Electrode assembly, secondary battery, and electric device

CN118891744APending Publication Date: 2024-11-01CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093620.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-11-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have difficulties in balancing high energy density, ultra-long life, and low cost. How to reduce expansion force without reducing the amount of negative electrode materials, avoid the risk of cycle diving, increase cruising range, and increase energy density.

Method used

By designing the relationship between the NP value of the electrode assembly and the storage ratio, set the lower limit and upper limit of NP, for example, 1.17-0.35S≤NP≤-0.41S+1.36, 50%≤S≤80%, and Reduce the total amount of negative electrode material, reduce expansion force, achieve low cost and long life, and at the same time, save space and increase energy density while ensuring that battery life during the life cycle is not affected.

Benefits of technology

It is possible to reduce the expansion force of secondary batteries, extend the life, increase energy density, reduce costs without affecting the cruising range, and solve the problem of battery cycle diving risk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891744A_ABST
    Figure CN118891744A_ABST
Patent Text Reader

Abstract

The invention provides an electrode assembly, a secondary battery and an electric device, and aims to consider that the corresponding NP value of the electrode assembly changes along with the increase of the number of cycles or the number of storage days. Therefore, the application considers the NP value design corresponding to the current capacity retention ratio not less than m and the storage ratio between 0.5 and 0.8, and the upper limit value of the NP is reduced along with the increase of the storage ratio, so that the NP value can be reduced, the total use amount of the negative electrode material can be reduced, the non-attenuated lithium embedding and removing capability of the silicon-doped negative electrode can be reused to the maximum extent, and the low cost is realized; and meanwhile, the total consumption of the negative electrode material is reduced, the expansibility of the secondary battery in circulation is reduced, the circulation diving risk of the secondary battery caused by overlarge expansibility is improved, and the long service life is realized. In addition, the total use amount of the negative electrode material is reduced, and more space is saved to further improve the energy density under the condition of ensuring that the endurance mileage in the life cycle is not influenced.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode assembly, secondary battery and electrical device Technical Field

[0001] The present application relates to the field of battery technology, and in particular to electrode assemblies, secondary batteries, and electrical devices. Background Art

[0002] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.

[0003] Lithium-ion batteries are increasingly common in new energy vehicles, and the end-market's pursuit of high energy density, ultra-long life, and low cost is a constant trend. However, balancing high energy density with ultra-long life and low cost presents an industry challenge. To increase the energy density of secondary batteries, the coating weight of the negative electrode sheet is reduced, meaning the designed NP value is lowered. This results in insufficient NPs during charging, leading to lithium deposition and a decrease in battery life. Alternatively, to increase battery life and avoid the risk of lithium deposition, the designed NPs are increased, which in turn reduces energy density.

[0004] Summary of the Invention

[0005] Based on this, it is necessary to provide an electrode assembly, a secondary battery and an electrical device that effectively take into account both high energy density and long life.

[0006] In the first aspect, the present application provides an electrode assembly, comprising: a positive electrode sheet and a negative electrode sheet; the conditions between NP and S corresponding to the current capacity retention rate of the electrode assembly being not less than m are: 1.17-0.35S≤NP≤-0.41S+1.36, 50%≤S≤80%, and m≥99%; wherein NP is the ratio of the unit area capacity of the negative electrode sheet to the unit area capacity of the positive electrode sheet; S is the storage ratio of the electrode assembly, and the storage days that the electrode assembly can achieve when its capacity retention rate is 80% under extreme storage is recorded as N1, the number of cycles that the electrode assembly can achieve when its capacity retention rate is 80% under extreme cycle charge and discharge is recorded as N2, S = 5N1 / (5N1+N2); extreme storage refers to the storage of the electrode assembly at 100% SoC state at an ambient temperature of 60°C; extreme cycling refers to the electrode assembly being charged at a rate of 0.5C and discharged at a rate of 1C at 25°C, and continuously cycling within the range of 0% to 100% SoC; the current capacity retention rate of the electrode assembly refers to the ratio of the current capacity T1 of the electrode assembly to the initial capacity T2 of the electrode assembly.

[0007] The above-mentioned electrode assembly takes into account that the corresponding NP value of the electrode assembly will change as the number of cycles or storage days increases. For this reason, this application considers the design of the NP value corresponding to the current capacity retention rate not lower than m. When designing the NP value, the value can be taken according to the different storage ratios of the electrode assembly, for example: 1.17-0.35S is used as the lower limit of the NP value, and -0.41S+1.36 is used as the upper limit of the NP value. For a storage ratio between 0.5 and 0.8, the upper and lower limits of NP decrease as the storage ratio increases, so that the NP value can be reduced in design, which is conducive to reducing the total amount of negative electrode materials used, maximizing the reuse of the silicon-doped negative electrode's unattenuated lithium insertion and extraction capabilities, and achieving low cost; at the same time, the total amount of negative electrode materials used is reduced, reducing the expansion force of the secondary battery during the cycle, improving the risk of secondary battery cycle diving caused by excessive expansion force, and achieving long life. In addition, the total amount of negative electrode materials used is reduced, and while ensuring that the cruising range within the life cycle is not affected, more space is saved to further improve the energy density.

[0008] In some embodiments, the NP of the electrode assembly during the first charge or first discharge is denoted as Y 0,S , Y 0,S The conditions satisfied between S are: Here, Y0 refers to the NP value set for the reference electrode assembly during its first charge or discharge, with 1.03 ≤ Y0 ≤ 1.2, and a refers to the capacity loss per charge and discharge cycle of the reference electrode assembly. Determining the NP value for an electrode assembly with S > 0% during its first charge or discharge using this formula helps reduce the total amount of negative electrode used, lowering design margins, and mitigating the risk of battery capacity loss during secondary cycles due to excessive expansion force, ultimately achieving an exceptionally long lifespan.

