Polydentate phosphite ligands, catalytic compositions containing such ligands, and catalytic processes utilizing such catalytic compositions
By using a catalyst complex formed by a multidentate phosphite ligand and nickel, the problem of insufficient efficiency and selectivity of existing catalysts in hydrocyanation and isomerization reactions is solved, and an efficient and stable catalytic effect is achieved. Suitable for the production of important compounds.
Patent Information
- Application Number
- CN202380028318.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-13
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-01
AI Technical Summary
Existing phosphorus ligand catalysts have insufficient efficiency and selectivity in commercially important reactions, especially in hydrocyanation and isomerization reactions, making it difficult to achieve rapid, stable and high-performance catalytic effects.
Using polydentate phosphite ligands to form catalyst complexes with transition metals, the reaction with olefins and hydrogen cyanide can achieve efficient hydrocyanation and isomerization reactions, including the use of nickel as a transition metal, in combination with specific Polydentate phosphite ligand and Lewis acid promoter.
It significantly improves the selectivity and efficiency of the catalyst, can complete the reaction in a short time, improves the yield and purity of the product, and is suitable for the preparation of important compounds such as adipiconet.
Smart Images

Figure CN118891102A_ABST
Abstract
Description
[0001] Citation of Related Applications
[0002] This application claims the benefit of U.S. Provisional Application No. 63 / 344,760, filed May 23, 2022, and UK Application No. 2215118.7, filed October 13, 2022. The entire contents of these applications are incorporated herein by reference in their entirety. Technical Field
[0003] The present application relates to multidentate phosphite ligands, catalytic compositions containing such ligands, and catalytic methods utilizing such catalytic compositions. Background Art
[0004] Phosphorus ligands are ubiquitous in catalysis and are used for many commercially important chemical conversions. Phosphorus ligands that are usually encountered in catalysis include phosphine (A) and phosphite (B), as shown below. In these representations, R can actually be any organic group. Monophosphine and monophosphite ligands are compounds containing a single phosphorus atom used as a metal donor. Diphosphine, diphosphite and bis(phosphorus) ligands usually contain two phosphorus atoms and usually form a cyclic chelate structure with transition metals.
[0005]
[0006] There are several commercially important catalytic processes that employ phosphorus ligands. For example, U.S. Pat. No. 5,910,600 to Urata et al. discloses that bisphosphite compounds can be used as constituent elements of homogeneous metal catalysts for various reactions such as hydrogenation, hydroformylation, hydrocyanation, hydrocarboxylation, hydroamidation, hydroesterification, and aldol condensation.
[0007] Some of these catalytic processes are used for the commercial production of polymers, solvents, plasticizers and other commodity chemicals. For example, the hydrocyanation of 1,3-butadiene and / or 3-pentenenitrile is a known approach to produce adiponitrile, which is a precursor for producing nylon-6,6. Therefore, due to the huge global chemical commodity market, in any of these commercially important reactions, even small incremental improvements in yield or selectivity are highly desirable. In addition, it is also highly desirable to find certain ligands that can be used for applications across a series of these commercially important reactions, not only for commercial benefit, but also in order to be able to merge and focus on a specific group of compounds with research and development efforts.
[0008] U.S. Pat. No. 5,512,696 to Kreutzer et al. discloses a hydrocyanation process using a multidentate phosphite ligand, and the patents and publications cited therein describe a hydrocyanation catalyst system using zero-valent nickel and a multidentate phosphite ligand, which pertains to the hydrocyanation of olefinically unsaturated compounds. U.S. Pat. Nos. 5,723,641, 5,663,369, 5,688,986, and 5,847,191 disclose a process and catalyst composition for the hydrocyanation of monoolefinically unsaturated compounds using zero-valent nickel and a multidentate phosphite ligand and a Lewis acid co-promoter.
[0009] U.S. Pat. No. 5,821,378 to Foo et al. discloses a liquid phase process for hydrocyanating diene compounds to produce non-conjugated acyclic nitriles and a liquid phase process for isomerizing those nitriles to 3-monoolefin linear nitriles and / or 4-monoolefin linear nitriles, wherein the reaction is carried out in the presence of zero-valent nickel and a multidentate phosphite ligand. Other catalytic methods for hydrocyanating olefins and isomerizing monoolefin nitriles are described in the patents and publications cited therein. Published International Application WO99 / 06357 discloses a multidentate phosphite ligand having an alkyl ether substituent on the carbon ortho to the terminal phenol group, which is used in a liquid phase process for hydrocyanating diene compounds to produce non-conjugated acyclic nitriles and a liquid phase process for isomerizing those nitriles to 3-monoolefin linear nitriles and / or 4-monoolefin linear nitriles.
[0010] Although the above-described catalyst systems may represent commercially viable catalysts, it is still desirable to provide even more effective, higher performing catalyst precursor compositions, catalytic compositions, and catalytic methods to achieve the full commercial potential of desired reactions. Effectiveness and / or performance may be achieved in terms of any or all of rapidity, selectivity, efficiency, or stability, depending on the reaction being performed. It is also desirable to provide improved catalyst systems and / or methods that can be optimized for one or more commercially important reactions such as hydroformylation, hydrocyanation, or isomerization. Summary of the invention
[0011] In one aspect, the present application provides a multidentate phosphite ligand comprising a catkin skeleton in which iptycene is optionally substituted with one or more C1 to C4 alkyl substituents and at least two aryl phosphite groups chemically bonded to the skeleton, wherein the catkin skeleton comprises two aromatic hydrocarbon groups attached to a bicyclooctatriene core of the skeleton, and each aryl phosphite group is chemically bonded to a different carbon atom of the core via an oxygen atom, or each aryl phosphite group is chemically bonded to a different C1 to C4 alkyl substituent of the core via an oxygen atom; or wherein the catkin skeleton comprises three aromatic hydrocarbon groups attached to a bicyclooctatriene core of the skeleton, and each aryl phosphite group is chemically bonded to a carbon atom of a different aromatic hydrocarbon group of catkin via an oxygen atom, and the aryl groups of the aryl phosphite groups are not chemically bonded to each other.
[0012] In another aspect, the present application provides a multidentate phosphite ligand having one of the following structures:
[0013]
[0014]
[0015] In other aspects, the present application provides a catalyst complex comprising a multidentate phosphite ligand as described herein and at least one transition metal.
[0016] In yet another aspect, the present application provides a method for hydrocyanating an organic compound containing at least one olefinic group, comprising reacting the organic compound with hydrogen cyanide in the presence of a catalyst complex as described herein.
[0017] In still another aspect, the present application provides a process for isomerizing a monoethylenically unsaturated compound, wherein the compound is contacted with a catalyst complex. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a simplified block diagram of an integrated process for producing adiponitrile according to one embodiment of the present disclosure, the integrated process including the steps of hydrocyanating 1,3-butadiene, isomerizing 2-methyl-3-butenenitrile, and hydrocyanating 3-pentenenitrile. DETAILED DESCRIPTION
[0019] Novel multidentate phosphite ligands and catalyst complexes comprising multidentate phosphite ligands and at least one transition metal are described herein. Catalytic processes using the catalyst complexes are also described, such as the hydrocyanation of organic compounds (particularly 1,3-butadiene and 3-pentenenitrile) containing at least one olefinic group, and the double bond isomerization of monoolefinic unsaturated compounds (such as 2-methyl-3-butenenitrile).
[0020] many Dental phosphite ligand
[0021] In its broadest aspect, the novel multidentate phosphite ligand comprises a catkin backbone and at least two aryl phosphite groups chemically bonded to the backbone. As used herein, the term "catkin" refers to an aromatic compound consisting of a varying number (1 to 3) of arene subunits bonded to a bridged bicyclooctatriene core structure. For example, triptycene has the following structure:
[0022]
[0023] The moieties in the backbone are optionally substituted with one or more C1 to C4 alkyl substituents.
[0024] Preferably, the catkin backbone comprises two or three arene subunits bonded to a bridged bicyclooctatriene core structure. Preferably, the arene subunits are phenyl groups.
[0025] As used herein, the term "aryl" refers to an aromatic carbocyclic group having a single ring (e.g., phenyl), multiple rings (e.g., biphenyl), or multiple condensed rings of which at least one is aromatic (e.g., 1,2,3,4-tetrahydronaphthyl, naphthyl, anthracenyl, or phenanthrenyl), all of which are optionally substituted.
[0026] In one embodiment, the catkin backbone of the novel multidentate phosphite ligand described herein comprises two aromatic groups attached to the bicyclooctatriene core of the backbone, each aromatic phosphite group being chemically bonded to a different carbon atom of the core or a different C1 to C4 alkyl substituent of the core, such as a methyl substituent, via an oxygen atom. The aromatic phosphite groups are not chemically bonded to the aromatic groups of the catkin.
