Preparation method and application of perovskite thin film
By using a mixed anti-solvent of ammonium salt and halogenated aromatic amine additives in the preparation of perovskite films, the problem that a single anti-solvent cannot improve the film quality is solved, and a high efficiency and high stability perovskite solar cell is achieved, improving the The crystallinity and device performance of perovskite films are achieved.
Patent Information
- Application Number
- CN202410817891.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-01
AI Technical Summary
Single anti-solvent cannot effectively solve the surface roughness and pinhole problems during the preparation of perovskite films, resulting in poor performance of perovskite solar cells and lack of passivator phase defects, affecting device stability.
Using a mixed anti-solvent composed of ammonium salt and halogenated aromatic amine additives, the crystal quality and orientation of the film are optimized to form high crystallinity and high-definition crystal surface orientation by extracting the perovskite precursor solution during the coating process. perovskite film.
The efficiency and stability of perovskite solar cells are significantly improved, and high-efficiency perovskite film preparation is achieved, which improves the cell efficiency and long-term stability of the device.
Smart Images

Figure CN118890946A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to a method for preparing a perovskite film using an anti-solvent and an application thereof. Background Art
[0002] Organic-inorganic hybrid perovskite materials have the advantages of high absorption coefficient, adjustable bandgap, long carrier diffusion length, high defect tolerance, simple preparation process, and low material and preparation costs. They are considered to be the new materials closest to commercialization in the photovoltaic market in recent years. After only more than a decade of research, single-junction perovskite cells have achieved a high photoelectric conversion efficiency, surpassing the currently commercialized cadmium telluride and copper indium gallium selenide cells, and are very close to the mainstream crystalline silicon (26.7%) solar cells in the market. Perovskite tandem solar cells have the advantages of high efficiency and low cost, and are considered to be one of the technologies that are expected to achieve large-scale terrestrial photovoltaic applications. Perovskite tandem cells have gradually become a hot topic in the world's photovoltaic research field in recent years due to their outstanding advantages such as high efficiency, low cost, and simple preparation process.
[0003] Although perovskite solar cells face problems related to the quality of perovskite films, such as rough surface and pinholes (resulting in poor device performance) in the early stages of manufacturing, researchers have developed many technologies to improve the quality of perovskite films. Among these developed technologies, the anti-solvent treatment method is undoubtedly one of the most successful technologies to date. Anti-solvent treatment increases the nuclear density during the film formation process and produces a uniform, pinhole-free perovskite film, which is beneficial to improving the efficiency of solar cells and reducing hysteresis and stability. However, in the preparation process of perovskite films of some components, only anti-solvent treatment can improve the quality of film preparation, but it is impossible to ultimately achieve the preparation of high-quality perovskite films. The present invention optimizes the anti-solvent process for the preparation of perovskite cells by using an anti-solvent with an additive added, thereby improving the efficiency and stability of perovskite solar cells. Summary of the invention
[0004] One of the purposes of the present invention is to provide a perovskite film, wherein the preparation method thereof is to first coat a perovskite precursor solution, extract the perovskite precursor solution with an anti-solvent during the coating process, and then obtain the perovskite film;
[0005] The anti-solvent is composed of a mixed additive and a mixed solvent, and the concentration range of the mixed additive in the mixed solvent is 0.1-10 mg / ml;
[0006] The mixed additive consists of a first additive and a second additive, the weight ratio of the first additive to the second additive is in the range of 1:10-10:1, the first additive is an ammonium salt that can form a stable crystal structure at the A position of the perovskite, selected from halogenated amines, halogenated methylamines, halogenated guanidines and halogenated formamidines, and the second additive is selected from halogenated aromatic amines, halogenated alkylammonium salts and halogenated diamines;
[0007] The mixed solvent consists of a first solvent and a second solvent, the volume ratio of the first solvent to the second solvent is 5%-50%, the first solvent is selected from chlorobenzene, chloroform, o-dichlorobenzene, anisole, toluene, bromobenzene, iodobenzene, ethyl acetate, diethyl ether and ethyl ether, and the second solvent is selected from ethanol, isopropanol and isobutanol.
[0008] Furthermore, the coating is performed by spin coating, spray coating or roll-to-roll coating.
[0009] A second object of the present invention is to provide an application of the above-mentioned perovskite film in the preparation of perovskite solar cells.
