Dispersions of carbon black in alkylene glycols and in situ polymerization of polyesters therefrom

By adding specific diols and surface treatment agents to the carbon black dispersion, a high load carbon black dispersion is solved, and the problems of low economic efficiency and high temperature instability of carbon black filling methods in the prior art are improved, and polyester fibers are improved blackness and toughness, and maintain dispersibility at high temperatures.

CN118891327APending Publication Date: 2024-11-01CABOT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031612.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-21
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, the carbon black filling method used to prepare filled polymer fibers is less economical, and the carbon black is unstable under high temperature conditions, affecting the production of polyester fibers.

Method used

Carbon black dispersions containing specific alkylene glycols, alicyclic glycols and aromatic glycols are used, and blended with diacids by surface treatment agents such as sulfonic acid groups and polyvinylpyrrolidone to form high loadings. Carbon black dispersion ensures stability at high temperatures.

Benefits of technology

A stable carbon black dispersion under high temperature conditions is achieved, allowing higher load carbon black to enter the polyester fiber, improving the blackness and toughness of the fibers, maintaining dispersion at high temperatures, and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891327A_ABST
    Figure CN118891327A_ABST
Patent Text Reader

Abstract

The carbon black dispersion comprises: a diol selected from the group consisting of an alkylene diol having 2 to 12 carbon atoms, an alicyclic diol having 6 to 24 carbon atoms, and an aromatic diol having 6 to 24 carbon atoms; 15-25% by weight of a modified carbon black having a BET surface area of 25-180 m2 / g measured prior to treatment, the modified carbon black being modified with a treatment agent comprising an organic group and a sulfonic acid group at a treatment agent concentration of 1.0-4.0 [mu] mol / m2 based on the nitrogen surface area (BET); and polyvinylpyrrolidone in an amount of 0-0.2: 1 relative to the amount of the modified carbon black. The carbon black dispersion contains less than 2.5% by weight of water, and the carbon black dispersion has a D99 of less than 1 micron.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to high temperature stable organic dispersions of chemically treated carbon black and their use in the preparation of filled polymer fibers. Background Art

[0002] Fiber manufacturers are seeking alternatives to the bath dying process for coloring polyester fibers. Carbon black can be used as a substitute for organic dyes. The pigment can be blended directly with virgin polyester and then spun into fibers. Alternatively, the pigment can be blended with a polymer to form a masterbatch. The masterbatch can then be combined with additional unfilled polymers and spun into fibers.

[0003] It would be desirable to have a more economical method of preparing carbon black filled polyester fibers. Summary of the invention

[0004] In one embodiment, the carbon black dispersion comprises: a diol selected from an alkylene diol having 2 to 12 carbon atoms, an alicyclic diol having 6 to 24 carbon atoms, and an aromatic diol having 6 to 24 carbon atoms; 15 to 25% by weight of a modified carbon black having a carbon black content of 25 to 180 m / s measured before treatment. 2 The modified carbon black is treated with a treating agent comprising an organic group and a sulfonic acid group to have a BET surface area of ​​1.0-4.0 μmol / m based on a nitrogen surface area (BET). 2 and polyvinyl pyrrolidone in an amount of 0-0.2:1 relative to the modified carbon black. The carbon black dispersion contains less than 2.5 wt% of water, and the D99 of the carbon black dispersion is less than 1 micron.

[0005] The diol may be ethylene glycol and may contain less than 1 wt % water. The modified carbon black may have attached phenylsulfonic acid groups. After 2 hours of incubation at 150° C., the D99 of the dispersion may be less than 1 micron. Polyvinyl pyrrolidone may be the sole dispersant. The number average molecular weight of the polyvinyl pyrrolidone may be 3000-80000 g / mol, such as 5000-30000 g / mol or 10,000-15000 g / mol.

[0006] In another embodiment, a method of making a polyester comprises forming a pigmented mixture by combining a carbon black dispersion with any of:

[0007] A) a diacid selected from aromatic dicarboxylic acids having 6 to 24 carbon atoms, alicyclic dicarboxylic acids having 6 to 24 carbon atoms and alkane dicarboxylic acids having 2 to 12 carbon atoms, or

[0008] B) a partially polymerized mixture of: B1) a diacid selected from aromatic dicarboxylic acids having 6 to 24 carbon atoms, alicyclic dicarboxylic acids having 6 to 24 carbon atoms and alkane dicarboxylic acids having 2 to 12 carbon atoms; and B2) a diol selected from alkylene glycols having 2 to 12 carbon atoms, alicyclic diols having 6 to 24 carbon atoms and aromatic diols having 6 to 24 carbon atoms.

[0009] The colored mixture is polymerized to form a polyester. The diacid may be terephthalic acid, and the polyester may be polyethylene terephthalate. The method may further include cutting the polyester into chips. The resulting polyester chips may contain 15-30% by weight of the modified carbon black or 0.5-3% by weight of the modified carbon black, such as 0.5-30% by weight of the modified carbon black.

[0010] In another embodiment, the polyester scrap comprises: 0.5-3 wt. % of a modified carbon black having a carbon black content of 25-180 m / s measured before treatment; 2 The modified carbon black is treated with a treating agent comprising an organic group and a sulfonic acid group to have a BET surface area of ​​1.0-4.0 μmol / m based on a nitrogen surface area (BET). 2 and polyvinyl pyrrolidone in an amount of 0-0.2:1 relative to the modified carbon black. The polyester may be polyethylene terephthalate and may have a molecular weight Mn of 17,000-25,000.

