Polymer bead composition and method for preparing polymer bead using the same
By adding specific ethylene monomers, chain transfer agents, phenolic compounds and surface coating agents to the polymer beads, the problem of insufficient heat resistance at high temperatures is solved, and the polymer beads is achieved above 310°C Excellent heat resistance and uniform particle size distribution, suitable for optical films and diffusion plates and other fields.
Patent Information
- Application Number
- CN202380028625.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-11
- Filing Date
- 2023-04-10
- Publication Date
- 2024-11-01
AI Technical Summary
The existing polymer beads have insufficient heat resistance at high temperatures, resulting in instability and optical performance changes in applications above 320°C, limiting their application in optical films and diffusion plates.
Using a polymer bead composition containing specific ethylene monomers, chain transfer agents, phenolic compounds and surface coating agents, the degree of crosslinking and the ratio of additives was adjusted to prepare excellent heat resistance and above 310°C and Polymer beads with uniform particle size distribution.
The heat resistance of polymer beads and color change suppression at high temperatures is achieved, ensuring their stability and performance consistency in optical applications.
Smart Images

Figure CN118891297A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This specification claims the benefit of the application date of Application No. 10-2022-0044652 filed with the Korean Intellectual Property Office on April 11, 2022, and its contents are incorporated herein. Technical Field
[0003] The present invention relates to a polymer bead composition and a method for preparing polymer beads using the same. Background Art
[0004] Background technologies related to the present disclosure are provided herein, which are not necessarily intended to be known technologies.
[0005] Polymer beads made of polymer materials are highly versatile particles used in various applications in the electrical and electronic fields, as well as in the chemical and biological fields. Currently, they are used as light diffusers in display devices, lighting fixtures, etc., and are also widely used as additives in various industrial fields such as coatings, plastic molded products, and cosmetics. Different physical properties are required depending on the application.
[0006] The thermal decomposition of polymer beads is divided into chain end unzipping at 250-300°C and unzipping by random scission at above 300°C according to the temperature range. For the thermal decomposition caused by chain end unzipping at around 300°C, due to the free radical polymerization characteristics of the polymer beads prepared by suspension polymerization, a heterogeneous reaction including vinyl groups (the vinyl groups have unsaturated bonds at the ends of the polymer chains generated during the termination reaction) is accompanied, free radicals are generated, resulting in unzipping from the chain ends, causing thermal decomposition, and thus reducing heat resistance.
[0007] In the Korean patent publication No. 2012-0010366, a polymer bead is disclosed. A chain transfer agent and a silane monomer are added to a composition containing a specific vinyl monomer, and after adjusting the stirring conditions to prepare a suspension, it is used for polymerization. As a result, under the thermogravimetric analysis (TGA) conditions, i.e., when allowed to stand at 300°C for 10 minutes, a weight loss rate of less than 20% is exhibited, and at 600°C, the remaining amount of the polymer beads is more than 3%.
[0008] However, the heat resistance of the polymer beads at 320°C is slightly insufficient. Due to the copolymerization of silane added to improve the heat resistance, optical properties such as refractive index change. When applied to optical films or diffusers, differences in brightness and concealment will occur due to the change in refractive index.
[0009] Therefore, the present inventors have achieved a polymer bead composition comprising a specific monomer, a chain transfer agent, a phenolic compound and a surface coating agent, and have confirmed that highly heat-resistant polymer beads having improved heat resistance at a temperature of 310° C. or higher and with little weight loss have been prepared, thereby completing the present invention.
[0010] [Prior art literature]
[0011] [Patent Document]
[0012] (Patent Document 1) Korean Patent Publication No. 10-2012-0010366 Summary of the invention
[0013] Technical issues
[0014] One embodiment of the present invention provides a polymer bead composition and a method for preparing polymer beads using the same.
[0015] Technical Solution
[0016] One embodiment of the present invention provides a polymer bead composition, comprising: a polymer seed, wherein the polymer seed is derived from one or more vinyl monomers selected from the group consisting of an aromatic vinyl monomer, a (meth)acrylic acid alkyl ester monomer having 1 to 20 carbon atoms, and a (meth)acrylic acid fluoroalkyl ester monomer having 1 to 20 carbon atoms;
[0017] A chain transfer agent of the following chemical formula 1;
[0018] A phenolic compound, wherein the phenolic compound comprises the following chemical formula 2 at both ends and the following chemical formula 3 and the following chemical formula 4 on the middle chain; and
[0019] Surface coating agent.
[0020] [Chemical formula 1]
[0021] R-SH
[0022] [Chemical formula 2]
[0023]
[0024] [Chemical formula 3]
[0025]
[0026] [Chemical formula 4]
[0027]
[0028] Wherein, in the chemical formula 1,
[0029] R is a linear or branched alkyl group having 10 to 30 carbon atoms.