[0009] In some embodiments, Y 0,S The conditions satisfied between S are: In this way, the upper limit of NP during the first charge or first discharge is further limited, and while the service life of the secondary battery 100 is improved, excessive NP design is avoided to affect the energy density of the secondary battery 100, thereby achieving a balance between high energy density and long life.

[0010] In some embodiments, Y0 also satisfies the condition: 1.05≤Y0≤1.15. Thus, further optimizing the value of Y0 makes the NP value of the designed electrode assembly more reasonable, which is conducive to further balancing high energy density and long life.

[0011] In some embodiments, a satisfies the condition: 0.00016≤a≤0.00026. Thus, by reasonably limiting the value of a, the NP value of the designed electrode assembly is also ensured to be reasonable, effectively achieving both high energy density and long life.

[0012] In some embodiments, a further satisfies the condition: 0.00018≤a≤0.00024. Thus, further optimizing the value of a makes the NP value of the designed electrode assembly more reasonable, which is conducive to further balancing high energy density and long life.

[0013] In some embodiments, when the storage ratio S is between 50% and 80%, the NP value of the electrode assembly is between 0.89 and 1.16. This design provides a range of values ​​between NP and S, facilitating the design of NP values ​​for different silicon contents. This not only ensures a high energy density and long life for the secondary battery, but also facilitates the selection of NP values.

[0014] In some embodiments, when the storage ratio S is 70% to 80%, the NP value of the electrode assembly is 0.95 to 1.07. In this way, the range of values ​​between the storage ratio and NP is further limited, making the value of NP more accurate.

[0015] In some embodiments, the capacity per unit area of ​​the negative electrode is recorded as P1, and the capacity per unit area of ​​the positive electrode is recorded as P2. The conditions satisfied by P1 and P2 are: 2.3 mAh / cm 2 ≤P1≤8.6mAh / cm 2 ; 1.5mAh / cm 2 ≤P2≤6.8mAh / cm 2 .

[0016] In some embodiments, the coating weight per unit area of ​​the negative electrode sheet is in the range of 3.9 mg / cm 2 ~13mg / cm 2 In this way, the coating weight range per unit area of ​​the negative electrode sheet is limited, which facilitates the guidance of the preparation of the negative electrode sheet.

[0017] In some embodiments, the coating weight per unit area of ​​the negative electrode sheet is in the range of 3.9 mg / cm 2 ~10mg / cm 2 .

[0018] In some embodiments, the coating weight per unit area of ​​the positive electrode sheet is in the range of 6.5 mg / cm 2 ~29mg / cm 2 In this way, the coating weight range per unit area of ​​the positive electrode sheet is limited, which facilitates the guidance of the preparation of the positive electrode sheet.

[0019] In some embodiments, the coating weight per unit area of ​​the positive electrode sheet is in the range of 9 mg / cm 2 ~21mg / cm 2 .

[0020] In some embodiments, the negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes at least one of a silicon material and a carbon material. Thus, silicon has a higher specific capacity than graphite. Therefore, incorporating a silicon-containing active material onto the negative electrode sheet is conducive to improving the energy density of the secondary battery.

[0021] In some embodiments, the silicon material includes at least one of Si and SiOz (0 < z < 2). Thus, the composition of the silicon-containing material is reasonably designed to obtain a silicon-containing electrode assembly that meets the requirements.

[0022] In some embodiments, the carbon material includes at least one of natural graphite, artificial graphite, mesocarbon microbeads, hard carbon, and soft carbon.

[0023] In some embodiments, the carbon material includes natural graphite and artificial graphite.

[0024] In some embodiments, the weight percentage of the silicon material in the negative electrode active material is 3% to 50%. Thus, the silicon content on the negative electrode sheet is reasonably controlled, and on the premise of ensuring a high energy density, the first efficiency of the negative electrode of the electrode assembly is effectively taken into account.

[0025] In some embodiments, the weight percentage of the silicon material in the negative electrode active material is 3% to 25%. Thus, the silicon content is further reasonably controlled to effectively take into account the high energy density and long life of the electrode assembly.

[0026] In some embodiments, the positive electrode sheet includes a positive electrode active material, and the positive electrode active material is an active substance capable of intercalating and deintercalating lithium ions.

[0027] In some embodiments, the positive electrode active material includes one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide; and compounds obtained from transition metals or non-transition metals.

[0028] In some embodiments, the positive electrode active material includes a lithium-containing transition metal composite oxide, wherein the transition metal includes at least one selected from nickel, cobalt, manganese, and aluminum. Thus, the composition of the positive electrode material layer is reasonably designed to obtain a silicon-containing electrode assembly that meets the requirements.

[0029] In a second aspect, the present application provides a secondary battery, including: a housing; an electrode assembly as described in any one of the above, housed in the housing; and an electrolyte, filled in the housing.

[0030] The above-mentioned secondary battery uses the above-mentioned electrode assembly, which is conducive to reducing the total amount of negative electrode materials used, maximizing the reuse of the silicon-doped negative electrode's undiminished lithium insertion and extraction capabilities, and achieving low cost; at the same time, the total amount of negative electrode materials used is reduced, reducing the expansion force of the secondary battery during circulation, improving the risk of secondary battery cycle diving due to excessive expansion force, and achieving long life.

[0031] In a third aspect, the present application provides an electrical device comprising the above secondary battery.

[0032] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0034] FIG1 is a schematic diagram of the exploded structure of a secondary battery provided in some embodiments of the present application;

[0035] FIG2 is a flowchart of a NP design method according to some embodiments of the present application;

[0036] FIG3 is a second flow chart of the NP design method provided in some embodiments of the present application.