[0011] In another embodiment, the polyester fiber comprises a treating agent with 1.0-4.0 μmol / m based on nitrogen surface area (BET). 2 A modified carbon black modified with a treating agent concentration of , wherein the treating agent comprises an organic group and a sulfonic acid group, wherein the polyester fiber has a jetness of 11-18 and any one or both of the following: a fiber tenacity of 2.0-3.5 cN / dtex and an elongation at break of 10-30%. Preferably, the modified carbon black has a fiber tenacity of 25-180 m / s measured before treatment. 2 / g of BET surface area.

[0012] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are intended to provide further explanation of the invention as claimed. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The present invention is described with reference to the several figures of the accompanying drawings, in which Figure 1 , 2 , 3, 4 and 5 are graphs showing the storage modulus of ethylene glycol dispersions of various surface treated carbon blacks as a function of angular frequency. DETAILED DESCRIPTION

[0014] The carbon black dispersion comprises: a diol selected from an alkylene diol having 2 to 12 carbon atoms, an alicyclic diol having 6 to 24 carbon atoms, and an aromatic diol having 6 to 24 carbon atoms; 15 to 25% by weight of a modified carbon black having a carbon black content of 25 to 180 m / s measured before treatment; 2 The modified carbon black is treated with a treating agent comprising an organic group and a sulfonic acid group to have a BET surface area of ​​1.0-4.0 μmol / m based on a nitrogen surface area (BET). 2 and polyvinyl pyrrolidone in an amount of 0-0.2:1 relative to the modified carbon black. The carbon black dispersion contains less than 2.5 wt% of water, and the D99 of the carbon black dispersion is less than 1 micron.

[0015] Chemically treated carbon black products enable higher loadings of pigment to be incorporated into organic solvents compared to conventional pigments. This in turn allows greater amounts of carbon black to be incorporated into polyester fibers, providing higher jetness, even in thinner filaments. In addition, because the chemically treated carbon black is pre-dispersed in the solvent, the final polymer product exhibits improved dispersion of the carbon black. This allows the fibers to be pulled out to greater lengths without breaking.

[0016] Preferably, the carbon black dispersion is stable after exposure to high temperatures. High temperature stability of the dispersion provides several advantages. For example, it is desirable that the dispersion be stable under high temperature conditions used to produce polyester. In some embodiments, the D99 of the dispersion is less than 1.0 microns after incubation at 150°C for 2 hours.

[0017] The chemically treated carbon black product may be present in the dispersion in an amount of at least 18 wt %, such as 20-25 wt %. Lower amounts of carbon black may also be used. Those skilled in the art will recognize that the amount of chemically treated carbon black in a polymer prepared from a carbon black dispersion will depend in part on the loading of the chemically treated carbon black in the dispersion and the amount of dispersion used in the polymerization process.

[0018] Suitable carbon black is known to those skilled in the art and includes channel black, furnace black, gas black and lamp black. Carbon black from various suppliers can be used. Some commercially available carbon blacks are sold with Regal®, Black Pearls®, Elftex®, Monarch®, Mogul®, Spheron®, Sterling® and Vulcan® trademarks, and are available from Cabot Corporation. Other commercially available carbon blacks include, but are not limited to, Raven®, Statex®, Furnex® and Neotex® trademarks sold carbon blacks, CD and HV lines available from Columbian Chemicals, and Corax®, Durax®, Ecorax®, Printex® and Purex® products available from Orion Engineered Carbons. Furnace black is preferably used in the embodiments provided herein. To prepare polyester fibers as described elsewhere herein, it may be desirable to use carbon blacks that are particularly suitable for use in fibers, such as Elftex 570, Regal 660, and Black Pearls 5550, 4560i, 5160, 3560, and 5560 carbon blacks from Cabot Corporation, and Printex L6 SQ and alpha SQ and Arosperse® 11, 138, and 26 carbon blacks from Orion Engineered Carbons.

[0019] The carbon blacks described herein may exhibit a specific range of nitrogen surface areas (BET, measured according to ASTM D6556). As used herein, the BET surface area of ​​the chemically treated carbon black is the surface area of ​​the carbon black prior to modification. In some embodiments, the BET surface area of ​​the chemically treated carbon black is 25 m 2 / g-180m 2 / g, 30m 2 / g-150m 2 / g, or 50m 2 / g-125m 2 / g. If the surface area of ​​the carbon black is too high, the carbon black will be difficult to disperse even with the surface treatment levels specified herein. In addition, the viscosity of the dispersion will be higher at a given solids loading, and / or the dispersion may exhibit gel-like behavior under shear (i.e., low dependence of the storage modulus on angular frequency).

[0020] Chemically treated carbon black can have various primary particle sizes known in the art. For example, carbon black can have 5nm-100nm, including 10nm-80nm and 15nm-50nm primary particle sizes. In some embodiments, carbon black can have a primary particle size less than 200, less than 100 or less than 75nm. In addition, carbon black can also have a wide range of OAN values ​​(oil adsorption values, measured according to ASTM D2414), which is a measure of the structure or branching of the pigment. For example, before surface modification, carbon black can have an OAN value of 25-250ml / 100g, such as 30-150ml / 100g or 50-100ml / 100g.