[0010] A third object of the present invention is to provide a perovskite solar cell, wherein the perovskite light-absorbing layer of the perovskite solar cell is the above-mentioned perovskite film.
[0011] Furthermore, the perovskite solar cell is a single-junction cell or a stacked cell.
[0012] In the present invention, the single junction cell comprises, from bottom to top, a transparent conductive layer, a first carrier transport layer, a perovskite light absorption layer, a second carrier transport layer and a top electrode;
[0013] The stacked battery includes, from bottom to top, a transparent conductive layer, a first carrier transport layer, a first perovskite light absorption layer, a second carrier transport layer, a tunneling composite layer, a third carrier transport layer, a second perovskite light absorption layer, a fourth carrier transport layer and a top electrode.
[0014] In the present invention, the transparent conductive layer may be an indium tin oxide (ITO) substrate, a fluorine-doped tin oxide (FTO) substrate, an indium zinc oxide (IZO) substrate, or the like.
[0015] In the present invention, the carrier transport layer is a hole transport layer or an electron transport layer.
[0016] The hole transport layer uses inorganic transport materials such as nickel oxide (NiO), cuprous oxide (Cu2O), molybdenum oxide (MoO3), copper iodide (CuI), and redox graphene, poly [bis (4-phenyl) (2,4,6-trimethylphenyl) amine] (PTAA, poly (triaryl amine)), 2,2',7,7'-tetrakis [N,N-di (4-methoxyphenyl) amino] -9,9'-spirobifluorene (Spiro-OMeTAD), poly 3,4-ethylenedioxythiophene: polystyrene sulfonate (PEDOT:PSS), poly [bis (4-phenyl) (4-butylphenyl) amine] (Ploy-TPD), [2- (9H-carbazole-9-yl) ethyl] phosphonic acid, [2- (3,6-dimethoxy-9H-carbazole-9-yl) ethyl] phosphonic acid and one or more organic p-type semiconductor materials.
[0017] The electron transport layer is made of titanium oxide (TiO2), tin oxide (SnO2), zinc oxide (ZnO), fullerene (C 60 ), graphene, fullerene derivatives (PCBM) and other one or more n-type semiconductor materials, the electron transport layer can be prepared by deposition methods including but not limited to electron beam evaporation, thermal evaporation, magnetron sputtering, atomic layer deposition, spin coating, scraping and the like.
[0018] In the present invention, the top electrode is made of gold, palladium, silver, titanium, chromium, nickel, aluminum, copper, indium tin oxide (ITO), indium zinc oxide (IZO) and the like.
[0019] In view of the current technical problem that a single anti-solvent cannot passivate bulk phase defects, the present invention improves the anti-solvent process by utilizing the additives in the anti-solvent to penetrate into the bulk phase during dripping, which can effectively improve the crystallization quality of the thin film, enhance the film orientation, passivate bulk phase defects, and achieve the preparation of perovskite films with high crystallinity and high preferred crystal plane orientation, thereby enhancing the performance of perovskite solar cells and improving the stability of the device.
[0020] Compared with the traditional single anti-solvent, the additive anti-solvent used in the present invention has the following advantages: 1) improving the crystallization quality of the film and enhancing the film orientation; 2) passivating the bulk defects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the structure of the perovskite solar cell of Example 1.
[0022] Figure 2 The crystallization performance diagram of the perovskite film of Example 1
[0023] Figure 3 This is a graph showing the effect of different additive ratios in antisolvents on device efficiency.
[0024] Figure 4 1 is the cell efficiency curve of the perovskite solar cell obtained in the embodiment and the comparative example. DETAILED DESCRIPTION
[0025] The preferred embodiments of the present invention will be described in detail below in conjunction with examples. It should be understood that the following examples are provided only for the purpose of illustration and are not intended to limit the scope of the present invention. Those skilled in the art may make various modifications and substitutions to the present invention without departing from the purpose and spirit of the present invention.