[0037] 100. Secondary battery; 10. End cap; 20. Electrode assembly; 30. Electrode terminal; 40. Housing. DETAILED DESCRIPTION

[0038] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0040] In the description of the embodiments of this application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood to indicate or imply relative importance or implicitly specify the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.

[0041] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0042] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.

[0043] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0044] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.

[0045] In the description of the embodiments of the present application, unless otherwise expressly specified or limited, technical terms such as "installed," "connected," "connected," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; internal connections between two components or interactions between two components. Those skilled in the art can understand the specific meanings of the above terms in the embodiments of the present application based on specific circumstances.

[0046] Currently, market developments indicate that secondary batteries are becoming increasingly widely used. They are not only used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric vehicles, as well as in military equipment and aerospace. As the application of secondary batteries continues to expand, market demand is also growing.

[0047] The use of secondary batteries in new energy vehicles is becoming increasingly common, and the end market's pursuit of high energy density, ultra-long life, and low cost is an unwavering trend. However, how to strike a balance between high energy density, ultra-long life, and low cost remains a challenge for the industry.

[0048] The applicant has noticed that the intrinsic limit cycle and limit storage life of the secondary battery have an important influence on the NP value of the battery. This application uses the intrinsic limit cycle and limit storage life as basic parameters and associates the NP value of the battery through the storage ratio.

[0049] Based on this, and to address the problem of secondary batteries blindly increasing NP to increase cycle life, which deteriorates energy density and fails to effectively balance high energy density and long life, the applicant has designed an electrode assembly after in-depth research. The NP design of the electrode assembly is linked to the storage ratio. The conditions between the NP and the storage ratio S corresponding to the electrode assembly with a current capacity retention rate of not less than m are as follows: 1.17-0.35S≤NP≤-0.41S+1.36, 50%≤S≤80%, and m≥99%.

[0050] The above-mentioned electrode assembly takes into account that the corresponding NP value of the electrode assembly will change as the number of cycles increases. For this reason, the present application considers the design of the NP value corresponding to the current capacity retention rate not lower than m. When designing the NP value, the value can be taken according to the different storage ratios of the electrode assembly, for example: 1.17-0.35S is used as the lower limit of the NP value, and -0.41S+1.36 is used as the upper limit of the NP value. For a storage ratio between 0.5 and 0.8, the upper and lower limits of NP decrease as the storage ratio increases, so that the NP value can be reduced in design, which is conducive to reducing the total amount of negative electrode materials, maximizing the reuse of the silicon-doped negative electrode's unattenuated lithium insertion and extraction capabilities, and achieving low cost; at the same time, the total amount of negative electrode materials is reduced, reducing the expansion force of the secondary battery in the cycle, improving the risk of secondary battery cycle diving due to excessive expansion force, and achieving long life.

[0051] In addition, the total amount of negative electrode materials used is reduced, which saves more space to further improve the energy density while ensuring that the cruising range during the life cycle is not affected.

[0052] It should be noted that NP refers to the ratio of the unit area capacity of the negative electrode sheet to the unit area capacity of the positive electrode sheet. The specific calculation formula is: Where CW represents the weight per unit area of ​​the coating material, in grams per square centimeter (g / cm 2 ), Cap represents the gram capacity of the active material, the unit is milliampere-hour per gram (mA·h / g), Loading represents the proportion of the active material, and the respective subscripts A represent the negative electrode and C represent the positive electrode.

[0053] Therefore, if the NP value of the electrode assembly is determined, the weight per unit area of ​​the coating material on the positive and negative electrodes can be inferred using the above formula. Of course, when confirming the copyright at a later stage, the above formula can be used for reverse deduction to obtain the NP value of the infringing product. For example, the competitor's electrode assembly can be disassembled in reverse, and the positive and negative electrodes of the same area are assembled with lithium sheets in reverse order. The capacity of the positive and negative electrodes is recorded, and the ratio of the negative electrode capacity to the positive electrode capacity is the reversed NP value.

[0054] The storage ratio refers to the ratio of the number of days an electrode assembly is stored during extreme storage to the number of cycles it achieves during extreme cycle charge and discharge. Different electrode assemblies have different storage ratios. The lifespan (days) of the electrode assembly 20 during extreme storage is N1, and the lifespan of the electrode assembly 20 during extreme cycle charge and discharge is N2. 5N1 / (5N1+N2) is defined as the storage ratio of the electrode assembly 20 and is recorded as S. Extreme storage refers to the storage of a battery at 100% SoC at an ambient temperature of 60°C. Extreme cycling refers to the continuous cycling of a battery at 25°C, with a charge rate of 0.5C and a discharge rate of 1C, within a range of 0% to 100% SoC. Lifespan refers to the number of days or cycles a battery is stored when the capacity retention rate of the electrode assembly 20 is 80%. The capacity retention rate of the electrode assembly 20 refers to the ratio of the current capacity of the battery at 0.5C / 1C full charge and discharge at 25°C to the initial capacity.

[0055] The current capacity test method of the electrode assembly 20 can be as follows: the secondary battery 100 having the electrode assembly 20 is charged to the full charge voltage at 0.5C under specific conditions (e.g., at 25°C); then, at the full charge voltage, it is charged at a constant voltage to a current ≤ 0.05C, left to rest for 30 minutes, and then discharged to the full discharge voltage at 1C; the capacity value at the end of discharge is recorded, which is the current capacity of the electrode assembly 20. As for obtaining the initial capacity of the electrode assembly 20, there are various ways to obtain it, such as: remaking the secondary battery 100 with the electrode assembly 20 without electrolyte, repeating the above charge and discharge steps with the new secondary battery 100, and using the recorded discharge capacity value as the initial capacity; or, directly using the initial capacity or rated capacity recorded in the factory information of the secondary battery 100 as the initial capacity of the electrode assembly 20, etc. Of course, the initial capacity can also be obtained by other testing methods, as long as it can truly reflect the initial capacity of the electrode assembly 100.

