Perovskite solar cell prepared based on perovskite surface defect in-situ etching reconstruction and preparation method and application thereof

Through the in-situ etching and reconstruction method of perovskite surface defects, the problem of difficult to optimize the film quality of perovskite solar cells is solved, the battery performance and stability are improved, and the efficient and low-cost perovskite solar cell preparation is achieved. , has promoted the industrialization process of perovskite solar cells.

CN118890943APending Publication Date: 2024-11-01SHANDONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410876949.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The quality of perovskite solar cells is difficult to optimize universally, resulting in poor performance and poor stability, hindering the preparation and application of perovskite solar cells.

Method used

Using an in-situ etching and reconstruction method based on perovskite surface defects, the shallow defect removal and recrystallization are formed by using a suitable etching agent such as ethyl methacrylate on a perovskite film to form high-quality pertituitine Ore film.

Benefits of technology

It improves the photoelectric conversion efficiency and stability of perovskite solar cells, reduces the defect state density, realizes perovskite solar cells with low cost, high environmental stability and high performance, and promotes the industrialization process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118890943A_ABST
    Figure CN118890943A_ABST
Patent Text Reader

Abstract

The invention discloses a perovskite solar cell prepared based on perovskite surface defect in-situ etching reconstruction and a preparation method and application thereof. The preparation method specifically comprises the following steps: in the preparation process of the perovskite solar cell, immersing a perovskite thin film into a weak-polarity solvent, dissolving surface defects of the perovskite thin film due to the interaction relationship between the perovskite thin film and the solvent, and realizing in-situ recrystallization under a heating condition to obtain the perovskite solar cell. Therefore, defects generated in the preparation process are eliminated, a high-quality perovskite thin film is obtained, and a high-performance perovskite solar cell is prepared. The solvent in-situ etching recrystallization process adopted in the method is easy to operate, low in cost, high in controllability, wide in application range, capable of treating a large-area perovskite thin film and capable of being widely applied to the perovskite industrialization process; the perovskite solar cell prepared by the method is high in efficiency and good in stability, and the commercialization process of the perovskite solar cell can be accelerated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the fields of new material technology and new energy technology, and specifically relates to a perovskite solar cell prepared based on in-situ etching and reconstruction of perovskite surface defects, and a preparation method and application thereof. Background Art

[0002] In the field of photovoltaic technology, perovskite solar cells have attracted widespread attention due to their outstanding energy conversion efficiency, low cost, and easy preparation. Perovskite materials can not only be used as light absorption layers, but also as electron and hole transport layers, from which perovskite solar cells with different structures can be prepared, which is one of the important development directions of new thin-film solar cells. In recent years, the preparation process of perovskites and the efficiency of cells have achieved rapid development. Despite this, the quality of perovskite thin films is still one of the problems that restrict battery performance.

[0003] In recent years, researchers have mostly optimized the quality of perovskite films by using specific additives to improve the photoelectric conversion efficiency and device stability of perovskite solar cells. However, due to the diversity of perovskite films, it is difficult to use a universal method to optimize the quality of the films, which has hindered the preparation and application of perovskite solar cells. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a perovskite solar cell prepared based on in-situ etching and reconstruction of perovskite surface defects, and a preparation method and application thereof. The present invention can solve the problems of poor performance and poor stability of perovskite solar cells in the prior art, and obtain high-efficiency and high-stability perovskite solar cells through process design and optimization. Moreover, the preparation method of the perovskite solar cell of the present invention has the advantages of good environmental stability, high performance, low cost and wide application range, and has important theoretical significance and practical value.

[0005] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions: The present invention proposes a method for preparing a perovskite solar cell based on in-situ etching and reconstruction of perovskite surface defects, comprising the following steps: (1) pattern etching, cleaning, and surface plasma treatment of a transparent conductive glass substrate, and constructing a charge transfer layer on the cleaned conductive glass substrate; (2) preparing a perovskite precursor solution; (3) Spin coating or scraping the perovskite precursor solution onto the surface of the charge transport layer to form a film, followed by annealing to obtain a high-quality perovskite film; (4) immersing the perovskite film prepared in step (3) in an etching solvent and heating it for a certain period of time; (5) The perovskite film obtained in step (4) is repeatedly rinsed with isopropanol, and then the residual isopropanol is volatilized by heating to obtain a perovskite film with surface defects in situ etched.