[0027] In another embodiment, the catkin backbone comprises three aromatic groups attached to a bicyclooctatriene core of the backbone, and each arylphosphite group is chemically bonded to a carbon atom of a different aromatic group of the catkin backbone via an oxygen atom, wherein the aryl groups of the arylphosphite groups are not chemically bonded to each other.
[0028] In some embodiments, each aryl phosphite group comprises at least one substituted phenyl group, such as at least one phenyl group substituted with one or more alkyl groups having 1 to 4 carbon atoms.
[0029] The aryl phosphite group has the general formula -OP-(O-aryl)2. Preferably, the aryl group is an optionally substituted phenyl group, more preferably a phenyl group substituted by one or more alkyl groups having 1 to 4 carbon atoms. Even more preferably, the aryl group is a phenyl group substituted by one or more methyl groups. Most preferably, the aryl group is a tolyl group or a xylyl group.
[0030] In a preferred embodiment, the aryl groups of the arylphosphite groups are not chemically bonded to each other.
[0031] Thus, the catkin backbone of the novel multidentate phosphite ligands described herein may comprise two aromatic hydrocarbon groups attached to a bicyclooctatriene core of the backbone, each aryl phosphite group being chemically bonded to a different carbon atom of the core via an oxygen atom, wherein the aryl group of the aryl phosphite group is an optionally substituted phenyl group, more preferably a phenyl group substituted with one or more alkyl groups having 1 to 4 carbon atoms, even more preferably a phenyl group substituted with one or more methyl groups, most preferably a tolyl group or a xylyl group.
[0032] Alternatively, the catkin backbone of the novel multidentate phosphite ligand described herein may comprise two aromatic hydrocarbon groups attached to the bicyclooctatriene core of the backbone, each aryl phosphite group chemically bonded to a different carbon atom of the core via an oxygen atom, wherein the aryl groups of the aryl phosphite groups are not chemically bonded to each other, wherein the aryl groups of the aryl phosphite groups are optionally substituted phenyl groups, more preferably phenyl groups substituted with one or more alkyl groups having 1 to 4 carbon atoms, even more preferably phenyl groups substituted with one or more methyl groups, most preferably tolylaryl or xylyl groups. As described above, the aryl phosphite groups of the catkin ligand comprising two aromatic hydrocarbon groups attached to the bicyclooctatriene core of the backbone are not chemically bonded to the aromatic hydrocarbon groups of the catkin.
[0033] Alternatively, the catkin backbone of the novel multidentate phosphite ligands described herein may comprise two aromatic hydrocarbon groups attached to a bicyclooctatriene core of the backbone, each aryl phosphite group being chemically bonded to a different C1 to C4 alkyl substituent of the core via an oxygen atom, preferably a methyl substituent, wherein the aryl group of the aryl phosphite group is an optionally substituted phenyl group, more preferably a phenyl group substituted with one or more alkyl groups having 1 to 4 carbon atoms, even more preferably a phenyl group substituted with one or more methyl groups, and most preferably a tolyl group or a xylyl group.
[0034] Alternatively, the catkin skeleton comprises three aromatic hydrocarbon groups attached to the bicyclooctatriene core of the skeleton, and each arylphosphite group is chemically bonded to a carbon atom of a different aromatic hydrocarbon group of the catkin skeleton via an oxygen atom, wherein the aryl group of the arylphosphite group is an optionally substituted phenyl group, more preferably a phenyl group substituted by one or more alkyl groups having 1 to 4 carbon atoms, even more preferably a phenyl group substituted by one or more methyl groups, most preferably a tolyl group or a xylyl group. The aryl groups of the arylphosphite group are not chemically bonded to each other.
[0035] Non-limiting examples of suitable multidentate phosphite ligands include the following:
[0036]
[0037]
[0038]
[0039] Synthesis of multidentate phosphite ligands
[0040] The synthesis of catkins and similar molecules is described in, for example, Hart, "Iptycenes, Cuppendophanes and Cappedophanes," Pure and Applied Chemistry, 65(1): 27-34 (1993); and Shahlia et al., "Synthesis of Supertriptycene and Two Related Iptycenes," Journal of Organic Chemistry, 56: 6905-6912 (1991), the contents of which are incorporated herein by reference. In some embodiments, the catkin skeleton can be synthesized via a Diels-Alder reaction between anthracene species and benzyne species.
[0041] In some embodiments, the novel multidentate phosphite ligands described herein are produced from a catkin precursor containing an -OH group at the position on the catkin backbone where the phosphite group is to be introduced. In this case, the synthesis of the desired ligand can be carried out by reacting the catkin precursor with a chlorophosphite of the following structure:
[0042]
[0043] Where R 1 and R 2 is the aryl substituent of each arylphosphite group.
[0044] Suitable catkin precursors containing OH are commercially available or can be prepared by methods known in the art. For example, catkin-based skeletons CAS#20678-93-7 suitable for producing ligands A and B can be obtained from Aldrich, and catkin-based skeletons CAS#26495-88-5 suitable for producing ligand C can be obtained from Accel Pharmatech. Catkin-based skeletons CAS#1312012-20-6 suitable for producing ligand D can be prepared by the method taught in Organic Letters 2011, 13, 5052. The synthesis of the diphosphites disclosed herein is completed using the procedure of US 9,221,852 B2.
[0045] The method used to produce the chlorophosphite is not critical, as many available methods are known in the art. For example, the chlorophosphite can be prepared by reacting PCl3 with an aromatic alcohol, R 1 OH and R 2 OH is reacted stepwise in the presence of a suitable organic base to first prepare a dichlorophosphite (e.g. (R 1 O) PCl2), which is then further reacted with an aromatic alcohol to prepare the desired chlorophosphite. The selective synthesis of suitable chlorophosphites is disclosed in, for example, PCT Publication Nos. WO 2004 / 050588 and EP 2,243,763 B1.
[0046] The resulting chlorophosphite is then contacted with a catkin precursor and a base (preferably an organic tertiary amine containing one or more basic nitrogen atoms) under conditions that promote the reaction between the chlorophosphite and the diol to produce the desired ligand. The contact is conveniently carried out by at least one contact method selected from the group consisting of: (i) feeding the catkin precursor to a mixture of the chlorophosphite and the organic tertiary amine, and (ii) feeding the catkin precursor and the organic tertiary amine to the chlorophosphite alone or as a mixture. In an embodiment, the feed is controlled so that during all stages of the contact, the ratio of the number of moles of chlorophosphite in the reaction mixture divided by the number of moles of the catkin precursor fed to the reaction mixture is at least 2.0, such as 2.1 to 2.7, and during all stages of the contact, the ratio of the number of moles of the basic nitrogen atoms from the organic tertiary amine fed to the reaction mixture divided by the number of moles of the chlorophosphite in the reaction mixture is at least 1.0, such as 1.0 to 1.5. Typically, the contacting is carried out at a temperature of about 10°C to about 110°C, such as about 20°C to about 110°C, such as about 30°C to about 110°C, such as about 40°C to about 110°C, such as about 50°C to about 110°C, such as about 60°C to about 110°C.
[0047] Examples of suitable organic tertiary amines containing a single basic nitrogen atom may be (R′)(R″)(R″′)N compounds, wherein R′, R″ and R″′ are independently selected from the group consisting of C1 to C 10 Alkyl groups and C6 to C 10 The amine may be a group consisting of an aromatic group, or may be an aromatic tertiary amine compound (e.g., pyridine), or may be a combination of organic tertiary amines containing a single basic nitrogen atom. An example of a suitable amine includes a trialkylamine having a single selected alkyl group and having 1 to 10 carbon atoms, such as triethylamine. Other examples include organic tertiary amines containing multiple basic nitrogen atoms, the organic tertiary amine having a nitrogen atom without an N--H bond; for example, N,N,N',N'-tetramethylethylenediamine.
[0048] In some embodiments, the reaction mixture may include at least one hydrocarbon solvent. For example, the catkin precursor may be fed into a reaction zone containing a chlorophosphite in the form of a solution thereof in a hydrocarbon solvent. In some embodiments, the hydrocarbon solvent may be selected from the group consisting of: a linear acyclic C5 to C 18 Aliphatic hydrocarbons, branched acyclic C5 to C 18 Aliphatic hydrocarbons, unsubstituted cyclic C5 to C 18 Aliphatic hydrocarbons, substituted cyclic C5 to C 18 Aliphatic hydrocarbons, unsubstituted C6 to C 10 Aromatic hydrocarbons and C7 to C 18 Substituted aromatic hydrocarbons. The hydrocarbon solvent may be selected from hydrocarbons having a boiling point of 70° C. to 145° C. at atmospheric pressure. Examples of suitable aromatic hydrocarbon solvents include C1-5 substituted benzenes such as xylene and toluene.
[0049] Contact method (i) and contact method (ii) can be carried out in a semi-batch, continuous flow or a combination of semi-batch and continuous flow modes. For example, the catkin precursor can be continuously or discontinuously fed into a stirred vessel comprising a chlorophosphite and an organic tertiary amine. In addition, the catkin precursor can be continuously or discontinuously fed into a tubular reactor comprising a continuous flow of a mixture of a chlorophosphite and an organic tertiary amine.