[0021] Alternatively, chemically treated carbon black can be prepared by any method known to those skilled in the art so that the sulfonic acid group is connected to the pigment. For example, the sulfonic acid group can be connected to carbon black using methods such as diazonium chemicals (chemistry), azo chemicals, peroxide chemicals, sulfonation and cycloaddition chemicals. Chemically treated carbon black can be prepared using any method known to those skilled in the art so that the organic chemical group is connected to the pigment. For example, chemically treated pigment can be prepared using the method described in U.S. Patent Nos. 5,554,739, 5,707,432, 5,837,045, 5,851,280, 5,885,335, 5,895,522, 5,900,029, 5,922,118, 6,042,643 and 6,337,358, the description of which is fully incorporated herein by reference. Compared with the dispersant type method using, for example, polymers and / or surfactants, such a method ensures a more stable connection of the organic group on carbon black. Other methods for preparing chemically treated carbon black include reacting carbon black with an available functional group with a reactant (reagent) containing an organic group, such as described in U.S. Patent No. 6,723,783, which is incorporated herein by reference in its entirety. Such functional pigments can be prepared using the method described in the document introduced above. In addition, chemically treated carbon black containing the functional group connected can also be prepared by the method described in U.S. Patent Nos. 6,831,194 and 6,660,075, U.S. Patent Publication Nos. 2003-0101901 and 2001-0036994, Canadian Patent No. 2,351,162, European Patent No. 1394221 and PCT Publication No. WO04 / 63289 and N. Tsubokawa, Polym. Sci., 17:417, 1992, each of which is also incorporated herein by reference in its entirety.

[0022] The diazo process disclosed in one or more of the documents of these introductions can be applicable to provide the reaction of at least one diazonium salt and carbon black pigment, and the carbon black pigment for example has not yet carried out the original or oxidized organic black pigment of surface chemical treatment with linking group.Diazonium salt is an organic compound with one or more diazo groups.In some techniques, diazonium salt can be prepared before reacting with the organic black pigment material, or more preferably, use the technical original position generation as described in the cited document.In-situ generation also allows to use unstable diazonium salt, for example alkyl diazonium salt, and avoids unnecessary processing or the operation of diazonium salt.In some techniques, nitrous acid and diazonium salt can both generate in-situ.

[0023] As is known in the art, diazonium salts can be produced by reacting primary amines, nitrites and acids. The nitrites can be any metal nitrites, preferably lithium nitrite, sodium nitrite, potassium nitrite or zinc nitrite, or any organic nitrites, such as isoamyl nitrite or ethyl nitrite. The acid can be any acid (inorganic or organic) that is effective in producing diazonium salts. Preferred acids include nitric acid HNO3, hydrochloric acid HCl and sulfuric acid H2SO4. Diazonium salts can also be produced by reacting primary amines with aqueous nitrogen dioxide solutions. Aqueous nitrogen dioxide solutions (NO2 / H2O) can provide the nitrous acid required to produce diazonium salts. Typically, when diazonium salts are produced from primary amines, nitrites and acids, two equivalents of acid are required based on the amine. In an in-situ process, one equivalent of acid can be used to produce diazonium salts. When the primary amine contains a strong acid group, it may not be necessary to add a separate acid in some processes. One or more acid groups of the primary amine can provide one or both of the required acid equivalents. When the primary amine contains a strong acid group, preferably, 0 to 1 equivalent of additional acid can be added to the process of generating the diazonium salt in situ. An example of such a primary amine that has shown excellent performance is p-aminobenzenesulfonic acid (benzenesulfonic acid) (sulfanilic acid).

[0024] Chemically treated carbon black comprises a carbon black pigment connected to at least one (individual) organic group, the organic group comprising an ion or an ionizable group. Chemically treated carbon black may be connected to at least one (individual) organic group having a formula -XZ, wherein X (which is the first chemical group directly connected to the carbon black) represents an arylene, a heteroarylene, an aralkylene, an alkylene or an alkarylene, and Z represents a sulfonic acid group. For example, -XZ may be phenylsulfonic acid or phenylsulfonate.

[0025] As noted, the group X can represent arylene or sub-heteroaryl, alkylene, sub-aralkyl or alkaryl. X can be directly connected to the pigment and further substituted by the Z group. X can be a linker group (linker group) (e.g., a linking diradical), which preferably can be directly bonded between the pigment surface and the Z group. Arylene and sub-heteroaryl can be aromatic groups, including but not limited to unsaturated cyclic hydrocarbons containing one or more rings. For sub-heteroaryl, one or more ring carbons of the aromatic group are replaced by heteroatoms. Heteroatoms are non-carbon atoms, such as N, S, O or other. The hydrogen of the aromatic group can be substituted or unsubstituted. As noted, X can represent sub-heteroaryl. When X is sub-aralkyl or alkaryl, the aromatic group can be arylene or sub-heteroaryl.

[0026] A heteroaryl group can be a linking group that includes, for example, at least one cyclic heterocyclic ring containing one or more heteroatoms (e.g., one, two, three or more heteroatoms). The cyclic heterocyclic ring can contain, for example, 3-12 ring member atoms, or 5-9 ring members, or, a 5-, 6-, 7-, or 8-membered ring. The cyclic heterocyclic ring can include, for example, at least one carbon atom, or at least two carbon atoms, or other numbers of carbon atoms. When multiple heteroatoms are used in the cyclic heterocyclic ring, the heteroatoms can be the same or different. The heterocyclic group can contain a single cyclic heterocyclic ring or a fused ring including at least one cyclic heterocyclic ring. A heteroaryl group can be, for example, an imidazolyl group, a pyrazolyl group, a thiazolyl group, an isothiazolyl ... Azolyl, Isopropylidene oxazolyl, thienylene, furanylene, fluorenylene, pyranylene, pyrrolylene, pyridylene, pyrimidylene, indolylene, isoindolylene, tetrazolylene, quinolylene, isoquinolylene, quinazolinylene, carbazolylene, purin ... pyrimidylene, pyrimidylene, In some embodiments, the alkylene group is a C1-C12 group. In some embodiments, the alkylene group is a C1-C3 group. In some embodiments, the alkylene group is a C1-C3 group. In some embodiments, the alkylene group is a C1-C12 ...