[0006] Furthermore, the conductive glass substrate in step (1) is FTO or ITO, and the charge transport layer includes TiO2, SnO2 and NiO x .

[0007] Furthermore, the perovskite component in the perovskite precursor solution in step (2) is (FAMACs)Pb(IBr)3, and its concentration is 0.7-1.5 mol / L.

[0008] Furthermore, in the step (3), the annealing temperature is 100 to 300 degrees Celsius, and the annealing time is 1 to 60 minutes.

[0009] Furthermore, the etching solvent in step (4) is a weak polar solvent, including but not limited to methyl methacrylate, ethyl methacrylate, butyl methacrylate, and pentyl methacrylate.

[0010] Furthermore, in step (4), the etching temperature is 50 to 150 degrees Celsius and the etching time is 1 to 15 minutes.

[0011] Furthermore, in step (5), the heating temperature is 100 to 300 degrees Celsius, and the heating time is 1 to 20 minutes.

[0012] Furthermore, the thickness of the perovskite film obtained in step (5) is 300 to 600 nanometers.

[0013] The present invention also provides a perovskite solar cell, which is obtained by constructing a charge transfer layer and an electrode on the perovskite film. The structure of the cell includes a formal, a transverse and a carbon electrode.

[0014] Furthermore, the perovskite solar cell has an open circuit voltage of 1.1 to 1.4 V and a short circuit current of 14 to 26 mA·cm -2 , filling factor is 0.7~0.85, and photoelectric conversion efficiency is 14~25%.

[0015] The present invention also provides the use of the perovskite solar cell in preparing photovoltaic cells, battery components or building power stations.

[0016] Compared with the prior art, the advantages and technical effects of the present invention are: 1. The present invention comprehensively considers the specific polarity, boiling point, volatility, cost and other requirements of the etchant, and finally selects ethyl methacrylate as the etchant through a large number of experiments. Ethyl methacrylate has moderate etching ability for perovskite, and can etch away shallow defects of perovskite film without destroying deep perovskite, laying a foundation for the preparation of high-efficiency batteries; it accelerates the industrialization process of perovskite solar cells, and has important practical and economic value.

[0017] 2. The present invention prepares a high-quality perovskite film by soaking the perovskite film in ethyl methacrylate to etch away shallow defects and simultaneously perform in-situ recrystallization. The method has low cost, simple operation, high efficiency and good repeatability. Compared with the untreated perovskite film, the perovskite film after etching and recrystallization has a smoother morphology, better quality and higher environmental stability. The defect state density is reduced, which is beneficial to improving the efficiency of battery devices.

[0018] 3. The etching and recrystallization method of the present invention has a wide application range and is applicable to all battery devices with a perovskite layer.

[0019] By utilizing the technical solution of the present invention, high-quality perovskite films can be prepared, thereby obtaining perovskite solar cells with low cost, good environmental stability and high performance, thereby accelerating the industrialization process of perovskite solar cells, and therefore has important practical and economic value. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the efficiency curve of the all-inorganic CsPbI2Br perovskite solar cell prepared by the present invention.

[0021] Figure 2 The SEM images of the untreated and all-inorganic CsPbI2Br perovskite films prepared in the present invention are shown in FIG.

[0022] Figure 3 The photovoltaic performance diagram of the battery prepared in Examples 1-3. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.

[0024] The present invention comprehensively considers the requirements of the etchant such as polarity, boiling point, volatility, cost, etc., and selects ethyl methacrylate as the etchant; the ethyl methacrylate used in the present invention can dissolve and etch the shallow defect state part of the perovskite film, and simultaneously perform in-situ recrystallization, thereby achieving quality improvement of the CsPbI2Br perovskite film. Example 1