[0056] The secondary battery disclosed in the embodiments of the present application can be used, but is not limited to, in electrical devices such as vehicles, ships, or aircraft. A power supply system comprising the secondary battery disclosed in the present application can be used to form the electrical device.

[0057] In the power supply system, there can be multiple secondary batteries, and the multiple secondary batteries can be connected in series, in parallel, or in a mixed connection. Mixed connection means that the multiple secondary batteries are both connected in series and in parallel. Multiple secondary batteries can be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple secondary batteries is accommodated in a box; of course, the battery can also be a battery module formed by connecting multiple secondary batteries in series, in parallel, or in a mixed connection, and then the multiple battery modules are connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in a box. The battery can also include other structures. For example, the battery can also include a busbar component for realizing electrical connection between multiple secondary batteries. Among them, the secondary battery can be cylindrical, flat, rectangular, or other shapes.

[0058] Please refer to Figure 1, which is a schematic diagram of the exploded structure of a secondary battery 100 provided in some embodiments of the present application. Secondary battery 100 is the smallest unit of a battery. As shown in Figure 1, secondary battery 100 includes an end cap 10, a housing 40, an electrode assembly 20, and other functional components.

[0059] The end cap 10 is a component that covers the opening of the housing 40 to isolate the internal environment of the secondary battery 100 from the external environment. Without limitation, the shape of the end cap 10 can be adapted to the shape of the housing 40 to match the housing 40. Optionally, the end cap 10 can be made of a material with a certain hardness and strength (such as an aluminum alloy). In this way, the end cap 10 is less likely to deform when squeezed or collided, giving the secondary battery 100 a higher structural strength and improved safety performance. Functional components such as electrode terminals 30 can be provided on the end cap 10. The electrode terminals 30 can be used to electrically connect to the electrode assembly 20 for outputting or inputting electrical energy into or out of the secondary battery 100. In some embodiments, the end cap 10 can also be provided with a pressure relief mechanism for relieving internal pressure when the internal pressure or temperature of the secondary battery 100 reaches a threshold. The end cap 10 can also be made of a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application do not impose any special restrictions on this. In some embodiments, an insulating member may be provided inside the end cap 10 to isolate the electrical connection components in the housing 40 from the end cap 10 to reduce the risk of short circuit.

[0060] The housing 40 is a component that cooperates with the end cap 10 to form the internal environment of the secondary battery 100. This internal environment can be used to accommodate the electrode assembly 20, electrolyte, and other components. The housing 40 and the end cap 10 can be separate components. An opening can be provided in the housing 40, and the end cap 10 is placed over the opening to form the internal environment of the secondary battery 100. Alternatively, the end cap 10 and the housing 40 can be integrated. Specifically, the end cap 10 and the housing 40 can form a common connection surface before other components are inserted into the housing. When the interior of the housing 40 needs to be enclosed, the end cap 10 is placed over the housing 40. The housing 40 can have a variety of shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the housing 40 can be determined based on the specific shape and size of the electrode assembly 20. The housing 40 can be made of a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and this embodiment of the present application does not impose any particular limitations on this.

[0061] The electrode assembly 20 is a component in the secondary battery 100 where electrochemical reactions occur. One or more electrode assemblies 20 may be contained in the housing 40. The electrode assembly 20 is mainly formed by winding or stacking a positive electrode sheet and a negative electrode sheet, and a separator is usually provided between the positive electrode sheet and the negative electrode sheet. The parts of the positive electrode sheet and the negative electrode sheet with active materials constitute the main body of the electrode assembly 20, and the parts of the positive electrode sheet and the negative electrode sheet without active materials each constitute a tab. The positive electrode tab and the negative electrode tab may be located together at one end of the main body or respectively at both ends of the main body. During the charge and discharge process of the battery, the positive electrode active material and the negative electrode active material react with the electrolyte, and the tabs are connected to the electrode terminals 30 to form a current loop.

[0062] According to some embodiments of the present application, an electrode assembly 20 is provided, and the electrode assembly 20 includes: a positive electrode sheet and a negative electrode sheet. Among them, when the current capacity retention rate of the electrode assembly 20 is not less than m, the conditions satisfied between NP and S corresponding to the following are: 1.17-0.35S≤NP≤-0.41S+1.36, 50%≤S≤80%, and m≥99%; wherein NP is the ratio of the unit area capacity of the negative electrode sheet to the unit area capacity of the positive electrode sheet; S is the storage ratio of the electrode assembly 20, and the number of storage days that the electrode assembly 20 can achieve when its capacity retention rate is 80% under extreme storage is recorded as N1, and the electrode assembly 20 is stored in the extreme cycle. The number of cycles that can be achieved when the capacity retention rate is 80% during charge and discharge is recorded as N2, S = 5N1 / (5N1+N2); limit storage refers to the storage of the electrode assembly in a 100% SoC state at an ambient temperature of 60°C; limit cycling refers to the electrode assembly being charged at a rate of 0.5C and discharged at a rate of 1C at 25°C, and continuously cycling within the range of 0% to 100% SoC; the current capacity retention rate of the electrode assembly 20 refers to the ratio of the current capacity T1 of the electrode assembly 20 to the initial capacity T2 of the electrode assembly 20.

[0063] The electrode assembly 20 also includes a separator, which is positioned between the positive and negative electrodes. This separator is a porous plastic film that allows lithium ions to pass freely through the electrode circuit while preventing contact between the two electrodes, providing electronic insulation. It can be made of, but is not limited to, a single-layer polyethylene film or a single-layer polypropylene film.