[0030] In addition, one embodiment of the present invention provides a method for preparing polymer beads, comprising: a step of preparing the above-mentioned polymer bead composition; and a step of polymerizing the polymer bead composition.
[0031] Effects of the Invention
[0032] According to one embodiment of the present invention, there is provided a polymer bead composition having excellent heat resistance and no color change at a temperature of 310° C. or higher.
[0033] One embodiment of the present invention provides a polymer bead composition having a uniform particle size distribution.
[0034] Another embodiment of the present invention provides a method for preparing polymer beads using the polymer bead composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The particle morphology of the polymer beads of Example 2 of the present invention is shown.
[0036] Figure 2 The results of TGA analysis of the polymer beads of Comparative Example 1 are shown.
[0037] Figures 3 to 6 The results of TGA analysis of the polymer beads of Examples 1 to 4 of the present invention are shown. DETAILED DESCRIPTION
[0038] Best Mode for Carrying Out the Invention
[0039] Hereinafter, before describing the present invention in detail, it should be understood that the terms used in the description are only used to describe specific embodiments and are not intended to limit the scope of the present invention which is only defined by the appended claims.
[0040] Furthermore, the terms or words used in this specification and claims shall not be interpreted in a limited manner as the ordinary meaning or the dictionary meaning, but shall be interpreted as the meaning and concept consistent with the technical idea of the present invention based on the principle that "the inventor can appropriately define the concept of the term in order to explain his own invention in the best way". However, unless otherwise specified, all technical terms and scientific terms used in this specification have the same meaning as those generally understood by ordinary technicians.
[0041] Unless otherwise stated, throughout this specification and claims, the terms "comprise", "comprises", "comprising" mean including the mentioned items, steps or some items and steps, and are not used as a meaning to exclude any certain other items, steps or some objects or steps.
[0042] On the other hand, unless explicitly stated to the contrary, various embodiments of the present invention may be combined with certain other embodiments. In particular, certain features indicated as preferred or advantageous may also be combined with certain features and certain features other than those indicated as preferred or advantageous.
[0043] In the present specification, (meth)acrylic acid means acrylic acid, methacrylic acid or a combination thereof.
[0044] One embodiment of the present invention provides a polymer bead composition, comprising: a polymer seed, wherein the polymer seed is derived from one or more selected from the group consisting of an aromatic vinyl monomer, a (meth)acrylic acid alkyl ester monomer having 1 to 20 carbon atoms, and a (meth)acrylic acid fluoroalkyl ester monomer having 1 to 20 carbon atoms; a chain transfer agent of the following chemical formula 1; a phenolic compound, wherein the phenolic compound comprises the following chemical formula 2 at both ends and the following chemical formula 3 and the following chemical formula 4 on the middle chain; and a surface coating agent.
[0045] [Chemical formula 1]
[0046] R-SH
[0047] [Chemical formula 2]
[0048]
[0049] [Chemical formula 3]
[0050]
[0051] [Chemical formula 4]
[0052]
[0053] Wherein, in the chemical formula 1,
[0054] R is a linear or branched alkyl group having 10 to 30 carbon atoms.
[0055] Conventional polymer beads are prepared by adding a chain transfer agent and a silane monomer to a composition including vinyl monomers. However, problems pointed out with polymer beads prepared by conventional preparation methods are that the particle size is several microns or more, and the particle size distribution shows a medium dispersion or above. In particular, when the polymer colloidal solution is used for preventing film adhesion, etc., it is necessary to have excellent heat resistance at the film processing temperature. However, with conventional methods, the physical properties change or yellowing occurs during processing at high temperatures, and the heat resistance cannot be ensured. In addition, the particle size distribution cannot be monodispersed, so its application range is limited.
[0056] Therefore, the present inventors have confirmed that when the polymer beads composition has the above components and is used to prepare polymer beads, the degree of crosslinking is adjusted, the heat resistance is excellent, and the particle size distribution is uniform, thereby completing the present invention.
[0057] In one embodiment of the present invention, the vinyl monomer may be one or more selected from the group consisting of aromatic vinyl monomers, (meth)acrylic acid alkyl ester monomers having 1 to 20 carbon atoms, and (meth)acrylic acid fluoroalkyl ester monomers having 1 to 20 carbon atoms.
[0058] In one embodiment of the present invention, the vinyl monomer may include at least one selected from the group consisting of methyl methacrylate, divinylbenzene, butyl methacrylate, trimethylolmethane tetraacrylate, trimethylolmethane triacrylate, trimethylolbutane triacrylate and ethylene glycol dimethacrylate. Preferably, the vinyl monomer may be styrene.
[0059] In one embodiment of the present invention, the polymer seed may include a solvent.
[0060] In one embodiment of the present invention, the solvent may be an aqueous solvent, such as water.
