporation rate is 2Å / S, the annealing temperature is 100°C, and the annealing time is 8min to obtain a stacked solar cell.

[0096] Example 2

[0097] The preparation process of the stacked solar cell in this embodiment is the same as that in Embodiment 2, except that the thickness of the ion diffusion layer L2 in this embodiment is 2 nm.

[0098] Example 3

[0099] The preparation process of the stacked solar cell in this embodiment is the same as that in Embodiment 2, except that the thickness of the ion diffusion layer L2 in this embodiment is 3 nm.

[0100] Comparative Example 1

[0101] The preparation method of the stacked solar cell in this comparative example is basically the same as that in Example 2, except that the preparation process of the perovskite layer in this comparative example is:

[0102] Lead iodide and cesium bromide are evaporated to the surface of the hole transport layer by co-evaporation, and a lead iodide / cesium bromide film is prepared on the surface of the hole transport layer. The ammonium salt precursor solution is then coated on the surface of the lead iodide / cesium bromide film by spin coating, and an ammonium salt film is prepared on the surface of the lead iodide / cesium bromide film. After the preparation is completed, the perovskite layer is annealed to obtain a perovskite layer having a thickness of 400 nm. The evaporation rate of lead iodide in the co-evaporation method is 8 A / s, the evaporation rate of lead iodide in the co-evaporation method is 0.8 A / s, the ratio of the evaporation rate of lead iodide in the co-evaporation method to the evaporation rate of lead iodide is 10:1, the evaporation time of the co-evaporation method is 1000 s, the spin coating speed of the spin coating method is 5000 rpm, the spin coating time is 30 s, the annealing temperature is 150° C., and the annealing time is 10 min, the molar ratio of formamidine iodide (FAI) and formamidine bromide (FABr) in the formamidine iodide (FAI) and formamidine bromide (FABr) solutions is 1:4.7, the formamidine iodide (FAI) and formamidine bromide (FABr) solutions also include an additive, the additive is methylammonium chloride (MACl), the mass fraction of the methylammonium chloride (MACl) accounts for 10% of the formamidine iodide (FAI) and formamidine bromide (FABr) solutions, and the concentrations of the formamidine iodide (FAI) and formamidine bromide (FABr) solutions are both 1 mol / L.

[0103] The laminated solar cells obtained in Examples 1-3 and Comparative Example 1 were tested under the following test conditions: a standard solar intensity calibration was performed using a solar simulator, and a solar cell with an area of ​​1.0 cm 2 The device of the embodiment is subjected to long-term IV test, with the starting voltage set to 1.95V, the cut-off voltage set to 0V, the range set to 100mA, and the result is rounded to two decimal places. The test results are shown in Table 1 below.

[0104] Table 1 shows the performance of the stacked solar cells in Examples 1-3 and Comparative Example 1

[0105] Photoelectric conversion efficiency (%) Open circuit voltage (V) <![CDATA[Short-circuit current density (mA / cm 2 ).]]> Decay rate (% / year) Example 1 29.08 1.92 21.01 0.7 Example 2 30.12 1.95 21.04 0.5 Example 3 28.06 1.83 20.88 1.4 Comparative Example 1 26.08 1.74 18.14 4.8

[0106] As shown in Table 1, the performance of the stacked solar cells described in Examples 1-3 and Comparative Example 1 is shown, wherein the stacked solar cells in Examples 1-3 have high photoelectric conversion efficiency and low attenuation rate. This embodiment introduces the preparation of an ion diffusion layer in the traditional two-step method. The ion radius of the ion diffusion molecule is smaller than the perovskite lattice radius, and it can diffuse freely inside the film, effectively promoting the formation of perovskite crystals and improving the quality of the generated film. The device prepared by this method has better performance and stability, wherein the effect is best when the thickness of the ion diffusion layer is set to 2nm, which is reflected in the photoelectric conversion efficiency, open circuit voltage and short circuit current density of the device obtained in Example 2, and has a lower attenuation rate. In contrast, the perovskite layer in Comparative Example 1 is prepared only by a two-step method, and its photoelectric conversion efficiency is low, and the attenuation rate is significantly improved.

[0107] The above embodiments are only preferred implementation modes of the present invention. It should be pointed out that for ordinary technicians in this technical field, various changes, modifications, substitutions and deformations can be made to these embodiments without departing from the principles of the present invention. These technical solutions that are equivalent to the claims of the present invention all fall within the protection scope of the present invention, and the protection scope of the present invention is limited by the attached claims and their equivalents.