[0064] The NP corresponding to the current capacity retention rate of the electrode assembly 20 when it is not less than m should be understood as follows: as the number of cycles of charge and discharge or the number of storage days increases, the active lithium will be consumed by side reactions, and the local crystal structure of the positive electrode material will change, resulting in capacity loss, while the electrochemical activity of silicon or graphite in the negative electrode material layer remains basically unchanged. Therefore, in the later stage of the cycle charge and discharge, the negative electrode has an excess lithium storage capacity and the NP is on an increasing trend. For this reason, the present application controls the current capacity retention rate of the electrode assembly 20 to be not less than m for consideration, for example: the current capacity retention rate of the electrode assembly 20 is not less than 99%, or the electrode assembly 20 is in the first charge or first discharge state (which can also be understood as a new electrode assembly 20 after leaving the factory); or the electrode assembly 20 is in an unformed state, etc.

[0065] Based on the storage ratio S of the electrode assembly 20, NP is controlled to be between 1.17-0.35S and -0.41S+1.36. For example, when S is 70%, NP can be 0.925-1.07; when S is 50%, NP can be 0.997-1.16, etc. Specifically, in some embodiments, when S is 70%, NP can be 1.02-1.06; when S is 50%, NP can be 1.00-1.06, etc.

[0066] This design reduces the NP value, which helps reduce the total amount of negative electrode material used. This maximizes the reuse of the silicon-doped negative electrode's undiminished lithium insertion and removal capacity, achieving low costs. Furthermore, this reduction in negative electrode material usage reduces the expansion force of the secondary battery 100 during cycling, mitigating the risk of excessive expansion force causing the secondary battery 100 to rupture during cycling, thereby extending its lifespan. Furthermore, this reduction in negative electrode material usage frees up space and further improves energy density while ensuring uncompromised range over the battery's lifetime.

[0067] According to some embodiments of the present application, the NP of the electrode assembly 20 during the first charge or first discharge is recorded as Y 0,S , Y 0,S The conditions satisfied between S are: Wherein, Y0 refers to the NP value set for the reference electrode assembly during the first charge or first discharge, and 1.03≤Y0≤1.2, and a refers to the capacity loss value caused by each cycle of charge and discharge of the reference electrode assembly.

[0068] Extreme storage refers to storing the electrode assembly 20 at 100% SoC at an ambient temperature of 60°C. Extreme cycling refers to continuously cycling the electrode assembly 20 at 25°C, charging at a rate of 0.5C and discharging at a rate of 1C, within a range of 0% to 100% SoC. Alternatively, the electrode assembly 20 can be considered to be continuously cycling between charge and discharge.

[0069] The reference electrode assembly refers to an electrode assembly used as a reference for obtaining the NP value range of the electrode assembly 20 of the present application or target (e.g., an electrode assembly for which an NP value design is required, an electrode assembly to be tested, etc.). The NP of the electrode assembly can be pre-set to a value between 1.03 and 1.2. For example, the reference electrode assembly can be an electrode assembly of conventional technology.

[0070] The initial charge of the electrode assembly 20 can be understood as the formation of the secondary battery 100. Its purpose is to make the secondary battery 100 electrochemically active and form a solid electrolyte interface film (SEI film) on the negative electrode surface. The initial discharge of the electrode assembly 20 refers to the process of discharging the electrode assembly 20 for the first time after formation.

[0071] To facilitate the understanding of the above inequality, the inequality can be simplified to Because Y 0,S The relationship between the values ​​of and n is negatively correlated (that is, n can be eliminated from the numerator and the formula can be transformed into: Therefore, the value of n can be 50 to 200. And since nas in the formula is always greater than 0, The value in should always be less than 1, so by The calculated NP of the electrode assembly 20 at the first charge or first discharge should be smaller than the Y0 of the reference electrode assembly at the first charge or first discharge. That is, when designing the NP of the electrode assembly 20, the design NP value can be lowered according to the storage ratio, which is beneficial to reducing the total amount of negative electrode used, reducing the design group margin, and improving the risk of the secondary battery diving after 100 cycles due to excessive expansion force, thereby achieving ultra-long life. At the same time, while ensuring that the cruising range is not affected during the life cycle, more space can be saved to further improve the energy density.

[0072] Determining the NP of the electrode assembly 20 during the first charge or first discharge using the above formula is beneficial to reducing the total amount of negative electrode used, reducing the design group margin, improving the risk of the secondary battery diving after 100 cycles due to excessive expansion force, and achieving ultra-long life; at the same time, while ensuring that the cruising range within the life cycle is not affected, more space is saved to further improve the energy density.

[0073] According to some embodiments of the present application, Y 0,S The conditions satisfied between S are:

[0074] Similarly, for ease of understanding, the above inequality can be simplified as follows: And n can be 100 to 200. So we can see that 0,S The upper limit of the inequality is limited, so that when the NP is initially designed, the service life of the secondary battery 100 is improved while avoiding excessively enlarging the NP design and affecting the energy density of the secondary battery 100.

[0075] The upper limit of NP during the first charge or first discharge is further limited. Under the premise of improving the service life of the secondary battery 100, the excessive enlargement of NP design is avoided to affect the energy density of the secondary battery 100, thereby achieving a balance between high energy density and long life.

[0076] According to some embodiments of the present application, Y0 further satisfies the condition: 1.05≤Y0≤1.15.

[0077] Similarly, when designing the NP of the electrode assembly 20 with a storage ratio of S during the first charge or first discharge, the value of Y0 can be controlled between 1.05 and 1.15. For example, Y0 is 1.05 or 1.15, and the above Y 0,S Calculate in the calculation formula.

[0078] Further optimizing the value of Y0 makes the NP value of the designed electrode assembly 20 more reasonable, which is conducive to further taking into account high energy density and long life.