[0050] Catalyst complex
[0051] The multidentate phosphite ligands disclosed herein can be used in combination with transition metals to form catalyst complexes (chelates). The catalyst complexes can be used for olefin hydrocyanation, for example, the hydrocyanation of dienes (such as 1,3-butadiene). In particular, for the hydrocyanation of monoolefins (such as 3-pentenenitrile), a catalyst promoter (such as a Lewis acid) can be optionally used.
[0052] The transition metal used in the catalyst complex can be any transition metal capable of the desired catalytic conversion and can additionally contain unstable ligands which are displaced during the catalytic reaction or which play an active role in the catalytic conversion. Any transition metal is contemplated in this regard. Preferred metals are those comprising Group VIII of the Periodic Table. Preferred metals for hydrocyanation and / or isomerization are nickel, cobalt and palladium, with nickel being particularly preferred for olefin hydrocyanation.
[0053] Nickel complexes of each of the multidentate phosphite ligands described herein are disclosed.
[0054] Nickel compounds can be prepared or generated according to techniques well known in the art, as described, for example, in U.S. Pat. Nos. 3,496,217, 3,631,191, 3,846,461, 3,847,959, and 3,903,120, which are incorporated herein by reference. Zero-valent nickel complexes containing ligands that can be replaced by organophosphorus ligands can be used as nickel sources. Two such zero-valent nickel complexes are Ni(COD)2 (COD is 1,5-cyclooctadiene) and Ni{P(Oo-C6H4CH3)3}2(C2H4), both of which are known in the art. Alternatively, divalent nickel compounds can be combined with a reducing agent to be used as a nickel source in the reaction. Suitable divalent nickel compounds include compounds of the formula NiY2, wherein Y is a halide, a carboxylate, or an acetylacetonate. Suitable reducing agents include metal borohydrides, metal aluminum hydrides, metal alkyls, Zn, Fe, Al, Na, or H2.
[0055] U.S. Patent No. 10,537,885 describes a method for preparing zero-valent nickel that is highly active for complexing with phosphorus-containing ligands and includes calcining a first nickel(II)-containing particle in an atmosphere containing an oxidizing component and at a temperature typically between 350°C and 600°C for a time sufficient to remove volatile components from the first nickel(II)-containing particle and produce a second nickel(II)-containing particle. The second nickel(II)-containing particle is then heated in a reducing atmosphere while rotating or tumbling the second nickel(II)-containing particle in a rotary processor at 275°C to 360°C for a time sufficient to produce a free-flowing particulate nickel metal (Ni(0)) product, wherein the reducing atmosphere does not contain added water or steam that is not generated by the reduction, and wherein a H2 / Ni molar ratio of about 1.9 to 2.5 is employed during the reduction step.
[0056] Elemental nickel, preferably nickel powder, is also a suitable source of zero-valent nickel when combined with a halogenation catalyst as described in US Pat. No. 3,903,120.
[0057] In some embodiments, elemental nickel may be present in an amount having at least about 1 m 2 The nickel particulate form may have at least 10% of the crystallites in the nickel form having a diameter (C10) of less than about 10 nm, and / or an average crystallite size of at least about 100 nm per gram of nickel. 15 The ratio of BETSSA to C50 in the form of nickel particles may be at least about 0.1×10 9 m / gm and preferably at least about 0.4×10 9 Examples of such small particle forms of nickel and methods of making them can be found in U.S. Pat. No. 9,050,591, the entire contents of which are incorporated herein by reference.
[0058] In some embodiments, the nickel used for complexing with the bidentate diphosphite ligand may contain at least about 1,500 ppmw sulfur in the form of amorphous nickel sulfide (NiS x ). Such sulfide-containing nickel precursors are described in U.S. Pat. No. 10,143,999 and can be prepared by contacting a nickel-containing starting material comprising a reducible sulfur source with a reducing agent, such as hydrogen, under conditions including a temperature of about 200° C. to about 350° C. The nickel starting material may include or may be doped with a sulfur source or may be separated from the sulfur source. Suitable nickel starting materials include one or more of nickel carbonate, nickel bicarbonate, nickel oxalate, nickel formate, nickel quarate, nickel hydroxide, and nickel oxide, with nickel formate being preferred, and suitable reducible sulfur sources including, for example, elemental sulfur, sulfates, sulfites, sulfides, hyposulfites, thiosulfates, sulfur dioxide, sulfur monoxide, sulfur halides, and the like. The entire contents of U.S. Pat. No. 10,143,999 are incorporated herein by reference.
[0059] Depending on the desired reaction to be performed, the catalyst composition may also include one or more Lewis acid promoters, which affect the activity and selectivity of the catalyst system. The promoter may be an inorganic or organometallic compound, wherein at least one element of the inorganic or organometallic compound is selected from scandium, titanium, vanadium, chromium, manganese, iron, cobalt, copper, zinc, boron, aluminum, yttrium, zirconium, niobium, molybdenum, cadmium, rhenium and tin. Examples include ZnBr2, Znl2, ZnCl2, ZnSO4, CuCl2, CuCl, Cu(O3SCF3)2, CoCl2, Col2, Fel2, FeCl3, FeCl2, FeCl2(THF)2, TiCl4(THF)2, TiCl4, TiCl3, ClTi(OiPr)3, MnCl2, ScCl3, AlCl3, (C8H 17 )AlCl2、(C8H 17)2AlCl, (iso-C4H9)2AlCl, Ph2AICI, PhAlCl2, ReCl5, ZrCl4, NbCl5, VCl3, CrCl2, MoCl5, YCl3, CdCl2, LaCl3, Er(O3SCF3)3, Yb(O2CCF3)3, SmCl3, B(C6H5)3, TaCl5. Suitable promoters are further described in U.S. Pat. Nos. 3,496,217, 3,496,218 and 4,774,353. These include metal salts such as ZnCl2, Col2 and SnCl2 and organometallic compounds such as RAlCl2, R3SnO3SCF3 and R3B, where R is an alkyl group or an aryl group. U.S. Pat. No. 4,874,884 describes how to select a synergistic combination of promoters to increase the catalytic activity of the catalyst system. Preferred promoters include CdCl2, FeCl2, ZnCl2, B(C6H5)3 and (C6H5)3SnX, where X is CF3SO3, CH3C6H5SO3 or (C6H5)3BCN. The molar ratio of promoter to nickel present in the reaction may range from about 1:16 to about 50:1.
[0060] Catalytic method using a catalyst complex
[0061] The above-mentioned catalyst complex can be used for a variety of catalytic reactions, such as hydrogenation, hydroformylation, hydrocyanation, hydrocarboxylation, hydroamidation, hydroesterification and aldol condensation. Preferred reactions include hydroformylation, wherein olefins react with carbon monoxide and hydrogen to produce aldehydes, and particularly hydrocyanation, wherein olefins react with hydrogen cyanide to produce nitrile. The particularly preferred use of the above-mentioned catalyst complex wherein the transition metal is nickel is for the catalytic hydrocyanation of 1,3-butadiene to produce 3-pentenenitrile, which is then converted into adiponitrile. In embodiments, in the first reaction zone, 1,3-butadiene reacts with hydrogen cyanide in the presence of the first catalyst to produce pentenenitrile comprising 3-pentenenitrile and 2-methyl-3-butenenitrile. In an optional second reaction zone, the 2-methyl-3-butenenitrile recovered from the first reaction zone is isomerized to 3-pentenenitrile on the second catalyst. In the third reaction zone, 3-pentenenitrile recovered from the first reaction zone and the second reaction zone reacts with hydrogen cyanide in the presence of a third catalyst and a Lewis acid to produce adiponitrile. One, two or all of the first catalyst, the second catalyst and the third catalyst may be the above catalyst complex.
[0062] For example, 3-pentenenitrile (3PN) can be formed from 1,3-butadiene through a series of reactions as shown in Equation 1 and Equation 2 below.
[0063]
[0064] According to the abbreviations used herein, BD is 1,3-butadiene, 2PN is 2-pentenenitrile, 3PN is 3-pentenenitrile, 4PN is 4-pentenenitrile, 2M2BN is 2-methyl-2-butenenitrile, 2M3BN is 2-methyl-3-butenenitrile, MGN is 2-methylglutaronitrile, and ADN is adiponitrile.
[0065] In the presence of transition metal complexes containing various phosphorus-containing ligands, such as the catalyst complexes described herein, dinitriles such as ADN, MGN, and ethylsuccinonitrile (ESN) can be formed by the hydrocyanation of 3PN and 2M3BN as shown below in Equations 3 and 4. Equation 4 also shows that 2M2BN can be formed when 2M3BN is undesirably isomerized in the presence of a Lewis acid promoter, which can be carried away from the pentenenitrile hydrocyanation reaction zone.