[0061] In one embodiment of the present invention, the polymer seed may be a mixture of the polymer seed derived from the vinyl monomer and the solvent.
[0062] In one embodiment of the present invention, based on the total weight of the polymer bead composition, the weight of the polymer seed and the weight of the solvent may be 40 to 60 parts by weight and 60 to 40 parts by weight, respectively.
[0063] In one embodiment of the present invention, the polymer bead composition may further include a styrene compound. In this case, the degree of crosslinking is adjusted, the heat resistance is excellent, and a uniform particle size distribution can be achieved.
[0064] In one embodiment of the present invention, the content of the styrene compound may be 10 to 40 parts by weight based on 100 parts by weight of the polymer seed. Preferably, it may be 10 to 35 parts by weight. When adjusted to the numerical range, the degree of crosslinking is adjusted, the heat resistance is excellent, and a uniform particle size distribution may be obtained.
[0065] In one embodiment of the present invention, the chain transfer agent (CT) is as shown in Chemical Formula 1, which can remove free radicals generated by the unsaturated bonds of the terminal vinyl groups, reduce the disproportionation termination reaction of the terminal vinyl groups and unreacted monomers, thereby removing monomers that decompose at high temperatures and improving heat resistance.
[0066] [Chemical formula 1]
[0067] R-SH
[0068] In the chemical formula 1, R is a linear or side chain alkyl group having 10 to 30 carbon atoms.
[0069] In one embodiment of the present invention, R may be a linear alkyl group having 10 to 30 carbon atoms. Preferably, R may be a linear alkyl group. In this case, the reactivity of the chain transfer agent is improved, and the chain transfer reaction (chain transfer) is easily induced. The polymer beads prepared using such a chain transfer agent have an excellent heat resistance.
[0070] In one embodiment of the present invention, the chain transfer agent may be one or more selected from the group consisting of n-dodecyl mercaptan, tert-dodecyl mercaptan, and tert-hexadecanethiol. Preferably, the chain transfer agent may be n-dodecyl mercaptan.
[0071] In one embodiment of the present invention, the chain transfer agent may be CAS 112-55-0.
[0072] In one embodiment of the present invention, the content of the chain transfer agent may be 0.1 to 0.8 parts by weight based on 100 parts by weight of the polymer seed. Preferably, it may be 0.3 to 0.5 parts by weight. When the chain transfer agent is used in excess, a large amount of polymers with a small molecular weight will be generated. Although the degree of reaction completion is improved, the solvent resistance is reduced, and there will be process difficulties when manufacturing optical films. Therefore, in order to provide heat resistance while also having solvent resistance, it is extremely important to use an appropriate amount of chain transfer agent. Specifically, within the numerical range, heat resistance can be improved, polymerization stability can be maintained, and reactants can be prevented from agglomerating.
[0073] In one embodiment of the present invention, by using the chain transfer agent together with the phenolic compound of the present invention, it is possible to prevent thermal decomposition from starting at 310°C or above, thereby improving operating efficiency, improving heat resistance, and reducing weight loss. However, when the chain transfer agent is used together with an antioxidant such as a phosphorus compound, an amine compound, a hindered amine compound, or a sulfur compound instead of the phenolic compound of the present invention, heat resistance and reactivity tend to decrease.
[0074] In one embodiment of the present invention, the phenolic compound may include the following chemical formula 2 at both ends, and the following chemical formula 3 and the following chemical formula 4 in the middle chain. In addition, the middle chain may include 8 to 15 carbon atoms and form a straight chain.
[0075] [Chemical formula 2]
[0076]
[0077] [Chemical formula 3]
[0078]
[0079] [Chemical formula 4]
[0080]
[0081] In one embodiment of the present invention, the polymer bead composition includes a phenolic compound, and the phenolic compound includes the following chemical formula 2 at both ends and the following chemical formula 3 and the following chemical formula 4 in the middle chain. The OH group of the chemical formula 2 in the phenolic compound acts as a free radical inhibitor, and when used alone in the polymer bead composition, it reduces the reaction, but by using it together with the chain transfer agent, it can easily capture and remove only the peroxide radical generated during the polymer decomposition reaction, thereby improving heat resistance. That is, the phenolic compound can be used as an antioxidant.
[0082] In one embodiment of the present invention, it is speculated that the phenolic compound includes Chemical Formula 2 at both ends and Chemical Formula 3 and Chemical Formula 4 in the middle chain, and the middle chain includes 8 to 15 carbon atoms to form a straight chain structure, thereby removing the polymer located at both ends of the phenolic compound where the peroxide free radicals generated during the polymer decomposition reaction are located to prevent the onset of thermal decomposition, thereby inhibiting the generation of smoke, improving heat resistance, inhibiting color changes and weight loss.