[0079] According to some embodiments of the present application, a satisfies the condition: 0.00016≤a≤0.00026.

[0080] a represents the capacity loss per cycle of the reference electrode assembly. The value of a can be between 0.00016 and 0.00026.

[0081] Reasonable limitation of the value of a also ensures that the NP value of the designed electrode assembly 20 is reasonable, effectively taking into account both high energy density and long life.

[0082] According to some embodiments of the present application, a further satisfies the condition: 0.00018≤a≤0.00024.

[0083] The value of a can be a value between 0.00018 and 0.00024. For example, a can be, but is not limited to, 0.00018 or 0.00024.

[0084] Further optimizing the value of a makes the NP value of the designed electrode assembly 20 more reasonable, which is conducive to further balancing high energy density and long life.

[0085] According to some embodiments of the present application, when the storage ratio S is 50% to 80%, the NP value of the electrode assembly 20 is: 0.89 to 1.16.

[0086] While satisfying the aforementioned inequality between NP and S, the range of values ​​between NP and S can be further narrowed. If the storage ratio S is 50% to 80%, the NP corresponding to the electrode assembly 20 having a current capacity retention rate not less than m should be a value between 0.89 and 1.16 (including the endpoint values), for example, NP can be, but is not limited to, 0.89, 1.0, 1.1, 1.15, or 1.16.

[0087] Such a design provides a range value relationship between NP and S, which can facilitate the design of NP values ​​with different silicon contents, not only taking into account the high energy density and long life of the secondary battery; but also facilitates the selection of NP values.

[0088] According to some embodiments of the present application, when the storage ratio S is 70% to 80%, the NP value of the electrode assembly is: 0.95 to 1.07.

[0089] When the storage ratio S is 70% to 80%, the value of NP can be, but is not limited to, 0.95, 1.0, 1.01, 1.03, 1.06, 1.07, etc.

[0090] The value range between storage ratio and NP is further limited to make the NP value more accurate.

[0091] According to some embodiments of the present application, the negative electrode sheet includes a negative electrode material layer, and the negative electrode material layer includes a silicon-containing active material.

[0092] According to some embodiments of the present application, the unit area capacity of the negative electrode sheet is recorded as P1, and the unit area capacity of the positive electrode sheet is recorded as P2. The conditions satisfied by P1 and P2 are: 2.3 milliampere hours per square centimeter (mAh / cm 2 )≤P1≤8.6mAh / cm 2 ; 1.5mAh / cm 2 ≤P2≤6.8mAh / cm 2 .

[0093] When designing NP, the NP value is determined for different silicon contents according to the above inequality 1.17-0.35S≤NP≤-0.41S+1.36; after determining the NP value, since the NP value is also related to the unit area capacity value on the positive and negative electrodes, when actually manufacturing the positive and negative electrodes, the respective value ranges of NP, P1 and P2 can be comprehensively considered for design.

[0094] Among them, the value of P1 can be 2.3mAh / cm 2 ~8.6mAh / cm 2 For example, P1 can be but not limited to 2.3 mAh / cm 2 、3mAh / cm 2 , 5mAh / cm 2 、8.6mAh / cm 2 Etc. Similarly, the value of P2 can be 1.5 mAh / cm 2 ~6.8mAh / cm 2 For example, P2 can be but not limited to 1.5 mAh / cm 2 、3mAh / cm 2 , 5mAh / cm 2 、6.8mAh / cm 2 wait.

[0095] Under the premise of satisfying the above-mentioned inequality relationship between NP and S, the unit area capacity of the positive and negative electrode sheets is limited to facilitate the actual design of the positive and negative electrode sheets.

[0096] According to some embodiments of the present application, the coating weight per unit area of ​​the negative electrode sheet is in the range of 3.9 mg / cm 2 ~13mg / cm 2 .

[0097] On the negative electrode sheet, the capacity per unit area is the product of the gram capacity of the active material and the coating weight of the active material per unit area. The gram capacity is mainly related to the composition of the active material; the coating weight per unit area can be, but is not limited to, 3.9 mg / cm2 , 4mg / cm 2 、10mg / cm 2 、13mg / cm 2 wait.

[0098] In this way, the coating weight range per unit area of ​​the negative electrode sheet is limited, which facilitates the guidance of the preparation of the negative electrode sheet.

[0099] According to some embodiments of the present application, the coating weight per unit area of ​​the negative electrode sheet is in the range of 3.9 mg / cm 2 ~10mg / cm 2 .

[0100] The coating weight per unit area may further be, but is not limited to, 3.9 mg / cm 2 , 4mg / cm 2 、10mg / cm 2 wait.

[0101] According to some embodiments of the present application, the coating weight per unit area of ​​the positive electrode sheet is in the range of 6.5 mg / cm 2 ~29mg / cm 2 .

[0102] On the positive electrode sheet, the capacity per unit area is the product of the gram capacity of the active material and the coating weight of the active material per unit area. The gram capacity is mainly related to the composition of the active material; the coating weight per unit area can be, but is not limited to, 6.5 mg / cm 2 , 8mg / cm 2 、10mg / cm 2 , 29mg / cm 2 wait.

[0103] In this way, the coating weight range per unit area of ​​the positive electrode sheet is limited, which facilitates the guidance of the preparation of the positive electrode sheet.

[0104] According to some embodiments of the present application, the coating weight per unit area of ​​the positive electrode sheet is in the range of 9 mg / cm 2 ~21mg / cm 2 .

[0105] The coating weight per unit area on the positive electrode sheet can be further but not limited to 9 mg / cm 2 , 12mg / cm 2 、18mg / cm 2 , 21mg / cm 2 wait.

[0106] According to some embodiments of the present application, the negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes at least one of a silicon material and a carbon material.