[0066]
[0067] According to one aspect of the present disclosure, 3-pentenenitrile is prepared in a method comprising two steps. In the first step, 1,3-butadiene reacts with hydrogen cyanide in the presence of a first catalyst complex comprising a transition metal (such as zero-valent nickel) and a first phosphorus-containing ligand in a first reaction zone to produce a reactor effluent comprising 3-pentenenitrile (3PN) and 2-methyl-3-butenenitrile (2M3BN). In the second step, at least a portion of the 2M3BN prepared in the first step is isomerized in the presence of a second catalyst complex comprising a transition metal (such as zero-valent nickel) and a second phosphorus-containing ligand in a second reaction zone to prepare a reaction product comprising 3PN. The first catalyst complex may be the same or different from the second catalyst complex, and may be a catalyst complex as described herein. Typically, the reactions in the first reaction zone and the second reaction zone are carried out in the absence of a Lewis acid promoter.
[0068] The effluent stream containing 3PN can be recovered from the second reaction zone. In addition, 3PN is usually also recovered from the reaction product of the first reaction zone, such as by distillation. The recovered 3PN can be contacted with HCN in the presence of a third catalyst complex comprising a transition metal (such as zero-valent nickel) and a third phosphorus-containing ligand in the third reaction zone in the third reaction step. The third catalyst complex can be the same or different from the first catalyst complex and / or the second catalyst complex, and can be a catalyst complex as described herein. The reaction in the third reaction zone is carried out in the presence of a Lewis acid promoter.
[0069] In addition to 3-pentenenitrile (3PN) and 2-methyl-3-butenenitrile (2M3BN), the reaction product from the first reaction zone also contains dinitriles. These dinitriles include adiponitrile (ADN) (which can be formed by the reaction of 3-pentenenitrile (3PN) with HCN) and methylglutaronitrile (MGN) (which can be formed by the reaction of 2-methyl-3-butenenitrile (2M3BN) with HCN). The formation of MGN in the first reaction zone is harmful because 2M3BN is converted before it can be recovered and isomerized to 3PN. In the process of recovering 3PN and reacting with HCN to form ADN, the production of one mole of MGN in the first reaction zone results in the loss of two moles of HCN and one mole of BD, which otherwise can be converted to ADN. Therefore, based on the moles of HCN and BD reacted, the generation of unwanted MGN in the first reaction zone results in a reduction in the yield of unwanted ADN.
[0070] Conversion of 1,3-butadiene to 3-pentenenitrile
[0071] The 1,3-butadiene feedstock of the first reaction zone may contain at least 98% by weight, preferably at least 99% by weight, more preferably at least 99.5% by weight of 1,3-butadiene based on the total weight of the feedstock. In one embodiment, the feedstock contains 99.5% to 99.9% by weight of 1,3-butadiene based on the total weight of the feedstock. The balance of the feedstock may contain impurities such as butane, butene, 1,2-butadiene and acetylene (such as propyne) at residual levels commonly found in commercial BD feedstocks. Typically, the feed containing BD contains less than a total of 100ppm of acetylene. The BD feedstock may also contain tert-butylcatechol (TBC), such as 4-tert-butylcatechol. Before 1,3-butadiene is charged to the first reaction step, a portion of the TBC present in the feedstock may be optionally removed.
[0072] The HCN feed to the first reaction zone and the third reaction zone can be a product of the Andrussow process, which is dried to less than about 250 ppm of water, such as less than 125 ppm of water, such as less than 80 ppm of water by distillation before entering the olefin hydrocyanation reaction zone. However, the HCN feed usually contains at least some water. Very dry HCN is unstable, and therefore, it may not be desirable to provide completely anhydrous HCN. Therefore, the HCN feed can contain at least 10 ppm, such as at least 25 ppm, such as at least 50 ppm of water. The HCN feed is preferably substantially free of carbon monoxide, oxygen and ammonia. The HCN can be introduced into the first reaction zone and the third reaction zone as a vapor, a liquid or a mixture thereof; see, for example, European Patent Publication No. 1344770. As an alternative, cyanohydrin can be used as a source of HCN; see, for example, U.S. Patent No. 3,655,723.
[0073] The total feed molar ratio of BD to HCN in the first reaction zone can be in the range of about 1:1 to about 100:1, such as in the range of about 1:1 to about 2:1. Excess BD in the first reaction zone can reduce the formation of dinitrile during the BD hydrocyanation reaction. The feed molar ratio of HCN to catalyst in the first reaction zone can be in the range of about 5:1 to about 100,000:1, such as in the range of about 100:1 to about 5,000:1.
[0074] The reaction conditions employed in the first reaction zone may include a temperature in the range of about -25°C to about 200°C, such as a temperature in the range of about 0°C to about 150°C. Typically, the reaction pressure should be sufficient to maintain BD and HCN in contact with the catalyst dissolved in the liquid reaction mixture, which pressure is at least partially a function of the amount of unreacted BD present in the reaction mixture. Although the disclosed process is not limited by an upper pressure limit for the first reaction step, for practical purposes, the pressure is typically in the range of about 15 psia to about 300 psia (about 1.03 bar to about 20.7 bar).
[0075] During the first reaction step, the non-oxidizing and anhydrous environment prevents oxidative deactivation of the catalyst. Therefore, a dry inert atmosphere (e.g., nitrogen) is typically used in the first reaction zone, although air may be used at the expense of losing a portion of the catalyst through oxidation and hydrolysis.
[0076] In the first reaction step, the HCN feed, the BD-containing feed, and the catalyst composition may be contacted in any suitable reactor or reactors known to those skilled in the art. Examples include a continuous stirred tank reactor, a loop bubble column reactor, a gas recycle reactor, a bubble column reactor, a tubular reactor, or a combination thereof, optionally with a means for removing at least a portion of the heat of reaction.
[0077] The residence time in the first reaction zone is usually determined by the expectation of obtaining a certain degree of conversion of BD, HCN or their combination. Usually, the residence time will be in the range of about 0.1 hour to about 15 hours, for example, in the range of about 1 hour to about 10 hours. The HCN conversion rate can be, for example, greater than 99%. Usually, the BD conversion rate in the first reaction zone can be less than 99%, for example, between 80% and 95% in total, for example, 90% in total. The staged HCN addition in the first reaction zone can be used.
[0078] Separation of the product from the first reaction zone
[0079] The reaction of 1,3-butadiene and hydrogen cyanide in the presence of a first catalyst in a first reaction zone produces a first reaction effluent comprising 3-pentenenitrile, 2-methyl-3-butenenitrile, unreacted 1,3-butadiene and the first catalyst. These components of the reaction effluent can be at least partially separated by one or more distillation steps. In particular, these distillation steps can be carried out in one or more distillation towers to provide: 1) at least one 1,3-butadiene-rich stream; 2) a 2-methyl-3-butenenitrile-rich stream; 3) a 3-pentenenitrile-rich stream; and 4) a first catalyst-rich stream. These streams are rich in specific components because they have higher concentrations of these components than the effluent from the first reaction zone. In an embodiment, the 2-methyl-3-butenenitrile-rich stream and the 3-pentenenitrile-rich stream may each contain a total of less than 500 parts per million parts by weight of phosphorus-containing ligands, such as less than 350 parts per million parts by weight of phosphorus-containing ligands, such as less than 200 parts per million parts by weight of phosphorus-containing ligands.
[0080] In an embodiment, at least partial separation of 3-pentenenitrile and 2-methyl-3-butenenitrile in the reaction effluent from the first reaction zone can be achieved by a multi-stage distillation process. For example, such a method may include a first distillation column device, which includes a feed inlet; an upper withdrawal outlet; and a bottom withdrawal outlet. The reaction effluent containing 3PN, 2M3BN and at least one catalyst including a phosphorus-containing ligand can be supplied to the feed stage of the first distillation column through the feed inlet. The distillation column may include a stripping section, a rectifying section, or both. There may be at least one separation stage between the feed inlet and the upper withdrawal outlet. A pentenenitrile-rich stream containing 3-pentenenitrile and 2-methyl-3-butenenitrile can be taken out from the upper withdrawal outlet. Relative to the phosphorus-containing ligand feed stream fed to the distillation column, such a stream is depleted of at least one phosphorus-containing ligand. The stream depleted of pentenenitrile can be taken out from the bottom withdrawal outlet. Relative to the phosphorus-containing ligand feed stream fed to the distillation column, such a stream depleted of pentenenitrile is rich in phosphorus-containing ligands. The first distillation column may be operated such that the pentenenitrile-depleted stream comprises at least 5 wt% pentenenitrile, including the sum of 3-pentenenitrile and 2-methyl-3-butenenitrile.