[0027] The group X may be further substituted with a group different from Z (eg, one or more alkyl or aryl groups).

[0028] As indicated, group Z is a sulfonic acid group. The sulfonic acid group may be in the acid form or may be anionic and may be associated with a counterion of opposite charge, including, for example, Na + , K + , Li + NH4 + 、NR'4 + The sulfonic acid group may include a counterion which is a monovalent metal salt such as Na + Salt, K + Salt or Li + Preferably, the organic group contains an aromatic group such as a phenyl or naphthyl group and a quaternary ammonium or quaternary The aromatic group is preferably directly attached to the carbon black. Quaternized cyclic amines and quaternized aromatic amines can also be used as organic groups. Thus, in this regard, N-substituted pyridines can be used. Compounds such as N-methyl-pyridinyl.

[0029] The level of attachment (treatment) of the sulfonic acid groups on the chemically treated carbon black should be sufficient to provide a stable dispersion of the chemically treated carbon black in the solvent. The level of attachment is provided as follows: number of moles of sulfonic acid groups / surface area of ​​the untreated carbon black (BET). For example, the ionic or ionizable groups can be present at 0.5-4.0 μmol / m 2 , 0.7-3.5μmol / m 2 or 1-3 μmol / m 2 In some embodiments where the organic group includes only one sulfonic acid group, the attachment levels of the organic group and the sulfonic acid group will be the same. When the organic group includes more than one sulfonic acid group, the attachment levels of the organic group and the sulfonic acid group will be different. In this case, the attachment levels of the groups (including the sulfonic acid groups) can also be quantified in equivalents / area. These attachment levels can be determined by methods known to those skilled in the art (e.g., elemental analysis).

[0030] Polyesters can be prepared using any polymerization method known to those skilled in the art. Suitable methods are disclosed in CN105839215, CN107326467, CN107447287, CN107624980, CN102731754, CN101691421, CN101338067, CN204237904U, JPS55066922A, RO79225, JPS58045227, and GB1049414, all of which are incorporated herein by reference. In a typical process, a dicarboxylic acid or its diester (e.g., wherein the carboxylic acid group is present as a methyl ester) is esterified (or transesterified) using a diol. For example, the diacid can be terephthalic acid. In addition to terephthalic acid, dicarboxylic acids such as 2,6-, 1,4-, 1,2- or 1,5-naphthalenedicarboxylic acid, isophthalic acid, isophthalic acid, adipic acid, glutaric acid, 1,4-cyclohexanedicarboxylic acid, p-hydroxybenzoic acid, diphenyldicarboxylic acid and diphenoxyethanedicarboxylic acid or 4,4'-biphenyldicarboxylic acid may also be used alone or in combination with terephthalic acid or in combination with each other. More generally, the dicarboxylic acid may be one or more of an aromatic dicarboxylic acid having 6 to 24 carbon atoms, an alicyclic dicarboxylic acid having 6 to 24 carbon atoms or an alkane dicarboxylic acid having 2 to 12 carbon atoms.

[0031] In certain embodiments, the diol is ethylene glycol. Typically, the diol may be one or more of an alkylene glycol having 2 to 12 carbon atoms, an alicyclic diol having 6 to 24 carbon atoms, or an aromatic diol having 6 to 24 carbon atoms. For example, the diol can be: an alkane diol having 2 to 8 carbon atoms, such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, diethylene glycol, trimethylene glycol, tetramethylene glycol, butanediol, hexanemethylene glycol, 2,2,4-trimethylpentane-1,3-diol, 1,6-hexanediol, etc.; an alicyclic diol having 6 to 24 carbon atoms, such as 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, etc.; an aromatic diol having 6 to 24 carbon atoms, such as bisphenol A, bisphenol S, hydroquinone, hydroxyphenol, xylylene glycol, etc.; or a mixture of two or more of these. Preferably, the diol contains less than 3 wt % water, such as less than 2 wt % water, less than 1 wt % water, less than 0.5 wt % water, or less than 0.1 wt % water. Any water will interfere with the esterification reaction and should be minimized.

[0032] Diol-carbon black dispersion can be prepared using any method known to those skilled in the art. For example, carbon black and diol can be combined using a media mill. Diol-carbon black dispersion preferably comprises 15-25 % by weight of modified carbon black, such as 18-23 % by weight, 15-20 % by weight, or 20-25 % by weight. Diol-carbon black dispersion preferably comprises less than 2.5 % by weight of water, such as less than 2 % by weight, less than 1.5 % by weight, less than 1 % by weight, less than 0.5 % by weight, or less than 0.1 % by weight of water.

[0033] The diol-carbon black dispersion optionally includes a dispersing aid. A preferred dispersing aid is polyvinyl pyrrolidone (PVP). PVP may be present in an amount of 0-0.2:1 (by weight) relative to carbon black, for example, up to 0.05:1, 0.05:1-0.1:1, or 0.1:1-0.15:1. PVP may have a number average molecular weight of 3000g / mol-80,000g / mol, for example 5000-60,000g / mol, 6000-50,000g / mol, 10000-30000g / mol or 10,000-15,000g / mol. Preferably, a lower molecular weight, for example, no more than 30,000g / mol or no more than 20,000g / mol, is used to promote the thermal stability of the carbon black dispersion. PVP may be harmful to thermal stability when the amount relative to carbon black is greater than 0.2:1. The appropriate amount of PVP will vary depending on the concentration of acidic groups on the carbon black.