[0107] The materials coated on the negative electrode sheet include negative electrode active materials, conductive agents, binders, etc. in a certain mixing ratio. Among them, the negative electrode active materials include silicon materials and carbon materials. For example, when preparing the negative electrode active materials, silicon-containing active materials can be blended into graphite in a certain proportion.

[0108] Among them, the conductive agent refers to a substance that increases the conductive contact between active materials and improves the electronic conductivity, such as conductive graphite, conductive carbon black, conductive carbon fiber, and graphene. The binder refers to a polymer compound that adheres the active material to the current collector, such as one of the group formed by polyvinylidene fluoride, polyacrylic acid, polymethacrylic acid, poly(methyl acrylate), poly(ethyl acrylate), pure acrylic emulsion, poly(acrylic acid-styrene) copolymer, polyvinylpyrrolidone, styrene-butadiene rubber, epoxy resin, neopentyl glycol diacrylate, polyacrylate series, polytetrafluoroethylene, polyimide, polyamides, polyesters, cellulose derivatives, polysulfones or one of the group formed by two or more of them.

[0109] Silicon has a higher specific capacity than graphite. Therefore, incorporating silicon-containing active materials into the negative electrode sheet is beneficial to improving the energy density of the secondary battery 100.

[0110] According to some embodiments of the present application, the silicon material includes at least one of Si and SiO₂ (0 < z < 2).

[0111] In the preparation process, compounds represented by Si and / or SiO₂ are blended into graphite in a certain proportion to prepare the negative electrode material layer of the negative electrode sheet.

[0112] Reasonably design the composition of the silicon-containing material to obtain a silicon-containing electrode assembly 20 that meets the requirements.

[0113] According to some embodiments of the present application, the carbon material includes at least one of natural graphite, artificial graphite, mesocarbon microbeads (abbreviated as MCMB), hard carbon, and soft carbon.

[0114] Specifically in some embodiments, the carbon material includes natural graphite and artificial graphite.

[0115] According to some embodiments of the present application, the weight percentage of the silicon material in the negative electrode active material is 3% - 50%.

[0116] Although silicon has a higher specific capacity than carbon, the first efficiency of the silicon negative electrode is relatively low. Therefore, in the design of the negative electrode active material, the silicon content can be controlled between 3% and 50%. For example, when designing the electrode assembly 20, the silicon material with the above content can be incorporated into the carbon material to obtain the required negative electrode sheet.

[0117] Reasonably control the silicon content on the negative electrode sheet, and effectively take into account the negative electrode primary effect of the electrode assembly while ensuring high energy density.

[0118] According to some embodiments of the present application, the weight percentage of the silicon material content in the negative electrode active material is 3% to 25%.

[0119] In the negative electrode active material, the silicon content may be, but is not limited to, 3%, 5%, 10%, 15%, 20%, 25%, etc.

[0120] The silicon content is further reasonably controlled to effectively balance the high energy density and long life of the electrode assembly 20.

[0121] According to some embodiments of the present application, the positive electrode sheet includes a positive electrode active material, which is an active substance capable of intercalating and deintercalating lithium ions.

[0122] There are many options for positive electrode active materials, such as lithium-containing transition metal oxides, phosphides such as LiCoO2, LiFePO4, etc.

[0123] According to some embodiments of the present application, the positive electrode active material includes one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide; and compounds obtained from transition metals or non-transition metals.

[0124] There are many types of positive electrode active materials for this application, such as layered lithium-containing oxides, spinel-type lithium-containing oxides, or olivine-type lithium-containing phosphate compounds. Of course, the positive electrode active materials of the embodiments of this application are not limited to the above materials, and other conventionally known materials that can be used as positive electrode active materials for lithium-ion batteries can also be used. In addition, the above positive electrode active materials can be used alone or in combination of two or more.

[0125] According to some embodiments of the present application, the positive electrode active material includes a lithium-containing transition metal composite oxide, wherein the transition metal includes at least one selected from nickel, cobalt, manganese, and aluminum.

[0126] The positive electrode material layer refers to the structure of the active material coated on the current collector, which includes a certain mixed ratio of active materials, conductive agents, binders, etc. Among them, the active material refers to a substance containing lithium or lithium iron phosphate, for example: the active material can be Li q (Ni c Co d Mn e ) The general formula of O2 structure is expressed, where 0.9≤q≤1.2, 0.2<c<1, 0<d<1, q+c+d=1.

[0127] The transition metal may be selected from one of nickel, cobalt, manganese and aluminum, or at least one of the group consisting of nickel, cobalt, manganese and aluminum. For example, the transition metal may be a combination of nickel, cobalt and manganese.

[0128] The composition of the positive electrode material layer is rationally designed to obtain a silicon-containing electrode assembly 20 that meets the requirements.

[0129] According to some embodiments of the present application, a secondary battery 100 is provided. The secondary battery 100 includes a housing 40, an electrode assembly 20 as described in any of the above solutions, and an electrolyte. The electrode assembly 20 is housed in the housing 40. The housing 40 is filled with an electrolyte.

[0130] The electrolyte refers to a carrier for lithium ion transmission in the secondary battery 100, such as ethylene carbonate, propylene carbonate, diethyl carbonate, etc.

[0131] The above-mentioned secondary battery 100 adopts the above-mentioned electrode assembly 20, which is conducive to reducing the total amount of negative electrode materials used, maximizing the reuse of the undiminished lithium insertion and extraction ability of the silicon-doped negative electrode, and achieving low cost; at the same time, the total amount of negative electrode materials used is reduced, reducing the expansion force of the secondary battery 100 during the cycle, improving the risk of the secondary battery 100 diving during the cycle due to excessive expansion force, and achieving long life.