[0081] The pentenenitrile-rich stream comprising 3-pentenenitrile and 2-methyl-3-butenenitrile can be distilled in a second distillation column to obtain a 2-methyl-3-butenenitrile-rich stream as an overhead product and a 2-methyl-3-butenenitrile-depleted stream (i.e., a 3-pentenenitrile-rich stream) as a bottom product. The 3-pentenenitrile-rich bottom stream can be recycled to the first reaction zone, while the 2-methyl-3-butenenitrile-rich overhead product can be fed to the second reaction zone for isomerization to produce additional 3-pentenenitrile.
[0082] The first catalyst-rich stream separated from the first reaction zone effluent is at least partially recycled to the first reaction zone, and in some cases to the second reaction zone. However, since this stream contains catalyst degradation products and reaction byproducts and may be poor in nickel, a portion of the first catalyst-rich stream is usually taken out and fed to the first catalyst purification system. In an embodiment, at least 80%, preferably at least 90%, such as 93% to 96%, at least 99%, at least 99.9%, and substantially all of the first catalyst is recycled, and the rest is fed to the purification system. Typically, the purification system includes one or more liquid / liquid extraction zones, wherein the first catalyst-rich stream is contacted with a non-polar solvent (such as cyclohexane or other cyclic or linear alkanes) and a polar solvent (such as adiponitrile) that is immiscible with the non-polar solvent (preferably in countercurrent flow). Typically, the temperature in the extraction zone that promotes phase separation and catalyst extraction can be 25°C to 135°C, such as 25°C to 90°C, such as 50°C to 75°C. In the extraction zone, a non-polar phase comprising the non-polar solvent and the first catalyst and a polar phase (eg, raffinate) comprising the polar solvent and, for example, reaction byproducts and catalyst degradation products are formed.
[0083] The non-polar phase is recovered from the extraction zone and then fed to a separation system, conveniently one or more distillation columns, wherein the purified first catalyst is separated from the non-polar solvent and then returned to the first reaction zone or the second reaction zone, optionally after additional nickel is added to the catalyst. The non-polar solvent can then be recycled to the liquid / liquid extraction zone. Similarly, the raffinate phase is recovered separately from the extraction zone and then fed to another separation system, conveniently one or more distillation columns, wherein reaction by-products and catalyst degradation products are separated from the polar solvent for further processing and / or disposal. The polar solvent can then be recycled to the liquid / liquid extraction zone.
[0084] Isomerization of 2-methyl-3-butenenitrile
[0085] A stream rich in 2-methyl-3-butenenitrile (2M3BN) separated from the effluent of the first reaction zone is fed to a second reaction zone, wherein 2M3BN is isomerized in the presence of a second catalyst complex to produce a reaction product comprising 3PN. Typically, the feed to the second reaction zone comprises at least 30 wt % 2M3BN and less than 70 wt % pentenenitriles other than 2M3BN. The second catalyst complex typically comprises a transition metal (such as zero-valent nickel) and a ligand, and may be the same as or different from the first catalyst complex. If a monodentate phosphorus-containing ligand is used for the second catalyst complex, the molar ratio of the monodentate ligand to the zero-valent nickel in the catalyst for the isomerization reaction may be from about 1:1 to about 50:1, for example, from about 1:1 to about 30:1. When a bidentate ligand is used, the molar ratio of the bidentate ligand to the zero-valent nickel in the catalyst for the isomerization reaction may be from 1:1 to 10:1, for example, from 1:1 to 5:1.
[0086] To promote the isomerization of 2M3BN to produce 3PN, the reaction temperature in the second reaction zone can be maintained in the range of about 0°C to about 200°C, for example, in the range of about 50°C to about 165°C, and the pressure is generally in the range of about 15 psia to about 300 psia (about 1.03 bar to about 20.7 bar). The feed mole ratio of 2M3BN to catalyst for the isomerization reaction step is generally greater than 1:1, generally in the range of about 5:1 to 20,000:1, for example, about 100:1 to about 5,000:1. Suitable reactors for the isomerization reaction include continuous stirred tank reactors, loop bubble column reactors, gas circulation reactors, bubble column reactors, tubular reactors, or combinations thereof, optionally with a device for removing at least a portion of the heat of reaction. The residence time of the isomerization reaction in the second reaction zone can be about 0.1 hours to about 15 hours, for example, about 1 hour to about 10 hours.
[0087] Separation of the product from the second reaction zone
[0088] The effluent from the second reaction zone mainly comprises 3-pentenenitrile, residual 2-methyl-3-butenenitrile and the second catalyst. These components can be separated at least in part by one or more distillation steps to provide: 1) a second stream rich in 2-methyl-3-butenenitrile; 2) a second stream rich in 3-pentenenitrile; and 3) a second stream rich in catalyst. The second stream rich in 2-methyl-3-butenenitrile and the second stream rich in 3-pentenenitrile can each contain a total of less than 500 parts per million parts by weight of phosphorus-containing ligands. For example, the second stream rich in 3-pentenenitrile can contain less than 300ppm, for example, less than 100ppm of phosphorus-containing ligands.
[0089] The second 3-pentenenitrile-rich stream may include a small amount of 2-methyl-3-butenenitrile, which may be separated from 3-pentenenitrile in one or more distillation columns, wherein 2-methyl-3-butenenitrile is recovered as an overhead product and 3-pentenenitrile is recovered as a bottoms product. For example, the first 3-pentenenitrile-rich stream and the second 3-pentenenitrile-rich stream may be combined and distilled in a single or shared distillation column, or these streams may be distilled in separate distillation columns. The 2-methyl-3-butenenitrile recovered from such distillation may be passed as a feed to the second reaction zone, and the 3-pentenenitrile recovered from such distillation may be passed as a feed to the third reaction zone.
[0090] The second 3-pentenenitrile-rich stream may further comprise (Z)-2-methyl-2-butenenitrile and may be distilled to obtain as an overhead product a (Z)-2-methyl-3-butenenitrile-rich stream comprising 2-methyl-3-butenenitrile and (Z,)-2-methyl-2-butenenitrile and other low boilers, and as a bottom product a (Z)-2-methyl-2-butenenitrile-depleted stream comprising 3-pentenenitrile, 2-methyl-3-butenenitrile and some (Z)-2-methyl-2-butenenitrile depending on the distillation conditions. 3-Pentenenitrile and 2-methyl-3-butenenitrile may be recovered separately from the (Z)-2-methyl-2-butenenitrile-depleted stream to be passed to the third reaction zone and recycled to the second reaction zone, respectively.
[0091] At least a portion of the second stream rich in 3-pentenenitrile can be used to prepare a catalyst solution. In particular, at least a portion of the second stream rich in 3-pentenenitrile can be passed into a catalyst reaction zone, wherein the nickel metal reacts with the phosphorus-containing ligand to produce a catalyst solution comprising a catalyst and pentenenitrile. A portion of such a catalyst solution can be passed into the second reaction zone. When the first catalyst and the second catalyst comprise the same phosphorus-containing ligand, a portion of the catalyst can be passed into the first reaction zone.
[0092] The second catalyst-rich stream recovered from the reaction effluent of the second reaction zone can be purified by liquid / liquid extraction, as discussed above for the first catalyst-rich stream separated from the effluent of the first reaction zone. In fact, when the first catalyst complex and the second catalyst complex are the same, a single liquid / liquid extraction system can be used to purify both catalysts.
[0093] Hydrocyanation of 3-pentenenitrile to adiponitrile
[0094] The 3-pentenenitrile produced in the first reaction zone and the second reaction zone is passed to a third reaction zone wherein the 3PN is reacted with additional hydrogen cyanide in the presence of a third phosphorus-containing catalyst complex to produce adiponitrile.
[0095] The 3-pentenenitrile feed to the third reaction zone is obtained from the above-mentioned distillation step and can generally contain at least 95 wt% 3PN, less than 5 wt% pentenenitrile other than 3PN and less than 0.1 wt% of the first phosphorus-containing ligand. The 3PN feed can contain less than 5000 parts per million (ppm), such as less than 2000 parts per million (ppm), such as less than 1000 parts per million (ppm), such as less than 600 parts per million (ppm) of C9 mononitriles.
[0096] The HCN feed entering the third reaction zone can be a product of an Andrussow process that has been dried by distillation to less than about 250 ppm of water, such as less than 125 ppm of water, such as less than 80 ppm of water. However, the HCN feed typically contains at least some water because very dry HCN is unstable. Therefore, the HCN feed can contain at least 10 ppm, such as at least 25 ppm, such as at least 50 ppm of water. The HCN feed entering the third reaction zone is preferably substantially free of carbon monoxide, oxygen, and ammonia. As an alternative, cyanohydrin can be used as a source of HCN; see, for example, U.S. Patent No. 3,655,723.