[0026] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0027] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0028] Example 1
[0029] The structure of the perovskite solar cell of this embodiment is as follows Figure 1 As shown, the preparation process is as follows:
[0030] 1. Place the ITO substrate in an ultrasonic cleaning box and clean it for 20 minutes;
[0031] 2. Depositing a layer of [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid as a hole transport layer on the cleaned ITO substrate;
[0032] 2. Deposition of FA on the hole transport layer 0.8 Cs 0.2 Pb(I 0.6 Br 0.4 )3 perovskite, during the last ten seconds of spin coating, an anti-solvent (mixture of anisole and isopropanol in a ratio of 10:1) with 3,4-dimethylphenylethylamine hydroiodide (3,4ME-PEAI) and methylamine iodide (MAI) was added dropwise;
[0033] 3. The perovskite after the rotation is placed on a hot plate at 100°C for annealing, and the thickness of the perovskite layer is about 500nm;
[0034] Meanwhile, the antisolvent without additives was used as blank, and the addition of single additive 3,4ME-PEAI or methylamine iodide (MAI) was used as control;
[0035] 4. Use thermal evaporation to deposit a layer of fullerene (C 60 ) as an electron transport layer with a thickness of about 25nm; a layer of tin dioxide (SnO2) is deposited by atomic layer as a hole blocking transport layer with a thickness of about 20nm;
[0036] 5. Use thermal evaporation to deposit a layer of metallic copper as an electrode.
[0037] The crystallinity of perovskite films changes as Figure 2 As shown in the X-ray diffraction pattern, the perovskite film treated with a mixed cationic antisolvent has a higher crystal strength and a higher (100) crystal plane orientation than the film treated with a single additive 3,4ME-PEAI and methylamine iodide (MAI). The (100) crystal plane has a lower defect state density and a higher carrier mobility in the perovskite material. The improvement of the (100) crystal plane orientation plays a vital role in improving the photovoltaic performance of the perovskite material. Figure 2 The performance test of the film with "3,4ME-PEAI and MAI anti-solvent added" corresponds to the 5th experiment in the table below, achieving an efficiency of 20.09%. Figure 4 The JV curve performance of "addition of anti-solvent of 3,4ME-PEAI and MAI" also corresponds to the 5th group of experiments in the following table.
[0038] The device prepared above was subjected to performance testing, and the results are as follows:
[0039]
[0040] As can be seen from the table above, the preparation of perovskite solar cells after introducing additives into anti-solvents can effectively improve the cell efficiency of the device; when using anti-solvent treatment with mixed additives, an efficiency of 20.09% was achieved on a single-junction cell, the cell efficiency when introducing one additive was 19.25%, and the efficiency when using a single anti-solvent treatment was 18.88%.
[0041] 6. The volume ratio of the mixed solvent in the additive to the total solvent is selected as the mixed solvent, which is a solution formed by dissolving 3,4ME-PEAI 1 mg / mL and MAI 2 mg / mL in IPA, which is solution A, and the anisole solution is solution B. Figure 3 The volume ratio obtained by A / (A+B) solution is shown. From the device efficiency results, it can be seen that when the volume ratio is in the range of 10%-50%, the efficiency of the perovskite device is significantly improved.
Claims
1. A perovskite film, characterized in that: The method for preparing the perovskite film comprises: first coating a perovskite precursor solution, extracting the perovskite precursor solution with an anti-solvent during the coating process, and then obtaining the perovskite film; The anti-solvent is composed of a mixed additive and a mixed solvent, and the concentration range of the mixed additive in the mixed solvent is 0.1-10 mg / ml; The mixed additive consists of a first additive and a second additive, and the weight ratio of the first additive to the second additive is in the range of 1:10-10:1; the first additive is an ammonium salt that forms a stable crystal structure at the A position of the perovskite, selected from halogenated amines, halogenated methylamines, halogenated guanidines and halogenated formamidines, and the second additive is selected from halogenated aromatic amines, halogenated alkylammonium salts and halogenated diamines; The mixed solvent consists of a first solvent and a second solvent, the volume ratio of the first solvent to the second solvent is 5%-50%, the first solvent is selected from chlorobenzene, chloroform, o-dichlorobenzene, anisole, toluene, bromobenzene, iodobenzene, ethyl acetate, diethyl ether and ethyl ether, and the second solvent is selected from ethanol, isopropanol and isobutanol.
2. The perovskite film according to claim 1, characterized in that The coating is performed by spin coating, spray coating or roll-to-roll coating.
3. Use of the perovskite film according to claim 1 in the preparation of perovskite solar cells.
4. The use according to claim 3, characterized in that: The perovskite solar cell is a single-junction cell or a stacked cell.
5. A perovskite solar cell, characterized in that: The perovskite light-absorbing layer of the perovskite solar cell is the above-mentioned perovskite film.
6. The perovskite solar cell according to claim 5, characterized in that: The perovskite solar cell is a single-junction cell or a stacked cell.