[0034] The diol-carbon black dispersion can have a low level of particle agglomeration. In a preferred embodiment, the D99 of the dispersion is less than 1.0 micron. More preferably, the diol-carbon black dispersion is stable with respect to heat. For example, after incubation at 150° C. for 2 hours, the D99 of the dispersion can be less than 1 micron.

[0035] During the initial esterification step, high temperature is used to react the diol and diacid. Metal oxide or metal acetate catalysts or other catalysts known to those skilled in the art can be used to drive the reaction toward the desired final product. Phosphorus-containing compounds (e.g., alkyl or aryl phosphites or phosphates, or phosphorous acid, phosphoric acid, phosphonic acid, carboxylphosphonic acid or compounds of these (such as salts or esters)) can be used to deactivate the esterification. After the initial esterification, the reaction temperature is increased to promote further polycondensation, during which the oligomer chains can be combined by transesterification to release diols as reaction products. Any diols produced and residual unreacted diols are preferably removed to prevent reverse (depolymerization) reactions. Polycondensation can also be carried out under vacuum to further help remove diols. Antimony-based catalysts or other suitable catalysts can also be used during polycondensation. After polycondensation, the polymer can be further maintained at high temperatures and / or low temperatures to promote the formation of high molecular weight polymers and further promote the evaporation of diols. The resulting product can have a molecular weight Mn of 17000-25000.

[0036] The carbon black dispersion can be added to the reaction mixture at any stage in the reaction where diol is still consumed. For example, the carbon black dispersion can be added before, during or after the esterification. If the esterification is carried out in two steps (e.g. at two different temperatures and / or pressures), the carbon black dispersion can be added before, during or after either step. Similarly, the carbon black dispersion can be added before the polycondensation or at the beginning of the polycondensation.

[0037] In one embodiment, polymerization using the carbon black dispersion provided herein is used to produce a polyester masterbatch. The polyester masterbatch can have a carbon black loading of 15-30% by weight and can be blended with another polyester resin and stretched or spun into fibers. Carbon blacks with lower surface areas can be used to achieve higher loadings, but may not provide the desired tinting strength for black fibers.

[0038] Alternatively, the newly produced polymer can be directly stretched or spun into fibers. In this embodiment, the polymer can have a lower carbon black loading, for example, more typically 0.5-3% for the fiber itself. In this embodiment, the fiber can be formed in the same process immediately after polymerization, or the polymer can be extruded into fibers at a later time. For example, the polymer can be formed into chips or other small particles, rather than into fibers, which can be fed into an extruder and then stretched into fibers. In any of these embodiments, the fiber can have a jetness of 11-18. and either or both of the following: a fiber tenacity of 2.0-3.5 cN / dtex and an elongation at break of 10-30%.

[0039] The present invention will be further illustrated by the following examples, which are merely exemplary in nature.

[0040] Example

[0041] Example 1

[0042] The BET surface area is 230 m 2 / g and OAN of 69ml / 100g carbon black were introduced into a continuous pin pelletizer at a rate of 100kg / hr and mixed with sulfanilic acid (10.51kg / hr), 20% sodium nitrite solution (22.06kg / hr) and additional water (65-75kg / hr). The resulting surface treated carbon black was dried at 140°C.

[0043] In order to prepare ethylene glycol dispersion, carbon black is combined with ethylene glycol and polyvinyl pyrrolidone (K30, MW 40000-80000, Ashland) to prepare 20% dispersion, wherein, PVP: carbon black ratio is 0.15.50mL of the dispersion is added to a half pint paint can (paint can) (total material=50g) with 75g 0.8mm zirconium beads. The paint can is shaken (shake) on LAU DAS200 disperser for 6 hours and filtered through a paint screen (paint screen). Particle size measurement is carried out in Horiba L-950V2 laser scattering particle size distribution analyzer. The sample dispersion is diluted 1:10 in isopropanol, and then 1-2 drops are added to the analyzer to be filled with water (about 50mL) of the microflow chamber (Miniflow chamber). D90 is 3.1 microns and D99 is 6.1 microns.

[0044] Example 2

[0045] The BET surface area of ​​the treated samples was 83 m 2 / g and OAN is the carbon black of 64ml / 100g. In the plow mixer (plow mixer) with water cooling jacket and chopper (chopper), water is added and stirred until the water reaches the target temperature of 60°C. Carbon black (29% loading) and PABA (564μmol / g) are added to water (filling factor 67%), and the chopper is started. Once the reaction mixture reaches 50°C, 20% sodium nitrite solution is added in 20 minutes to reach the sodium nitrite of 1:1 molar ratio, thereafter, the reaction is continued for 2 hours at a temperature of 65°C with plow mixing and chopper. Sufficient water is added to the reactor so that the filling factor reaches 85%, and the reactor is cooled to 40°C. The slurry is discharged and diafiltered (diafilter) to remove residual salt, and then concentrated to a solid loading of 30%.