[0083] In one embodiment of the present invention, the content of the phenolic compound may be 0.1 to 1 part by weight based on 100 parts by weight of the polymer seed. Preferably, it may be 0.4 to 0.8 parts by weight. Within the numerical range, heat resistance is improved, polymerization stability is maintained, and agglomeration of reactants can be prevented.
[0084] In one embodiment of the present invention, a typical example of the phenolic compound is antioxidant 245, with CAS No. 36443-68-2.
[0085] In one embodiment of the present invention, the polymer bead composition includes a surface coating agent. By including the surface coating agent, the stability and dispersibility of the polymer substrate that can be used for various purposes can be improved.
[0086] In one embodiment of the present invention, the surface coating agent may be one or more selected from the group consisting of acrylate compounds, silane compounds, silicate compounds, phosphonate compounds, phosphate compounds, and acidic compounds.
[0087] In one embodiment of the present invention, as specific examples of the surface coating agent, a material selected from 3-trimethoxysilylpropyl methacrylate, silicon dioxide, tetraethyl orthosilicate, vinyl trimethoxysilane, vinyl triethoxysilane, allyl trimethoxysilane, allyl triethoxysilane, triethoxyvinyl silane, 3-(trimethoxysilyl)propyl acrylate, trimethoxy(7-octen-1-yl)silane, trimethoxymethylsilane, triethoxymethylsilane, ethyltrimethoxysilane, triethoxy(ethyl)silane, trimethoxyphenylsilane, trimethoxy(2-phenylethyl)silane, trimethoxy(propyl)silane, n-propyltriethoxysilane, isobutyl(trimethoxy)silane, isobutyltriethoxysilane, vinylphosphonic acid, vinylphosphine phosphonic acid, dimethyl ester, diethyl vinyl phosphonate, diethyl allyl phosphonate, diethyl (2-methylallyl) phosphonate, octyl phosphonic acid, butyl phosphonic acid, decyl phosphonic acid, hexyl phosphonic acid, hexadecyl phosphonic acid, n-dodecyl phosphonic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, propionic acid, butyric acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, undecanoic acid, tridecanoic acid, pentadecanoic acid, heptadecanoic acid, nonadecanoic acid, hexanedidecanoic acid, behenic acid, tricosanoic acid, tetracosanoic acid, pentacosanoic acid, hexacosanoic acid, heptadecanoic acid, octacosanoic acid, nonacosanoic acid, triacontylic acid, hexanedidecanoic acid, dotriacontylic acid, tritriacontylic acid, tetratriacontylic acid, pentacosanoic acid, hexatriacontylic acid (hexatriacontylic acid) acid), heptatriacontanoic acid, octadecanoic acid, oleic acid, linoleic acid, linolenic acid, arachidonic acid, hexadecatrienoic acid, octadecatetraenoic acid, eicosatrienoic acid, eicosatetraenoic acid, eicosapentaenoic acid, eicosapentaenoic acid, docosapentaenoic acid, clupanodonic acid At least one of the group consisting of oleic acid, docosahexaenoic acid, tetracosapentaenoic acid, tetracosahexaenoic acid, octadecatrienoic acid, eicosadienoic acid, docosadienoic acid, docosatetraenoic acid, docosapentaenoic acid, tetracosatetraenoic acid, tetracospentaenoic acid, 5-dodecenoic acid, 7-tetradecenoic acid, palmitoleic acid, vaccenic acid, eicosenoic acid, 15-eicosenoic acid, 17-tetracosenoic acid, elaidic acid, 11-eicosenoic acid, eicosatrienoic acid, erucic acid, nervonic acid, rumenic acid, octadecatrienoic acid, orchidic acid, eleostearic acid, catalpaic acid, punicic acid, rumenic acid, loquat acid, octadecatrienoic acid, pinolenic acid and podocarpic acid.
[0088] In one embodiment of the present invention, the content of the surface coating agent may be 10 to 35 parts by weight based on 100 parts by weight of the polymer seed. Preferably, it may be 18 to 35 parts by weight, 18 to 30 parts by weight, or 20 to 25 parts by weight. Within the numerical range, the stability and dispersibility of the polymer may be improved.
[0089] In one embodiment of the present invention, the polymer beads composition may include one or more selected from the group consisting of a cross-linking agent and an initiator.
[0090] In one embodiment of the present invention, the cross-linking agent may be a compound including two or more unsaturated carbon atoms.