[0097] The third phosphorus-containing catalyst complex typically comprises a transition metal (such as zero-valent nickel) and a monodentate or bidentate phosphorus-containing ligand, which may be the same or different from the ligand used in the first catalyst complex or the second catalyst complex. However, the third phosphorus-containing catalyst complex typically includes one or more promoters to improve the production of dinitrile. As known in the art, promoters affect catalyst activity and selectivity to the desired ADN. The promoters used include salts of metals with atomic numbers of 13, 21-32, 39-50 and 57-80, such as zinc, and compounds of formula BR'3, wherein R' is an alkyl group or an aryl group of up to 18 carbon atoms, such as triphenylboron. The anions of such metal salts may include halides, such as chlorides, sulfates, phosphates, and lower aliphatic carboxylates. Useful promoters are generally referred to as Lewis acids in the art. In one embodiment, when the Lewis acid promoter is ZnCl2, the molar ratio of promoter to nickel in the third catalyst complex may be 1:20 to 50:1, such as 0.2:1 to 2:1.
[0098] The conditions employed in the third reaction zone may typically include a temperature in the range of about 0°C to about 150°C, such as a temperature in the range of about 25°C to about 80°C. Typically, the reaction pressure should be sufficient to maintain contact between the HCN and the catalyst dissolved in the liquid reaction mixture. The pressure is at least partially a function of the amount of unreacted HCN present in the reaction mixture. Although the upper pressure limit for this reaction step is not limited to any particular pressure, for practical purposes, the pressure is typically in the range of about 15 psia to about 300 psia (about 1.03 bar to about 20.7 bar). The total feed molar ratio of 3PN to HCN in the third reaction zone may be 1:1 to 100:1, such as 1:1 to about 5:1, and the molar ratio of HCN to catalyst may be 10:1 to 5000:1, such as 100:1 to 3000:1, such as 300:1 to 2000:1. The phosphorus-containing ligand used in the reaction of 3PN with HCN is preferably a bidentate ligand. The molar ratio of bidentate ligand to nickel in the catalyst for the 3PN hydrocyanation step can be 1:1 to 10:1, such as 1:1 to 5:1, such as 1:1 to 3:1. The residence time in the third reaction zone is generally determined by the desire to obtain a certain degree of conversion of pentenenitriles, HCN or a combination thereof. In addition to the residence time, catalyst concentration and reaction temperature will also affect the conversion of reactants to products. Typically, the residence time will be in the range of about 0.1 hour to about 30 hours, such as in the range of about 1 hour to about 20 hours. The HCN conversion rate can be greater than 99%.
[0099] Suitable reactors for the third reaction zone include continuous stirred tank reactors, loop bubble column reactors, gas recycle reactors, bubble column reactors, tubular reactors or combinations thereof, optionally with means for removing at least a portion of the heat of reaction.
[0100] Separation of the product from the third reaction zone
[0101] The reaction product mixture from the third reaction zone is mainly composed of dinitriles, especially the desired adiponitrile (ADN) and some 2-methylglutaronitrile (MGN), pentenenitrile (such as 3PN, 2PN and (E)-2M2BN), catalyst, catalyst degradation products and promoter. These components can be separated by any method known in the art, but are usually treated by a combination of distillation and liquid / liquid extraction steps. For example, one or more distillation stages can be included between the third reaction zone and the downstream liquid extraction zone to remove lower boiling components from the product mixture, including unreacted 3-pentenenitrile. The remaining product mixture is then fed to the liquid / liquid extraction zone, where the mixture is contacted with an extraction solvent. In the extraction zone, an extraction phase comprising the extraction solvent and the third catalyst and a raffinate phase comprising adiponitrile, catalyst degradation products and promoter are formed.
[0102] The extract phase is passed into a distillation column, in which the extraction solvent is separated from the catalyst to be recycled back to the extraction zone. A catalyst stream is taken out from the distillation column and recycled back to the third reaction zone. The raffinate phase can be distilled in one or more distillation steps to separate adiponitrile (ADN) and 2-methylglutaronitrile (MGN) from compounds having a boiling point higher than adiponitrile (ADN) and compounds having a boiling point lower than 2-methylglutaronitrile (MGN) to obtain a first refined dinitrile stream. The first refined dinitrile stream can be further distilled to remove 2-methylglutaronitrile (MGN) from the first refined dinitrile stream to obtain a second refined dinitrile stream rich in adiponitrile. At least a portion of the second refined dinitrile stream is recycled to the liquid / liquid extraction step as a dinitrile recycle stream.
[0103] Now refer to Figure 1 An embodiment of a representative method for preparing adiponitrile by 1,3-butadiene is described. As shown in the figure, in the method shown, 1,3-butadiene feed is supplied to the first reaction zone Z1 by pipeline 100, which also receives the supply of hydrogen cyanide by pipeline 120, and receives the supply of the first phosphorus-containing catalyst complex by pipeline 140. In the first reaction zone Z1, the control conditions are such that 1,3-butadiene reacts with hydrogen cyanide to produce a reaction product substantially comprising 3-pentenenitrile (3PN) and 2-methyl-3-butenenitrile (2M3BN). The reaction effluent stream is removed from the first reaction zone Z1 by pipeline 122 and introduced into a separation section 125, to obtain a concentrated catalyst stream 140 and a product stream 200 comprising 2-methyl-3-butenenitrile (2M3BN) in particular. The separation section 125 may include one or more distillation columns. Unreacted hydrogen cyanide and 1,3-butadiene may also be separated from the reaction product and the catalyst in the separation section 125. Unreacted 1,3-butadiene can be Figure 1 The feed stream containing 3-pentenenitrile (3PN) can also be recycled to the first reaction zone Z1 through a pipeline not shown in FIG. Figure 1 A pipeline not shown in FIG. 1 is taken out from the separation section 125 .
[0104] A portion of the catalyst separated from the reaction products in separation section 125 is recycled to first reaction zone Z1 via line 140, while another portion of the catalyst is removed and fed to liquid / liquid extraction zone 150 via line 126 to at least partially purify or regenerate the catalyst. A non-polar solvent, such as an alkane, is fed to liquid / liquid extraction zone 150 via line 130, and a polar solvent that is immiscible with the non-polar solvent is also fed to liquid / liquid extraction zone 150 via line 500. In an alternative embodiment ( Figure 1In the extraction zone 150 (not shown), the spent catalyst in line 126 and the polar solvent in line 500 are mixed before the combined stream is charged to the extraction zone 150. In the extraction zone 150, a non-polar phase comprising the non-polar solvent and the catalyst and a polar phase (e.g., raffinate) comprising the polar solvent and, for example, reaction byproducts and catalyst degradation products are formed. The non-polar phase is withdrawn from the extraction zone 150 via line 134 and fed to the distillation system 155. The polar phase is withdrawn from the extraction zone 150 via line 510 to the separation stage 1000.
[0105] The distillation system 155 is operated to recover the non-polar solvent as an overhead stream which is returned to the extraction zone 150 via line 130, with make-up non-polar solvent optionally added to the overhead stream. The bottoms from the distillation system 155 contain partially purified catalyst which is collected and removed from the distillation system 155 via line 156 and introduced at any point for recycle to the first reaction zone Z1. Figure 1 In the embodiment of the present invention, the partially purified catalyst can be removed from the distillation column 155 through the pipeline 156 and transferred to the pipeline 146 for introduction into the catalyst recycle pipeline 140 for recycling to the first reaction zone Z1. Figure 1 Stream 146 is shown introduced downstream of withdrawn stream 126, but may optionally be introduced upstream of withdrawn stream 126. Optionally, at least a portion of the partially purified catalyst stream in line 156 may be recycled to second reaction zone Z2. Figure 1 In the embodiment of the present invention, the partially purified catalyst stream in line 156 can be transferred to line 246 for introduction into catalyst recycle line 240 for recycling to the second reaction zone Z2. Make-up catalyst or catalyst components (additional zero-valent Ni and / or additional phosphorus-containing ligands) can be added to the first and second reaction zones Z1 and Z2 via lines 145 and 245, respectively.
[0106] The separation system 1000 conveniently includes a plurality of distillation columns that separate the reaction by-products and catalyst degradation products from the polar solvent, which is then returned to the extraction zone 150 via line 500 .
[0107] The product stream 200 containing 2M3BN separated from the reaction product of the first reaction zone Z1 in the separation section 125 is introduced into the second reaction zone Z2 through pipeline 240, and the second reaction zone receives a supply of a second phosphorus-containing catalyst complex, which can be the same as or different from the first phosphorus-containing catalyst complex. In the second reaction zone Z2, the conditions are controlled so that the 2M3BN undergoes isomerization to produce a reaction product substantially containing 3PN. The effluent stream containing the second phosphorus-containing catalyst complex and the 3PN product is taken out from the second reaction zone Z2 via pipeline 222 and passed into the separation section 225 to obtain, in particular, a 3PN product stream 300 and a concentrated catalyst stream 240. The separation section 225 may include one or more distillation columns.