[0046] The obtained carbon black was combined with PVP10 polyvinyl pyrrolidone (MW=10000, Aldrich) and ethylene glycol in a half-pint paint can with 75g of 0.8mm zirconium oxide beads in the proportions given in Table 1. All formulations have 25% by weight of carbon black and 50g of total material except grinding media. The can was stirred in a LAU DAS 200 disperser for 4 hours. After mixing, the dispersion was separated from the grinding media with a paint filter, and the amount of the dispersion collected was recorded in grams (Table 1; N / A=too sticky to filter through the paint screen). The amount of material collected after sieving (i.e., not retained on the screen) is a rough indication of the viscosity of the dispersion. For thermal stability testing, 10g of various filtered dispersions were heat aged for 2 hours at 150°C in a glass vial covered with aluminum foil in an air circulation oven. Particle size measurements were performed in a Horiba L-950V2 laser scattering particle size distribution analyzer. The sample dispersion was diluted 1:10 in isopropanol and then 1-2 drops were added to the analyzer's microflow chamber filled with water (about 50 mL). Rheological measurements were performed at 25°C in an AR2000 rheometer from TA Instruments using a 40 mm steel parallel plate geometry. The step flow was used at 0.1-1000 s -1 The viscosity was measured at a shear rate of 100 rad / s and the storage modulus (g') was measured at an angular frequency of 0.1-500 rad / s.

[0047] Table 1

[0048]

[0049] The particle size distribution measurements of the dispersions before and after aging are shown in Table 2. The treated and untreated carbon black dispersions exhibited agglomeration upon aging, which was not improved with the use of PVP.

[0050] Table 2

[0051]

[0052] Example 3

[0053] The BET surface area is 117 m 2 / g and OAN of 97cc / 100g carbon black is treated with 1μmol / m 2 Butyl amino benzoate (Example 3A) or 3 μmol / m 2 Butyl aminobenzoate (Example 3B) is processed. 700g of carbon black is loaded into the mixing chamber of the chamber of 4 liters of ProcessAll Tilt-A-Mix plow mixer. The chamber is heated to 60 ℃, and butyl aminobenzoate (BAB), methylsulfonic acid (MSA) and water (Water 1) are sprayed into the mixing chamber in the amount listed in the following table 3 in about 1 minute. The reactants are mixed for about 1 minute with 60rpm, and then sodium nitrite and water (Water 2) are sprayed into the chamber in about 1 minute with the amount listed in the table 3. Air purge is set to about 10SLPM, and the reaction is carried out for 80 minutes, while continuing to mix. The reaction mixture is cooled to below (below) 40 ℃ and discharged into the tray. The tray is dried in an oven set to 105 ℃ until the moisture content is about 2.5 weight %.

[0054] Table 3

[0055]

[0056] The resulting carbon black and an untreated carbon black control were each combined with PVP (MW = 10000, Aldrich) and ethylene glycol in a half-pint paint can in the proportions given in Table 4 and 75 g of 0.8 mm zirconium oxide beads. All formulations had 25 wt% carbon black and 50 g of total material excluding grinding media. The can was agitated for 4 hours in a LAU DAS 200 disperser. After mixing, the dispersion was separated from the grinding media with a paint filter and the amount of dispersion recovered was recorded in grams (Table 4; N / A = too viscous to filter through a paint sieve). Aging and dispersion characterization were performed as described in Example 2. The data in Table 4 show that even at 3 μmol / m 2 At 1 μmol / m2 The particle size distributions in the dispersions of ) and untreated carbon black are thermally stable (Table 5), but the storage moduli of both dispersions no longer show a fluid-like variation of the storage modulus with frequency after heat treatment ( Figure 1 , solid squares - untreated carbon black, open squares - untreated carbon black dispersion after aging; solid circles (closed circles) - Example 3A, open circles (open circles) - Example 3A dispersion after aging), indicating that heating the dispersion results in a more gel-like behavior.

[0057] Table 4

[0058]

[0059] Table 5

[0060]

[0061] Example 4

[0062] The “pellet” or “slurry” treatments described below were performed with 3 or 6 μmol / m 2 The BET surface area of ​​sulfanilic acid treatment is 117 m 2 / g and carbon black with an OAN of 97cc / 100g.

[0063] In the "pellet" method, the chamber of a 4-liter ProcessAll Tilt-A-Mix plow mixer was heated to 70° C. A 1-gallon container was used to premix 300 g of carbon black and 18.3 or 36.6 g of sulfanilic acid and the mixture was charged to the mixer chamber, followed by the addition of 219.9 or 186.3 g of water (for 3 or 6 μmol / m, respectively). 2 The reaction mixture was mixed at maximum speed for 3 minutes. A 20% aqueous sodium nitrite solution was prepared and 42 or 84 g of the solution (for 3 or 6 μmol / m 2 After mixing for another 5 minutes, the treated pellets were discharged into a tray at a depth of about 2 cm. The tray was placed in a preheated oven at 110° C. and dried for about 2 hours until the moisture content was less than 2%.

[0064] In the "slurry" method, 300 g of carbon black and 18.3 or 36.6 g of sulfanilic acid were charged to the chamber of a 4 liter ProcessAll Tilt-A-Mix plow mixer with a water bath set at 55°C. Once the bath reached a temperature of over 50°C, 450 g of water was added to the mixing chamber and the plow was run at maximum speed for 30 minutes while the chopper function of the mixer was also activated. At this point, 43.8 or 87.6 g (for 3 or 6 μmol / m, respectively) of sulfanilic acid were added over 10 minutes. 2 20% sodium nitrite aqueous solution (treatment) was added to the reactor, after which the bath was set to 65°C. Any remaining nitrite from the delivery device was rinsed with 50mL of deionized water. The bath was kept at 65°C for another 2 hours, and the reaction mixture was agitated for another 2 hours with a plow and a chopper as described above. At this point, 188.2ml of deionized water was fed into the reaction chamber over 15 minutes; after the first five minutes, the bath was cooled to less than 50°C by setting the bath to 20°C. 15 minutes after the last addition of deionized water to the reaction chamber, the reactor was discharged. After the discharge, the reactor was rinsed twice with two 410mL aliquots of deionized water, after which the entire reaction mixture was diluted to a total mass of 2000g. The diluted mixture was diafiltered to remove residual salts and to a solids loading of 15% and then further concentrated to 22% solids. The resulting slurry was dried in a tray in an air circulation oven at 110°C until the moisture content was less than 2%.