[0091] In one embodiment of the present invention, the crosslinking agent may include a crosslinking agent selected from 1,2-ethylene glycol diacrylate, 1,3-propylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butylene glycol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, divinylbenzene, ethylene glycol diacrylate, propylene glycol diacrylate, butylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, polybutylene glycol diacrylate, allyl acrylate, 1,2-ethylene glycol dimethacrylate, 1,3-propylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, divinylbenzene, ethylene glycol diacrylate, propylene glycol diacrylate, butylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, polybutylene glycol diacrylate, allyl acrylate, 1,2-ethylene glycol dimethacrylate, 1,3-propylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol diacrylate At least one selected from the group consisting of dimethacrylate, 1,5-pentanediol dimethacrylate, 1,6-hexanediol dimethacrylate, ethylene glycol dimethacrylate, propylene glycol dimethacrylate, butanediol dimethacrylate, triethylene glycol dimethacrylate, trimethylolpropane triacrylate, polyethylene glycol dimethacrylate, trimethylolpropane triacrylate, polypropylene glycol dimethacrylate, butanediol dimethacrylate, triethylene glycol methacrylate, polyethylene glycol dimethacrylate, polypropylene glycol dimethacrylate, polybutylene glycol dimethacrylate, allyl methacrylate and diallyl maleate.
[0092] In one embodiment of the present invention, the cross-linking agent may include a first cross-linking agent and a second cross-linking agent that are different from each other, and a weight ratio of the first cross-linking agent to the second cross-linking agent may be 1:2 to 2:1.
[0093] In one embodiment of the present invention, the content of the crosslinking agent may be 15 to 75 parts by weight based on 100 parts by weight of the polymer seed. Preferably, 20 to 72 parts by weight may be used. If the content of the crosslinking agent is less than 15 parts by weight, the crosslinking agent cannot function as a crosslinking agent. If the content exceeds 75 parts by weight, it will be difficult to adjust the heat of reaction. If the degree of crosslinking of the particles increases, the reaction will be reduced due to the exothermic reaction.
[0094] In one embodiment of the present invention, the initiator includes a free radical initiator. The free radical initiator can be a fat-soluble initiator or a water-soluble initiator. The fat-soluble initiator can include one or more selected from the group consisting of benzoyl peroxide, azobisisobutyronitrile, azodiphenylbutyronitrile and azobis(cyclohexanecarbonitrile). The water-soluble initiator includes one or more selected from the group consisting of potassium sulfate, sodium sulfate, ammonium persulfate and azo water-soluble initiators.
[0095] In one embodiment of the present invention, the content of the initiator may be 1 to 3 parts by weight based on 100 parts by weight of the polymer seed. If the content of the initiator is less than 0.1 parts by weight, the degree of reaction completion will be reduced, and if it exceeds 3 parts by weight, it will be difficult to adjust the reaction heat.
[0096] In one embodiment of the present invention, the particle size of the polymer seed may be 100 nm to 1000 nm. Specifically, it may be greater than 100 nm, greater than 200 nm, greater than 300 nm, greater than 400 nm, greater than 500 nm, greater than 600 nm, greater than 700 nm, greater than 800 nm, greater than 900 nm, or greater than 1000 nm. Within the above range, the structural stability of the polymer seed may be improved, and the particle size distribution may be kept uniform.
[0097] In one embodiment of the present invention, the polymer bead composition may further include a dispersion stabilizer.
[0098] In one embodiment of the present invention, the dispersion stabilizer may use 1,1-dichloroethane, potassium hydroxide, sodium hydroxide, adipic acid salt compounds, amide compounds, sulfonate compounds or mixtures thereof. Specifically, the dispersion stabilizer may use 1,1-dichloroethane, potassium hydroxide, sodium hydroxide, poly(1,6-hexamethylene adipate), N,N'-dibenzyl-1,6-diaminohexane, sodium 4-vinylbenzenesulfonate or mixtures thereof. More specifically, the dispersion stabilizer may use 1,1-dichloroethane, potassium hydroxide, sodium hydroxide, poly(1,6-hexamethylene adipate), N,N'-dibenzyl-1,6-diaminohexane, sodium 4-vinylbenzenesulfonate, etc.
[0099] In one embodiment of the present invention, the content of the dispersion stabilizer may be 0.01 to 1 part by weight based on 100 parts by weight of the polymer seed. Within the above numerical range, the dispersion stability may be improved.
[0100] In one embodiment of the present invention, the polymer bead composition may be in a colloidal state. In this case, the colloidal state means that the components contained in the polymer bead composition exist in nanoparticle size (1 micron to 100 microns). As a specific example, it means that the polymer seed, chain transfer agent, phenolic compound or surface coating agent, etc. exist in a state of being uniformly dispersed in a solvent in a nanoparticle size, wherein the polymer seed is derived from one or more vinyl monomers selected from the group consisting of aromatic vinyl monomers, (meth) alkyl acrylate monomers having 1 to 20 carbon atoms, and (meth) fluoroalkyl acrylate monomers having 1 to 20 carbon atoms.
[0101] One embodiment of the present invention provides a method for preparing polymer beads, comprising: a step of preparing the above-mentioned polymer bead composition; and a step of polymerizing the polymer bead composition.