[0108] exist Figure 1 In the particular embodiment shown, the second reaction zone Z2 is provided with a second catalyst recovery system for recycling catalyst to the second reaction zone Z2. In this second catalyst recycle system, a portion of the concentrated catalyst stream in line 240 is diverted and fed to the liquid / liquid extraction zone 250 via line 226. A non-polar solvent (such as an alkane) is fed to the liquid / liquid extraction zone 250 via line 230, and a polar solvent that is immiscible with the non-polar solvent is also fed to the liquid / liquid extraction zone 250 via line 700. In one embodiment (not shown), the catalyst stream 226 and the polar solvent in line 700 are mixed before the combined streams are fed to the extraction zone 250. Additionally, the catalyst stream 226 and the polar solvent in line 700 are mixed before the combined streams are fed to the extraction zone 250. Figure 1 Dinitrile from a source not shown in the drawing (such as a portion of the refined dinitrile product stream from the third reaction zone Z3) may be added to the extraction zone 250 as needed to accomplish the desired phase separation and extraction.
[0109] In the extraction zone 250, a non-polar phase comprising the non-polar solvent and the catalyst and a polar phase (e.g., raffinate) comprising, for example, the polar solvent, reaction byproducts, and certain catalyst degradation products are formed. The non-polar phase is removed from the extraction zone 250 via line 234 and fed to the distillation system 255. The polar phase is removed from the extraction zone 250 and fed to the separation stage 2000 via line 710.
[0110] The distillation system 255 is operated to recover the non-polar solvent as an overhead stream, which is returned to the extraction zone 250 via line 230, with make-up non-polar solvent optionally being added to the overhead stream. The bottoms from the distillation system 255 include partially purified catalyst, which may be removed via line 248 for introduction into the catalyst recycle line 240 for recycling to the second reaction zone Z2. Optionally, a side stream may be taken from line 248 and enter line 247, and this side stream may be used as catalyst feed to the first reaction zone Z1, for example by introducing the side stream from line 247 into line 146 or line 140. Any partially purified catalyst stream subsequently fed to the second reaction zone Z2 may be provided with additional zero-valent Ni and / or phosphorus-containing ligands, for example via line 245. Although not described herein, the catalyst feed may be provided by the catalyst recycle line 240 to provide a catalyst feed to the second reaction zone Z2. Figure 1 245, but line 245 may optionally feed directly into line 246 or line 248 rather than line 240. Other means of introducing make-up catalyst are known in the art and may be used.
[0111] The separation system 2000 conveniently includes a plurality of distillation columns that separate the reaction by-products and catalyst degradation products from the polar solvent, which is then returned to the extraction zone 250 via line 700 .
[0112] although Figure 1 1, but the first reaction zone Z1 and the second reaction zone Z2 may share a single catalyst recovery system. A shared catalyst recovery system may be desirable when the first phosphorus-containing ligand and the second phosphorus-containing ligand are the same. In this shared system, the following features may be eliminated or shut down: lines 226, 230, 234, 247, 248, 700, and 710; extraction zone 250; distillation apparatus 255; and separation section 2000. Instead of withdrawing a purified stream via line 226, a purified stream may be withdrawn via line 227 and introduced into line 126 or directly into extraction zone 150. In this shared catalyst recovery system, any partially purified catalyst stream entering the second reaction zone Z2 will be removed by a purification step according to Figure 1 Lines 246 and 240 are configured as shown.
[0113] The 3PN product separated from the reaction product of the second reaction zone Z2 in separation section 225 is introduced into the third reaction zone Z3 via pipeline 300, and the third reaction zone also receives a supply of HCN via pipeline 220. The 3PN from separation section 125 can also be introduced into the third reaction zone Z3 via pipeline 300. Figure 1One or more pipelines not shown in the figure are introduced into the third reaction zone Z3. A third catalyst comprising, for example, zero-valent Ni and a third phosphorus-containing ligand (collectively referred to as the third catalyst system) and a Lewis acid promoter is introduced into the third reaction zone Z3 through a pipeline 340. The reaction of 3PN and HCN in the third reaction zone Z3 produces a reaction product containing adiponitrile. A reaction product stream is taken out from the third reaction zone Z3 through a pipeline 400. The reaction product stream contains, for example, adiponitrile, a catalyst, a promoter, and unreacted reactants. Before separating the catalyst from the adiponitrile product, the reaction product stream may optionally be passed through a separation section ( Figure 1 (not shown) to remove unreacted reactants.
[0114] The catalyst and adiponitrile product of the product stream from line 400 are passed into liquid / liquid extraction zone 370. A non-polar solvent (such as an alkane) is fed into liquid / liquid extraction zone 370 via line 330. The non-polar solvent introduced into liquid / liquid extraction zone 370 may have the same or different composition as the non-polar solvent introduced into liquid / liquid extraction zone 150. The non-polar solvent from line 330 and the adiponitrile product from line 400 together constitute an extractant system of immiscible components. In extraction zone 370, a non-polar phase comprising a non-polar solvent and a catalyst and a polar phase (e.g., raffinate) comprising adiponitrile, a promoter, and catalyst degradation products are formed. The non-polar phase is taken out from extraction zone 370 to distillation system 375 via line 334. The polar phase comprising adiponitrile is taken out from extraction zone 370 and fed to adiponitrile purification section 3000 via line 600.
[0115] The distillation system 375 is operated to recover the non-polar solvent as an overhead stream, which is returned to the extraction zone 370 via line 330, with make-up non-polar solvent optionally added to the overhead stream. The bottoms from the distillation system 375 include partially purified catalyst and can be removed from the distillation system 375 via line 340 for recycling to the third reaction zone Z3. Make-up amounts of additional zero-valent Ni and / or a third phosphorus-containing ligand along with a promoter can be added to the partially purified catalyst in line 340 via line 345.
[0116] Adiponitrile purification section 3000 may collectively include a series of distillation columns that provide separation of impurities (such as reaction byproducts and catalyst degradation products) from a purified adiponitrile product (which is recovered in line 660). A portion of the purified adiponitrile product may optionally be returned to extraction zone 150 or extraction zone 250 (via Figure 1 Lines not shown in the figure) are provided to facilitate phase separation in these extraction zones.
[0117] The present invention will now be described in more detail with reference to the following non-limiting examples.
[0118] The term "DN distribution" as used herein refers to DN distribution = 100*ADN / (ADN+MGN+ESN).
[0119] Comparative Example 1-Synthesis of nickel complex solution of 2'-(bis(o-tolyloxy)methoxy)-[1,1'-di(cyclohexane)]-2-yl phosphite di-o-tolyl ester.
[0120] Comparative Example 2-2, Synthesis of a nickel complex solution of diisopropyl 2'-bis((bis(o-tolyloxy)phosphinoyl)oxy)-[1,1'-binaphthyl]-3,3'-dicarboxylate.
[0121] Comparative Example 3 - Isomerization of 2-methyl-3-butenenitrile using a nickel complex solution of 2'-(bis(o-tolyloxy)methoxy)-[1,1'-di(cyclohexane)]-2-yl phosphite di-o-tolyl ester.
[0122] Comparative Example 4 - Isomerization of 2-methyl-3-butenenitrile using a nickel complex solution of diisopropyl 2,2'-bis((bis(o-tolyloxy)phosphinoyl)oxy)-[1,1'-binaphthyl]-3,3'-dicarboxylate.
[0123] Comparative Example 5 - Hydrocyanation of 3PN using a nickel complex solution of 2'-(bis(o-tolyloxy)methoxy)-[1,1'-di(cyclohexane)]-2-yl phosphite di-o-tolyl ester.
[0124] Comparative Example 6 - Hydrocyanation of 3PN using a nickel complex solution of diisopropyl 2,2'-bis((bis(o-tolyloxy)phosphinoyl)oxy)-[1,1'-binaphthyl]-3,3'-dicarboxylate.
[0125] Experimental Example 1. Synthesis of the nickel complex of ligand A
[0126] In a glove box with an argon atmosphere, nickel metal powder (0.41 g), ligand A (1.00 g), zinc chloride (0.05 g) and 3-pentenenitrile (5.10 g) were combined in a 10 mL serum bottle sealed with a polytetrafluoroethylene-lined septum. The solution was stirred with a magnetic stirrer at 60° C. for 21 hours to obtain a solution of the nickel complex of ligand A in 3-pentenenitrile solution. The concentration of the nickel complex of ligand A in the solution was measured by high performance liquid chromatography.
[0127] Experimental Example 2. Synthesis of the Nickel Complex of Ligand B
[0128] The procedure of Experimental Example 1 was repeated except that ligand B was used instead of ligand A.
[0129] Experimental Example 3. Synthesis of the Nickel Complex of Ligand C
[0130] The procedure of Experimental Example 1 was repeated except that ligand C was used instead of ligand A.
[0131] Experimental Example 4. Synthesis of the Nickel Complex of Ligand D
[0132] The procedure of Experimental Example 1 was repeated except that ligand D was used instead of ligand A.