[0065] Ethylene glycol dispersions with 20 wt% carbon black were prepared with polyvinylpyrrolidone (MW=10,000, Aldrich) at ratios of 0, 0.05, 0.1 and 0.2 (PVP / CB) as described in Example 1. The samples were characterized and aged as described in Example 2. The yields after dispersion filtration are shown in Table 6 below.

[0066] Table 6

[0067]

[0068] The results showed that a higher (6 μmol / m 2 ) levels of sulfanilic acid treatment produced less filterable dispersion. However, the yield did not vary with the concentration of PVP. Tables 7-9 show the particle size data for the samples before and after aging. The results show that the sulfanilic acid treated samples are relatively stable under aging regardless of the amount of PVP. However, the untreated carbon black dispersion showed agglomeration after aging.

[0069] Table 7

[0070]

[0071] Table 8

[0072]

[0073] Table 9

[0074]

[0075] Figure 2 and 3 The dispersions with the carbon blacks of Examples 4B and 4D are shown before aging ( Figure 2 ) and after ( Figure 3 ) Storage modulus G' as a function of angular frequency (squares - no PVP; circles - PVP: CB = 0.05; upward pointing triangles - PVP: CB = 0.1; downward pointing triangles - PVP: CB = 0.2; solid symbols - slurry method; open symbols - pellet method). Figure 2 The nearly horizontal curve of Example 4D without PVP indicates that this dispersion exhibits gel-like behavior, while the other dispersions exhibit more fluid-like behavior, with little change with the use of PVP. Figure 3 The dispersions of both aged dispersions of treated carbon black (Examples 4B and 4D) show that both dispersions exhibit gel-like behavior without the use of PVP. In contrast, the aged dispersions of Examples 4C and 4E do not exhibit a fluid-like change in storage modulus with frequency, indicating that the more highly treated carbon black (6 μmol / m 2 ) leads to a more gel-like dispersion ( Figure 4 ; squares - no PVP; circles - PVP:CB = 0.05; upward pointing triangles - PVP:CB = 0.1; downward pointing triangles - PVP:CB = 0.2; solid symbols - slurry method; open symbols - pellet method).

[0076] Dispersions were prepared using the carbon black of Examples 4B and 4D but using PVP40 (Mn = 40,000, Aldrich). Figure 5 Storage modulus data for Examples 4B and 4D with two different molecular weights of PVP (at a ratio of 0.1 relative to carbon black) are shown (solid symbols - initial dispersion; open symbols - aged dispersion; squares - dispersion with carbon black of Example 4B and PVP40; circles - dispersion with carbon black of Example 4B and PVP10; upward pointing triangles - dispersion with carbon black of Example 4B and PVP40; downward pointing triangles - dispersion with carbon black of Example 4D and PVP10). Although the effect of higher molecular weight on aging behavior is very small, the storage modulus of the samples with higher molecular weight PVP is consistently higher.

[0077] Example 5

[0078] The BET surface area is 60 m 2 / g and OAN of 47ml / 100g carbon black were introduced into a continuous pin granulator at a rate of 100kg / hr and mixed with sulfanilic acid (2.4kg / hr) and 20% sodium nitrite aqueous solution (5.56kg / hr) and 42.1kg / hr of additional water. The resulting surface-treated carbon black was then dried at 140 ° C. The resulting carbon black was used to produce polyethylene terephthalate (PET) crumbs with 1.5% by weight of carbon black. The ethylene glycol dispersion was prepared by mixing the formulations in the following table 10 (all amounts are in grams) at 1000rpm in a 1.5L reaction vessel using a high-speed overhead mixer. The carbon black dispersion was processed in an Eiger Mill M100 VSE sand mill (Engineered Mills, Inc.) with 1 mm diameter zirconia beads at a ratio of 1.5:1 (beads:dispersion) at 2800 rpm for five cycles until the D50 was less than 200 nm.

[0079] Table 10

[0080]

[0081] Polyethylene terephthalate crumb was prepared by combining 2594 g of terephthalic acid (PTA) and 1453 g of monoethylene glycol (1.5:1 molar ratio) in a 10-liter reactor. After manual mixing at 20-30° C. for 10 minutes, 225 g of one of the dispersions 5A-B and 1.5 g of ethylene glycol antimony catalyst were added. Esterification was carried out at 240° C. for 3 hours, after which the temperature was raised to 280° C. for polycondensation under vacuum (90 KPa) for 2 hours.

[0082] The properties of the obtained PET crumbs are shown in Table 11 below. Intrinsic viscosity was measured using an automatic viscometer IV400-2 from Hangzhou Zhongwang Technology Co. Ltd. according to GBT 14190. Number average molecular weight (Mn) and molecular weight distribution (MWD) were measured using a PL-GPC-50 gel permeation chromatography system from Agilent, wherein the test temperature was set to 40° C. and hexafluoroisopropanol was used as solvent. The melting point was determined using a Mettler Toledo Model DSC822e differential scanning calorimeter by heating the sample from 0° C. to 300° C. at 10 K / min and then cooling the sample back to 0° C. at the same ramp rate.