[0102] In one embodiment of the present invention, the step of preparing the polymer bead composition may include the step of preparing a polymer seed by polymerizing one or more vinyl monomers selected from the group consisting of aromatic vinyl monomers, (meth)acrylic acid alkyl ester monomers having 1 to 20 carbon atoms, and (meth)acrylic acid fluoroalkyl ester monomers having 1 to 20 carbon atoms. In this case, the one or more vinyl monomers selected from the group consisting of the vinyl monomers, (meth)acrylic acid alkyl ester monomers having 1 to 20 carbon atoms, and (meth)acrylic acid fluoroalkyl ester monomers having 1 to 20 carbon atoms and the polymer seed may be the same as those described above for the polymer bead composition.
[0103] In one embodiment of the present invention, the step of polymerizing the vinyl monomer to prepare the polymer seed may include: a step of polymerizing at 50° C. to 90° C. for 5 to 48 hours. Within the above range, the shape of the prepared polymer seed can be maintained and the polymerization reaction can be started smoothly.
[0104] In the preparation method, the content of each component may be the same as that described for the polymer bead composition.
[0105] In one embodiment of the present invention, the step of polymerizing the polymer bead composition may include: polymerizing at 50° C. to 90° C. for 5 to 48 hours. The polymerization temperature may range from 60° C. to 80° C., and the polymerization reaction time may be 12 to 30 hours.
[0106] The polymerization step is performed by bringing the temperature of the reactor containing the emulsion to the temperature range under a nitrogen atmosphere and performing the polymerization at the temperature range, so that the chain transfer agent can react before the phenolic compound during the polymerization, compared with performing the polymerization while increasing the reactor temperature. Therefore, it is possible to prevent the thermal decomposition from starting at a temperature of 310° C. or higher, thereby improving the heat resistance.
[0107] In one embodiment of the present invention, the step of polymerizing the polymer bead composition may include the step of stirring at a stirring speed of 100 rpm to 1000 rpm. The stirring speed may be 200 rpm to 800 rpm or 300 rpm to 600 rpm. Within the above range, the polymerization stability is excellent and the physical properties of the obtained polymer beads are excellent.
[0108] Specific ways to implement the invention
[0109] Preferred embodiments are provided below to help understand the present invention. However, the following embodiments are merely examples of the present invention, and the scope of the invention is not limited by the following embodiments.
[0110] <Comparative Examples and Examples>
[0111] Comparative Example 1
[0112] In a cylindrical reactor, 11 parts by weight of methyl alcohol, 0.2 parts by weight of sodium 4-vinylbenzenesulfonate as a stabilizer, and 0.1 parts by weight of potassium persulfate as a polymerization initiator were added to 100 parts by weight of the polymer seed, and dissolved in an aqueous phase (76.7 parts by weight of water, 100 parts by weight of the polymer seed) by stirring at 280 rpm at room temperature under a nitrogen atmosphere. In the dissolved substance, 12 parts by weight of styrene monomer was mixed with 100 parts by weight of the polymer seed, stirred, and polymerized at 70° C. for 24 hours to obtain a polystyrene polymer seed.
[0113] 45 parts by weight of the polystyrene polymer seed obtained by the polymerization were mixed with 55 parts by weight of water.
[0114] Based on 100 parts by weight of the mixed material, 33 parts by weight of styrene, 22 parts by weight of 3-(trimethoxysilyl)propyl acrylate as a surface coating agent, 0.6 parts by weight of azobisisobutyronitrile as an initiator, and 22.2 parts by weight of trimethylolprapanetriacrylate and divinylbenzene as crosslinking agents, totaling 44.4 parts by weight, were mixed to prepare a polymer bead composition.
[0115] Example 1
[0116] 45 parts by weight of the polystyrene polymer seed prepared in Comparative Example 1 and 55 parts by weight of water were mixed. Based on 100 parts by weight of the mixed material, 32 parts by weight of styrene, 0.4 parts by weight of CAS 112-55-0 as a chain transfer agent, 0.6 parts by weight of CAS 36443-68-2 as a phenolic compound, 22 parts by weight of 3-(trimethoxysilyl)propyl acrylate as a surface coating agent, 0.6 parts by weight of azobisisobutyronitrile as an initiator, and 22.2 parts by weight each of trimethylolprapanetriacrylate and divinylbenzene as crosslinking agents were mixed to obtain a polymer bead composition, totaling 44.4 parts by weight.
[0117] Example 2
[0118] In a cylindrical reactor, 19 parts by weight of methylalcohol, 0.08 parts by weight of sodium 4-vinylbenzenesulfonate as a stabilizer, and 0.1 parts by weight of potassium persulfate as a polymerization initiator are dissolved in an aqueous phase (68.82 parts by weight of water, based on 100 parts by weight of the polymer seed) under nitrogen atmosphere at room temperature at 280 rpm. 12 parts by weight of styrene monomer are mixed with 100 parts by weight of the polymer seed, stirred, and polymerized at 70° C. for 24 hours to obtain a polystyrene polymer seed.