[0133] Comparative Example 1 - Synthesis. 2′-(bis(o-tolyloxy)methoxy)-[1,1′-di(cyclohexane)]-2-yl phosphite di-o-tolyl ester “CEx1” was prepared according to the procedure of WO 99 / 06357A1, and the corresponding nickel complex was synthesized following the procedure of Experimental Example 1, but with ligand A replacing CEx1.
[0134]
[0135] Comparative Example 2-Synthesis. Diisopropyl 2,2′-bis((bis(o-tolyloxy)phosphinoyl)oxy)-[1,1′-binaphthyl]-3,3′-dicarboxylate “CEx2” was prepared according to the procedure of WO 99 / 06357A1, and the corresponding nickel complex was synthesized following the procedure of Experimental Example 1, but using ligand A in place of CEx2.
[0136]
[0137] Experimental Example 5. Preparation of 2-methyl-3-butenenitrile using the nickel complex solution prepared in Experimental Example 1 Isomerization
[0138] A portion (0.50 g) of the solution containing the nickel catalyst from Experimental Example 1 was filtered and placed in a 5 mL glass serum vial with 5.00 g of 2-methyl-3-butenenitrile. The resulting solution was heated to 100° C. and maintained at that temperature for 5 hours, then cooled to room temperature and then analyzed by gas chromatography (GC) within 5 minutes of the end of the experiment. The conversion of 2M3BN was determined to be 81%, and the selectivity to 3-pentenenitrile was 94%.
[0139] Experimental Example 6. Preparation of 2-methyl-3-butenenitrile using the nickel complex solution prepared in Experimental Example 2 Isomerization
[0140] The procedure of Experimental Example 5 was repeated, except that the nickel complex of ligand A was replaced by the nickel complex of ligand B. The conversion of 2M3BN was determined to be 74%, and the selectivity to 3-pentenenitrile was 91%.
[0141] Experimental Example 7. Preparation of 2-methyl-3-butenenitrile using the nickel complex solution prepared in Experimental Example 3 Isomerization
[0142] The procedure of Experimental Example 5 was repeated, except that the nickel complex of ligand C was substituted for the nickel complex of ligand A. The conversion of 2M3BN was determined to be 82%, and the selectivity to 3-pentenenitrile was 97%.
[0143] Experimental Example 8. Preparation of 2-methyl-3-butenenitrile using the nickel complex solution prepared in Experimental Example 4 Isomerization
[0144] The procedure of Experimental Example 5 was repeated, except that the nickel complex of ligand A was replaced by the nickel complex of ligand D. The conversion of 2M3BN was determined to be 86%, and the selectivity to 3-pentenenitrile was 95%.
[0145] Comparative Example 3 - Isomerization of 2-methyl-3-butenenitrile (2M3BN) using the nickel complex of CEx1 The procedure of Experimental Example 5 was followed, but the nickel complex of CEx1 was substituted for the nickel complex of Ligand A. The conversion of 2M3BN was determined to be 80%, and the selectivity to 3-pentenenitrile was 90%.
[0146] Comparative Example 4 - Isomerization of 2-methyl-3-butenenitrile (2M3BN) using the nickel complex of CEx2 The procedure of Experimental Example 5 was followed, but the nickel complex of CEx2 was substituted for the nickel complex of Ligand A. The conversion of 2M3BN was determined to be 73%, and the selectivity to 3-pentenenitrile was 91%.
[0147] Experimental Example 9. Hydrocyanation of 3-pentenenitrile using the nickel complex solution prepared in Experimental Example 1 .
[0148] To a temperature-controlled 50 mL glass reaction vessel equipped with a magnetic stirrer was added 2.5 grams of the solution prepared by the procedure of Experimental Example 1 and 5 mL of 3-pentenenitrile. The mixture was treated with HCN at a nitrogen flow rate of 0.01 mL / min at 70° C. for 1 hour. GC analysis of the resulting product mixture indicated an ADN yield of 91.1% and a DN distribution of 82.5%.
[0149] Experimental Example 10. Hydrocyanation of 3-pentenenitrile using the nickel complex solution prepared in Experimental Example 2
[0150] The procedure of Experimental Example 9 was repeated, except that the nickel complex of ligand A was replaced by the nickel complex of ligand B. GC analysis of the resulting product mixture indicated an ADN yield of 88.5% and a DN distribution of 87.2%.
[0151] Experimental Example 11. Hydrocyanation of 3-pentenenitrile using the nickel complex solution prepared in Experimental Example 3
[0152] The procedure of Experimental Example 9 was repeated, except that the nickel complex of ligand C was substituted for the nickel complex of ligand A. GC analysis of the resulting product mixture indicated an ADN yield of 87.0% and a DN distribution of 86.5%.
[0153] Experimental Example 12. Hydrocyanation of 3-pentenenitrile using the nickel complex solution prepared in Experimental Example 4
[0154] The procedure of Experimental Example 9 was repeated, except that the nickel complex of ligand D was substituted for the nickel complex of ligand A. GC analysis of the resulting product mixture indicated an ADN yield of 84.1% and a DN distribution of 85.6%.
[0155] Comparative Example 5 - Hydrocyanation of 3-Pentenenitrile The procedure of Experimental Example 9 was followed using the nickel complex solution prepared from CEx1, but substituting the nickel complex of ligand CEx1 for the nickel complex of ligand A. GC analysis of the resulting product mixture indicated an ADN yield of 32% and a DN distribution of 83%.
[0156] Comparative Example 6 - Hydrocyanation of 3-Pentenenitrile The procedure of Experimental Example 9 was followed using the nickel complex solution prepared from CEx2, but substituting the nickel complex of ligand CEx2 for the nickel complex of ligand A. GC analysis of the resulting product mixture indicated an ADN yield of 36% and a DN distribution of 67%.
[0157] While the present invention has been described and illustrated by reference to particular embodiments, those skilled in the art will appreciate that the present invention lends itself to variations not necessarily illustrated herein. Therefore, reference should be made solely to the appended claims in order to determine the true scope of the present invention.
Claims
1. A multidentate phosphite ligand comprising a catkin backbone wherein catkins are optionally substituted with one or more C1 to C4 alkyl substituents and at least two aryl phosphite groups chemically bonded to the backbone, wherein the catkin backbone comprises two aromatic hydrocarbon groups attached to a bicyclooctatriene core of the backbone, and each arylphosphite group is chemically bonded to a different carbon atom of the core backbone via an oxygen atom, or each arylphosphite group is chemically bonded to a different C1 to C4 alkyl substituent of the core via an oxygen atom; or wherein the catkin backbone comprises three aromatic groups attached to a bicyclooctatriene core of the backbone, and each aryl phosphite group is chemically bonded to a carbon atom of a different aromatic group of the catkin via an oxygen atom, and the aryl groups of the aryl phosphite groups are not chemically bonded to each other.
2. A ligand according to any preceding claim, wherein each aryl phosphite group comprises at least one substituted phenyl group.
3. A ligand according to any preceding claim, wherein each aryl phosphite group comprises at least one phenyl group substituted with one or more alkyl groups having from 1 to 4 carbon atoms.
4. The ligand of claim 1, wherein the aryl group of the aryl phosphite group is a phenyl group substituted with one or more alkyl groups having 1 to 4 carbon atoms.
5. The ligand of claim 1, wherein the aryl group of the aryl phosphite group is a phenyl group substituted with one or more methyl groups. The ligand according to claim 1 , wherein the aryl group of the aryl phosphite group is a tolyl group or a xylyl group.
7. A multidentate phosphite ligand according to claim 1, wherein the multidentate phosphite ligand has one of the following structures:
8. A catalyst complex comprising a multidentate phosphite ligand according to any preceding claim and at least one transition metal.
9. The catalyst complex of claim 8, wherein the at least one transition metal comprises nickel.
10. A process for the hydrocyanation of an organic compound containing at least one olefinic group, the process comprising reacting the organic compound with hydrogen cyanide in the presence of a catalyst complex according to claim 8 or claim 9.
11. The method of claim 10, wherein the organic compound comprises 1,3-butadiene.
12. The method of claim 10, wherein the organic compound comprises 3-pentenenitrile.
13. A process for the isomerization of monoethylenically unsaturated compounds, wherein the compounds are contacted with a catalyst complex according to claim 8 or claim 9.
14. The method of claim 13, wherein the monoethylenically unsaturated compound comprises 2-methyl-3-butenenitrile.
Citation Information
Patent Citations
Phosphite derivative, its preparing process, and catalyst precarsor containing phosphite
CN1356335A
Multidentate phosphite ligands, catalytic compositions containing such ligands and catalytic processes utilizing such catalytic compositions
CN1374943A
Multidentate phosphite ligands, catalytic compositions containing such ligands and catalytic processes utilizing such catalytic compositions
CN1680291A
Sterically hindered chelate phosphinite-phosphite ligand, catalyst, comprising at least one nickel(0) complex stabilized by said ligand and method for production of nitriles
CN1875025A