[0083] Table 11

[0084]

[0085] The chips were spun at 3000 m / min in a partially oriented yarn spinning machine using a 48-hole spinneret die (Zibo Linzi Fangchen Masterbatch Factory, Model FCF-1) and then processed in a draw texturing machine (Zibo Linzi Fangchen Masterbatch Factory, Model FCF-10) at a drawing ratio of 1.67 to produce a textured yarn having a yarn count of 150D / 45F and the properties listed in Table 12. Mechanical properties were performed in a temperature and humidity controlled room (25°C / 50% relative humidity) according to ASTM D2256. The fibers were knitted using a knitting machine (Wuxi Tianxiang Knitting Machinery Co., Ltd) model KU483T to make socks. The color of the socks ( ) were measured using a Hunter UltraScan colorimeter with the following settings: D (diffuse) / 8° geometry (Model SCI), 10° observer, D65 illuminant.

[0086] Table 12

[0087]

[0088] For the purpose of illustration and description, the foregoing description of the preferred embodiments of the present invention has been presented. It is not intended to be exhaustive or to limit the present invention to the precise form disclosed. Modifications and variations are possible in light of the above teachings or may be obtained from the practice of the present invention. The embodiments are selected and described to explain the principles of the present invention and its practical application so that those skilled in the art can utilize the present invention in various embodiments and with various modifications suitable for the intended specific use. The scope of the present invention is intended to be limited by the appended claims and their equivalents.

[0089] What is sought for protection is what is claimed in the present application as described in the appended claims.

Claims

1. A carbon black dispersion comprising: a diol selected from the group consisting of an alkylene diol having 2 to 12 carbon atoms, an alicyclic diol having 6 to 24 carbon atoms, and an aromatic diol having 6 to 24 carbon atoms; 15-25 wt. % of modified carbon black having a carbon black content of 25-180 m 2 The modified carbon black is treated with a treating agent comprising an organic group and a sulfonic acid group to obtain a BET surface area of ​​1.0-4.0 μmol / m based on a nitrogen surface area (BET). 2 Modification of treatment agent concentration; and Polyvinyl pyrrolidone, the amount of which relative to the modified carbon black is 0-0.2:1, wherein the carbon black dispersion contains less than 2.5 wt % water, and wherein the carbon black dispersion has a D99 of less than 1 micron.

2. The carbon black dispersion according to claim 1, wherein the diol is ethylene glycol.

3. The carbon black dispersion according to claim 1 or 2, containing less than 1% by weight of water.

4. The carbon black dispersion according to any one of claims 1 to 3, wherein the modified carbon black has attached phenyl sulfonic acid groups.

5. The carbon black dispersion according to any one of claims 1 to 4, wherein the D99 of the dispersion is less than 1 micron after incubation at 150°C for 2 hours.

6. The carbon black dispersion according to any one of claims 1 to 5, wherein the polyvinyl pyrrolidone is the only dispersant.

7. The carbon black dispersion according to any one of claims 1 to 6, wherein the number average molecular weight of the polyvinyl pyrrolidone is 3000-80000 g / mol, such as 5000-30000 g / mol or 10,000-15000 g / mol.

8. A method for preparing polyester, comprising: The carbon black dispersion according to any one of claims 1 to 7 is combined with any one of the following to form a pigmented mixture: A) a diacid selected from aromatic dicarboxylic acids having 6 to 24 carbon atoms, alicyclic dicarboxylic acids having 6 to 24 carbon atoms and alkane dicarboxylic acids having 2 to 12 carbon atoms, or B) a partially polymerized mixture of: B1) a diacid selected from aromatic dicarboxylic acids having 6 to 24 carbon atoms, alicyclic dicarboxylic acids having 6 to 24 carbon atoms and alkane dicarboxylic acids having 2 to 12 carbon atoms; and B2) a diol selected from alkylene glycols having 2 to 12 carbon atoms, alicyclic diols having 6 to 24 carbon atoms and aromatic diols having 6 to 24 carbon atoms; as well as The pigmented mixture is polymerized to form a polyester.

9. The process of claim 8, wherein the diacid is terephthalic acid.

10. The method of claim 8 or 9, wherein the polyester is polyethylene terephthalate.

11. The method of any one of claims 8-10, further comprising cutting the polyester into chips.

12. Polyester scrap prepared according to the method of any one of claims 8 to 11.

13. The polyester crumb according to claim 12, wherein the polyester crumb comprises 15-30 wt% of the modified carbon black.

14. The polyester scrap according to claim 12 or 13, wherein the polyester scrap comprises % by weight of the modified carbon black.

15. Polyester scraps, including: % by weight of modified carbon black having a carbon black content of 25-180 m 2 The modified carbon black is treated with a treating agent comprising an organic group and a sulfonic acid group to obtain a BET surface area based on the nitrogen surface area (BET) of μmol / m 2 Modification of treatment agent concentration; and Polyvinyl pyrrolidone, the amount of which relative to the modified carbon black is .

16. The polyester crumb according to claim 15, wherein the polyester is polyethylene terephthalate.

17. Polyester crumb according to claim 15 or 16, wherein the polyester has a molecular weight Mn of 17000-25000.

18. Polyester fibers, comprising: μmol / m 2 The modified carbon black is modified with a treating agent concentration of 10000 g / cm2, wherein the treating agent comprises an organic group and a sulfonic acid group, wherein the polyester fiber has a blackness of 11 to 18 and either or both of the following: cN / dtex fiber tenacity and 10-30% elongation at break.

19. The polyester fiber according to claim 18, wherein the modified carbon black has a carbon black content of 25-180 m / s measured before treatment. 2 / g of BET surface area.