[0025] The method for preparing a perovskite solar cell based on in-situ etching and reconstruction of perovskite surface defects in this embodiment comprises the following steps: 1. Use hydrochloric acid and zinc powder to etch the FTO conductive glass into the required pattern; 2. Add 7 mL of isopropyl titanate to 2-3 mL of diethanolamine, dilute to 50 mL with anhydrous ethanol, and ultrasonicate for 20-40 minutes to prepare a titanium dioxide precursor solution; 3. Take 80 μl of the solution in step 2 and spin-coat it onto the FTO substrate in step 1, then calcine it at 500 degrees Celsius in a muffle furnace for 60 minutes, and take it out after cooling to room temperature; 4. Add 277 mg PbI2, 312 mg CsI, 220 mg PbBr2, and 5 mg MACl to 1 mL DMSO to prepare a 1.0 mol / L perovskite precursor solution. Dissolve it in a water bath ultrasound for 30 minutes and filter it with a filter to prepare a CsPbI2Br precursor solution. 5. Take 80 μl of the CsPbI2Br perovskite precursor solution prepared in step 4 and spin-coat it on the titanium dioxide film obtained in step 3, then heat it at 160 degrees Celsius for 5 minutes in an air environment, and then heat it at 270 degrees Celsius for 10 minutes to form a CsPbI2Br perovskite film; 6. Place the CsPbI2Br perovskite film prepared in step 5 into 20 mL of preheated ethyl methacrylate and heat in a water bath at 80 degrees Celsius for 3 minutes; Figure 2 The SEM images of the perovskite film before and after treatment show that the grain size of the perovskite film has increased significantly, and the quality and crystallinity of the perovskite film have improved after surface etching and recrystallization.

[0026] 7. The etched CsPbI2Br perovskite film obtained in step 6 was repeatedly rinsed with isopropanol, and then heated at 120 degrees Celsius for 3 minutes to volatilize the residual isopropanol; 8. Scrape the carbon slurry on the surface of the CsPbI2Br perovskite layer prepared in step 7, then heat and dry it at 200 degrees Celsius for 10 minutes to assemble the perovskite CsPbI2Br solar cell. Example 2

[0027] The method for preparing a perovskite solar cell based on in-situ etching and reconstruction of perovskite surface defects in this embodiment comprises the following steps: 1. Use hydrochloric acid and zinc powder to etch the FTO conductive glass into the required pattern; 2. Add 8 mL of isopropyl titanate to 2-3 mL of diethanolamine, dilute to 50 mL with anhydrous ethanol, and ultrasonicate for 20-40 minutes to prepare a titanium dioxide precursor solution; 3. Take 80 μl of the solution in step 2 and spin-coat it on the FTO substrate, then calcine it at 500 degrees Celsius in a muffle furnace for 60 minutes, and take it out after cooling to room temperature; 4. Add 194 mg PbI2, 218.5 mg CsI, 154 mg PbBr2, and 3.5 mg MACl to 1 mL DMSO to prepare a perovskite precursor solution with a concentration of 0.7 mol / L. Dissolve it in a water bath ultrasound for 30 minutes and filter it with a filter to prepare a CsPbI2Br precursor solution. 5. Take 80 μl of the CsPbI2Br perovskite precursor solution prepared in step 4 and spin-coat it on the titanium dioxide film obtained in step 3, then heat it at 180 degrees Celsius for 2 minutes in an air environment, and then heat it at 270 degrees Celsius for 10 minutes to form a CsPbI2Br perovskite film; 6. Place the CsPbI2Br perovskite film prepared in step 5 into 20 mL of preheated methyl methacrylate and heat in a water bath at 80 degrees Celsius for 1 minute; 7. The etched CsPbI2Br perovskite film obtained in step 6 was repeatedly rinsed with isopropanol, and then heated at 120 degrees Celsius for 3 minutes to volatilize the residual isopropanol; 8. Scrape the carbon slurry on the surface of the CsPbI2Br perovskite layer prepared in step 7, then heat and dry it at 200 degrees Celsius for 10 minutes to assemble the perovskite CsPbI2Br solar cell. Example 3