[0119] 45 parts by weight of the polystyrene polymer seed obtained as a result of the polymerization and 55 parts by weight of water were mixed.
[0120] Based on 100 parts by weight of the mixed material, 32 parts by weight of styrene, 0.4 parts by weight of CAS 112-55-0 as a chain transfer agent and 0.6 parts by weight of CAS 36443-68-2 as a phenolic compound, 14 parts by weight of 3-(trimethoxysilyl)propyl acrylate as a surface coating agent, 0.6 parts by weight of azobisisobutyronitrile as an initiator, and 26.2 parts by weight each of trimethylolprapanetriacrylate and divinylbenzene as crosslinking agents were mixed to obtain a polymer bead composition.
[0121] Example 3
[0122] 45 parts by weight of the polystyrene polymer seed prepared in Example 2 and 55 parts by weight of water were mixed. Based on 100 parts by weight of the mixed material, 13 parts by weight of styrene, 0.4 parts by weight of CAS112-55-0 as a chain transfer agent and 0.6 parts by weight of CAS 36443-68-2 as a phenolic compound, 14 parts by weight of 3-(trimethoxysilyl)propyl acrylate as a surface coating agent, 0.6 parts by weight of azobisisobutyronitrile as an initiator, and 35.7 parts by weight each of trimethylolprapanetriacrylate and divinylbenzene as crosslinking agents were mixed to prepare a polymer bead composition in a total of 71.4 parts by weight.
[0123] Example 4
[0124] 45 parts by weight of the polystyrene polymer seed prepared in Example 2 and 55 parts by weight of water were mixed. Based on 100 parts by weight of the mixed material, 32 parts by weight of styrene, 0.4 parts by weight of CAS112-55-0 as a chain transfer agent and 0.6 parts by weight of CAS 36443-68-2 as a phenolic compound, 14 parts by weight of 3-(trimethoxysilyl)propyl acrylate as a surface coating agent, 0.6 parts by weight of azobisisobutyronitrile as an initiator, and 52.4 parts by weight of divinylbenzene as a crosslinking agent were mixed to prepare a polymer bead composition.
[0125] <Preparation of polymer beads>
[0126] Polymer beads were prepared using the polymer bead compositions of the comparative examples and the examples, respectively.
[0127] Specifically, each polymer bead composition was polymerized in a nitrogen atmosphere at 70° C. and 280 rpm for 24 hours to prepare polymer beads. These are comparative polymer beads and polymer beads 1 to 4, respectively.
[0128] <Experimental example>
[0129] Experimental Example 1: Appearance Evaluation
[0130] The polymer beads prepared by using the polymer beads composition of the comparative example and the example were dried, and solid samples were collected to analyze the particle morphology by scanning electron microscopy (SEM, scanning electron microscopy, COXEM).
[0131] Figure 1 The particle morphology of the polymer beads of Inventive Example 2 is shown. Specifically, it can be confirmed that the polymer beads of Inventive Example 2 have a uniform particle size and a smooth surface.
[0132] Experimental Example 2: Heat resistance evaluation
[0133] The heat resistance of the polymer beads prepared using the polymer bead compositions of the comparative examples and examples, specifically the comparative polymer beads and polymer beads 1 to 4, was evaluated by thermogravimetric analysis (TGA).
[0134] It was confirmed that the comparative polymer beads prepared in Comparative Example 1 showed a relatively low thermal decomposition temperature ( Figure 2 ), in Example 1 ( Figure 3 )、Example 2( Figure 4 )、Example 3( Figure 5 ) and Example 4 ( Figure 6 ) exhibited a relatively high thermal decomposition temperature for each of the polymer beads 1 to 4 obtained. Specifically, Figure 2 It can be seen that the comparative polymer beads prepared in Comparative Example 1 thermally decomposed at around 307°C, while Figures 3 to 6 It can be seen that the polymer beads 1 to 4 obtained in Examples 1 to 4 did not undergo thermal decomposition at least at 314° C., and in Example 4, thermal decomposition was confirmed to occur at around 330° C. In other words, it can be confirmed that the polymer beads of the present invention have excellent thermal stability, that is, excellent heat resistance.
Claims
1. A polymer bead composition comprising: A polymer seed derived from one or more selected from the group consisting of an aromatic vinyl monomer, an alkyl (meth)acrylate monomer having 1 to 20 carbon atoms, and a fluoroalkyl (meth)acrylate monomer having 1 to 20 carbon atoms; A chain transfer agent of the following chemical formula 1; A phenolic compound, wherein the phenolic compound comprises the following chemical formula 2 at both ends and the following chemical formula 3 and the following chemical formula 4 on the middle chain; and Surface coating agents; [Chemical formula 1] R-SH [Chemical formula 2] [Chemical formula 3] [Chemical formula 4] Wherein, in the chemical formula 1, R is a linear or branched alkyl group having 10 to 30 carbon atoms.