Claims

1. A method for preparing a perovskite layer, characterized in that: The preparation method comprises the following steps: S1, providing a battery substrate, and co-evaporating lead iodide and cesium bromide onto the surface of the battery substrate by a co-evaporation method to obtain a lead iodide / cesium bromide thin film; S2, on the surface of the lead iodide / cesium bromide film in S1, evaporating an ion diffusion material by an evaporation method to obtain an ion diffusion layer; S3. Spin-coating the surface of the ion diffusion layer in S2 with an ammonium salt precursor solution, followed by annealing to obtain the perovskite layer.

2. The method for preparing a perovskite layer according to claim 1, characterized in that: The battery substrate comprises a crystalline silicon bottom battery, a tunneling layer and a hole transport layer in sequence from bottom to top, and the lead iodide / cesium bromide film is disposed on the surface of the hole transport layer.

3. The method for preparing a perovskite layer according to claim 1, characterized in that: The ratio of the evaporation rate of lead iodide in the co-evaporation method to the evaporation rate of the lead iodide is (2:1)-(10:1).

4. The method for preparing a perovskite layer according to claim 1, characterized in that: The ion diffusion material in step S2 is one or more of rubidium fluoride (RbF), potassium fluoride (KF), sodium fluoride (NaF), rubidium chloride (RbCl), potassium chloride (KCl), and sodium chloride (NACl).

5. The method for preparing a perovskite layer according to claim 1, characterized in that: The vacuum degree of the evaporation method in step S2 is 1×10 -4 -5×10 -4 Pa, the evaporation temperature is 50-400℃, and the evaporation rate is 0.05-1Å / S.

6. The method for preparing a perovskite layer according to claim 1, characterized in that: The thickness of the ion diffusion layer in step S2 is 1-100 nm.

7. The method for preparing a perovskite layer according to claim 1, characterized in that: The ammonium salt precursor solution in step S3 is a mixed solution of formamidine iodide (FAI) and formamidine bromide (FABr).

8. The method for preparing a perovskite layer according to claim 1, characterized in that: The annealing temperature in step S3 is 50-150° C., and the annealing time is 5-40 min.

9. A stacked solar cell, characterized in that: It comprises a crystalline silicon bottom cell, a tunneling layer and a perovskite top cell, wherein the perovskite top cell comprises a hole transport layer, a perovskite layer, an electron transport layer, a second transparent electrode layer, a second metal electrode layer and an anti-reflection layer, and the perovskite layer is prepared by the perovskite preparation method according to any one of claims 1 to 8.

10. A method for preparing the laminated solar cell according to claim 9, characterized in that: The following steps are involved: Providing a textured crystalline silicon substrate, preparing a base passivation layer on the back of the textured crystalline silicon substrate, preparing a P-type base doping layer on the surface of the base passivation layer, preparing a first transparent electrode layer on the surface of the P-type base doping layer, and preparing a first metal electrode layer on the surface of the first transparent electrode layer; And a substrate surface passivation layer is prepared on the surface of the velvet crystalline silicon substrate, an N-type substrate doping layer is prepared on the surface of the substrate surface passivation layer, a tunneling layer is prepared on the surface of the N-type substrate doping layer, a hole transport layer is prepared on the surface of the tunneling layer, a perovskite layer is prepared on the surface of the hole transport layer, a passivation layer is prepared on the surface of the perovskite layer, an electron transport layer is prepared on the surface of the passivation layer, a buffer layer is prepared on the surface of the electron transport layer, a second transparent electrode layer is prepared on the surface of the buffer layer, a second metal electrode layer is prepared on the surface of the second transparent electrode layer, and an anti-reflection layer is prepared on the surface of the second metal electrode layer.

Citation Information

Patent Citations

  • Spectral gradient filter, preparation method thereof and diffusion exchange reaction mold

    CN118259391A

  • Perovskite layer of trihalide, perovskite unijunction solar cell, perovskite silicon laminated solar cell and preparation methods of perovskite layer, perovskite unijunction solar cell and perovskite silicon laminated solar cell

    CN118317662A

  • Method for preparing perovskite thin film through heat dissipation and laminated solar cell

    CN118475202A

Cited By

  • Perovskite thin film preparation method and solar cell

    CN119300680A

  • Perovskite thin film gas passivation method and laminated solar cell

    CN119403414A

  • Perovskite thin film gas passivation method and laminated solar cell

    CN119421621A

  • Laminated cell, preparation method thereof, cell preparation device and photovoltaic module

    CN121815890A

  • Method for preparing perovskite layer, tandem solar cell, and preparation method

    WO2026066490A1