[0028] The method for preparing a perovskite solar cell based on in-situ etching and reconstruction of perovskite surface defects in this embodiment comprises the following steps: 1. Use hydrochloric acid and zinc powder to etch the FTO conductive glass into the required pattern; 2. Add 8 mL of isopropyl titanate to 2-3 mL of diethanolamine, dilute to 50 mL with anhydrous ethanol, and ultrasonicate for 30 minutes to prepare a titanium dioxide precursor solution; 3. Take 80 μl of the solution in step 2 and spin-coat it on the FTO substrate, then calcine it at 500 degrees Celsius in a muffle furnace for 60 minutes, and take it out after cooling to room temperature; 4. Add 340.5 mg PbI2, 468 mg CsI, 330 mg PbBr2, and 7.5 mg MACl to 1 mL DMSO to prepare a 1.5 mol / L perovskite precursor solution. Dissolve it in a water bath ultrasound for 30 minutes and filter it with a filter to prepare a CsPbI2Br precursor solution. 5. Take 80 μl of the CsPbI2Br perovskite precursor solution prepared in step 4 and spin-coat it on the titanium dioxide film obtained in step 3, then heat it at 200 degrees Celsius in an air environment for 1 minute, and then heat it at 270 degrees Celsius for 10 minutes to form a CsPbI2Br perovskite film; 6. Place the CsPbI2Br perovskite film prepared in step 5 into 20 mL of preheated butyl methacrylate and heat in a water bath at 80 degrees Celsius for 5 minutes; 7. The etched CsPbI2Br perovskite film obtained in step 6 was repeatedly rinsed with isopropanol, and then heated at 120 degrees Celsius for 3 minutes to volatilize the residual isopropanol; 8. Scrape the carbon slurry on the surface of the CsPbI2Br perovskite layer prepared in step 7, then heat and dry it at 200 degrees Celsius for 10 minutes to assemble the perovskite CsPbI2Br solar cell.

[0029] The etchant in step 6 of the present invention is a weak polar solvent. The present invention obtains an open circuit voltage of 1.0-1.6 V and a current density of 10-15 mA·cm -2 , a perovskite solar cell with a fill factor of 0.70 to 0.85 and a photoelectric conversion efficiency of 13 to 16%. The cell was placed in an air environment for two months and its efficiency remained above 90% of the initial value.

[0030] Through Figure 3 The results analysis shows that the fill factor, open circuit voltage and short circuit current density of the battery treated with ethyl methacrylate are improved, and the photoelectric conversion efficiency of the battery is significantly better than that of the battery treated with methyl methacrylate and butyl methacrylate.

[0031] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.

Claims

1. A method for preparing a perovskite solar cell based on in-situ etching and reconstruction of perovskite surface defects, characterized in that: The following steps are involved: (1) pattern etching, cleaning, and surface plasma treatment of a transparent conductive glass substrate, and constructing a charge transfer layer on the cleaned conductive glass substrate; (2) preparing a perovskite precursor solution; (3) Spin coating or scraping the perovskite precursor solution onto the surface of the charge transport layer to form a film, followed by annealing to obtain a high-quality perovskite film; (4) immersing the perovskite film prepared in step (3) in an etching solvent and heating it; (5) The perovskite film obtained in step (4) is repeatedly rinsed with isopropanol, and then the residual isopropanol is volatilized by heating to obtain a perovskite film with surface defects in situ etched.

2. The preparation method according to claim 1, characterized in that: The conductive glass substrate in step (1) is FTO or ITO, and the charge transport layer includes TiO2, SnO2 and NiO x .

3. The preparation method according to claim 1, characterized in that: The perovskite precursor component in step (2) is (FAMACs)Pb(IBr)3, and its concentration is 0.7-1.5 mol / L.

4. The preparation method according to claim 1, characterized in that: In the step (3), the annealing temperature is 100 to 300 degrees Celsius, and the annealing time is 1 to 60 minutes.

5. The preparation method according to claim 1, characterized in that: The etching solvent in step (4) is a weak polar solvent, including at least one of methyl methacrylate, ethyl methacrylate, butyl methacrylate, and pentyl methacrylate.

6. The preparation method according to claim 1, characterized in that: In the step (4), the etching temperature is 50 to 150 degrees Celsius and the etching time is 1 to 15 minutes.

7. The preparation method according to claim 1, characterized in that: The thickness of the perovskite film obtained in step (5) is 300 to 600 nanometers.

8. A perovskite solar cell, characterized in that: The perovskite solar cell is obtained by constructing a charge transfer layer and an electrode on the perovskite film prepared according to claim 1.

9. The perovskite solar cell according to claim 8, characterized in that: The perovskite solar cell has an open circuit voltage of 1.1 to 1.4 V and a short circuit current of 14 to 26 mA·cm -2 , filling factor is 0.7~0.85, and photoelectric conversion efficiency is 14~25%.

10. Use of the perovskite solar cell according to claim 8 in preparing photovoltaic cells, battery modules or building power stations.