2. The polymer bead composition according to claim 1, wherein The vinyl monomer includes at least one selected from the group consisting of methyl methacrylate, divinylbenzene, butyl methacrylate, trimethylolmethane tetraacrylate, trimethylolmethane triacrylate, trimethylolpropane triacrylate, trimethylolbutane triacrylate, and ethylene glycol dimethacrylate.
3. The polymer bead composition according to claim 1, wherein Also included are styrene compounds.
4. The polymer bead composition according to claim 3, wherein Based on 100 parts by weight of the polymer seed, the content of the styrene compound is 10 to 40 parts by weight.
5. The polymer bead composition according to claim 1, wherein The chain transfer agent is one or more selected from the group consisting of n-dodecyl mercaptan, tert-dodecyl mercaptan, and tert-hexadecanethiol.
6. The polymer bead composition according to claim 1, wherein Based on 100 parts by weight of the polymer seed, the content of the chain transfer agent is 0.1 to 0.8 parts by weight.
7. The polymer bead composition according to claim 1, wherein Based on 100 parts by weight of the polymer seed, the content of the phenolic compound is 0.1 to 1 part by weight.
8. The polymer bead composition according to claim 1, wherein The surface coating agent is one or more selected from the group consisting of acrylate compounds, silane compounds, silicate compounds, phosphonate compounds, phosphate compounds, and acidic compounds.
9. The polymer bead composition according to claim 1, wherein Based on 100 parts by weight of the polymer seed, the content of the surface coating agent is 10 to 35 parts by weight.
10. The polymer bead composition according to claim 1, wherein The present invention comprises at least one selected from the group consisting of a cross-linking agent and an initiator.
11. The polymer bead composition according to claim 10, wherein The crosslinking agent is selected from 1,2-ethylene glycol diacrylate, 1,3-propylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butylene glycol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, divinylbenzene, ethylene glycol diacrylate, propylene glycol diacrylate, butylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, polybutylene glycol diacrylate, allyl acrylate, 1,2-ethylene glycol dimethacrylate, 1,3-propylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, One or more selected from the group consisting of 1,4-butanediol dimethacrylate, 1,5-pentanediol dimethacrylate, 1,6-hexanediol dimethacrylate, ethylene glycol dimethacrylate, propylene glycol dimethacrylate, butanediol dimethacrylate, triethylene glycol dimethacrylate, trimethylolpropane triacrylate, polyethylene glycol dimethacrylate, polypropylene glycol dimethacrylate, butanediol dimethacrylate, triethylene glycol methacrylate, polyethylene glycol dimethacrylate, polypropylene glycol dimethacrylate, polybutylene glycol dimethacrylate, allyl methacrylate and diallyl maleate.
12. The polymer bead composition according to claim 10, wherein The cross-linking agent includes a first cross-linking agent and a second cross-linking agent that are different from each other, and a weight ratio of the first cross-linking agent to the second cross-linking agent is 1:2 to 2:
1.
13. The polymer bead composition according to claim 10, wherein Based on 100 parts by weight of the polymer seed, the content of the crosslinking agent is 15 to 75 parts by weight.
14. The polymer bead composition according to claim 1, wherein The particle size of the polymer seed is 100 nm to 1000 nm.
15. The polymer bead composition according to claim 1, wherein The polymer bead composition is in a colloidal state.
16. A method for preparing polymer beads, comprising: A step of preparing a polymer bead composition according to any one of claims 1 to 15; and A step of polymerizing the polymer bead composition.
17. The method for preparing polymer beads according to claim 16, wherein: The steps of preparing the polymer bead composition include: A step of preparing a polymer seed by polymerizing one or more vinyl monomers selected from the group consisting of aromatic vinyl monomers, (meth)acrylic acid alkyl ester monomers having 1 to 20 carbon atoms, and (meth)acrylic acid fluoroalkyl ester monomers having 1 to 20 carbon atoms.
18. The method for preparing polymer beads according to claim 17, wherein: The step of polymerizing the vinyl monomer to prepare the polymer seed comprises: A step of polymerizing at 50°C to 90°C for 5 to 48 hours.
19. The method for preparing polymer beads according to claim 16, wherein: The step of polymerizing the polymer bead composition includes the step of polymerizing at 50° C. to 90° C. for 5 to 48 hours.
20. The method for preparing polymer beads according to claim 16, wherein: The step of polymerizing the polymer bead composition includes the step of stirring at a stirring speed of 100 rpm to 1000 rpm.