[0132] According to some embodiments of the present application, referring to FIG. 2 , the present application provides a secondary battery NP design method, where NP refers to the ratio of the unit area capacity of the negative electrode sheet to the unit area capacity of the positive electrode sheet, comprising the following steps:

[0133] S100, determining the storage ratio of the target secondary battery, denoted as S, and determining the NP value of the reference secondary battery at the time of first charge or first discharge, denoted as Y0, wherein the number of storage days that the electrode assembly can achieve when its capacity retention rate is 80% under extreme storage is denoted as N1, and the number of cycles that the electrode assembly can achieve when its capacity retention rate is 80% under extreme cycle charge and discharge is denoted as N2, 5N1 / (5N1+N2) is defined as the storage ratio of the electrode assembly, the reference secondary battery refers to an existing secondary battery, and can also be understood as a set or known secondary battery, and 1.03≤Y0≤1.2;

[0134] S200: Determine the NP value of the target secondary battery when it is first charged or discharged according to the following formula, and record it as Y 0,S ; Wherein, n refers to the NP of the reference secondary battery when it is cycled for n cycles of charge and discharge being equal to the NP of the target secondary battery when it is cycled for n cycles of charge and discharge, and a refers to the capacity loss value caused by each cycle of charge and discharge of the reference secondary battery.

[0135] In step S100 , the target secondary battery refers to the battery for which the NP is to be designed in this application. The storage ratio of the target secondary battery can be determined according to design requirements or user requirements.

[0136] In step S200 , the value of a can be obtained by conducting a cyclic charge-discharge experiment on a reference secondary battery; or it can be obtained based on experience, for example, a can be a value between 0.00016 and 0.00026; or it can be a value between 0.00018 and 0.00024.

[0137] The NP determined through the above design method is conducive to reducing the total amount of negative electrode used, lowering the design group margin, improving the risk of secondary batteries diving after 100 cycles due to excessive expansion force, and achieving ultra-long life; at the same time, while ensuring that the cruising range within the life cycle is not affected, more space is saved to further improve the energy density.

[0138] According to some embodiments of the present application, refer to FIG. 3 , S200, according to the following formula, the NP value of the target secondary battery when it is first charged or first discharged is determined and recorded as Y 0,S The steps include:

[0139] S210, obtaining the change relationship of the NP value during the cycle of the target secondary battery, and fitting the following formula: Where Y n,S It refers to the NP value of the target secondary battery when it is cycled n times;

[0140] S220, obtaining the variation relationship of the NP value during the cycle of the reference secondary battery, and fitting the following formula: Where Y n Refers to the NP value of the reference secondary battery when it is cycled n times;

[0141] S230, according to Y n,S= Y n In principle, the formula is: And determine the NP value of the target secondary battery when it is charged or discharged for the first time.

[0142] The design concept of the NP in this application is based on the failure mechanism of the positive and negative electrode materials, quantifies the dynamic changes of the NP during the cycle, and reversely designs the NP of the secondary battery 100 based on the NP of the nth cycle of the reference secondary battery.

[0143] In step S210, the target secondary battery with different storage ratios may be subjected to multiple cycles of charge and discharge, and the NP value after the cycles is recorded, and a relationship between NP, S and n after different numbers of cycles is fitted.

[0144] In step S220 , the secondary battery may be subjected to multiple cycles of charge and discharge, and the NP values ​​after the cycles may be recorded, and a relationship between NP and n after different numbers of cycles may be fitted.

[0145] Since the failure mode of the target secondary battery is that the active lithium is consumed in the form of side reactions, the capacity loss is caused by the change of the local crystal structure of the positive electrode material, while the electrochemical activity of silicon or graphite in the negative electrode active material remains basically unchanged, and the ability to deintercalate and deintercalate lithium is always maintained. Therefore, the lithium storage capacity of the negative electrode in the later stage of the target secondary battery cycle is often excessive, and NP is increasing. To this end, in step S230, in order to maximize the use of this characteristic of the negative electrode, high energy density and long life are achieved. This application comprehensively considers the changes in NP during the cycle, and designs the NP of the target secondary battery based on the NP value of the nth cycle of the reference secondary battery.

[0146] In this way, using the above design method, the initial NP design can be reduced, the energy density can be improved, and the cost can be reduced; at the same time, the cycle life can be guaranteed.

[0147] According to some embodiments of the present application, referring to FIG. 1 to FIG. 3 , the present application provides a method for designing NPs of a target secondary battery. The dynamic change of NPs during the cycle can be expressed as follows:

[0148]

[0149] In order to maximize the use of this characteristic of the negative electrode and achieve high energy density, long life and low cost, the present invention comprehensively considers the changes in NP during the cycle and designs the NP of the silicon-doped negative electrode based on the NP value of the nth cycle (preferably the 200th cycle) of a conventional secondary battery. The design criteria are:

[0150] Y n,S =Y n (2)

[0151] Substitute formula 2 into formula 1 to obtain:

[0152] In order to make the purpose, technical solutions and advantages of this application more concise and clear, this application is illustrated with the following specific examples, but this application is by no means limited to these examples. The embodiments described below are only preferred embodiments of this application and can be used to describe this application. They should not be understood as limiting the scope of this application. It should be pointed out that any modifications, equivalent replacements and improvements made within the spirit and principles of this application should be included in the scope of protection of this application.

[0153] In order to better illustrate the present application, the present application is further described below in conjunction with the embodiments. The following are specific embodiments.

[0154] Example 1

[0155] positive electrode

[0156] The positive electrode active material ternary material nickel cobalt manganese (NCM811), the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are mixed evenly in a mass ratio of 97:2:1 and added to the solvent NMP to prepare the positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, dried at 85°C and cold pressed, and then die-cut and slit to make the lithium-ion battery positive electrode sheet.

[0157] negative electrode

[0158] The negative electrode active material graphite, commercial silicon oxide, conductive agent acetylene black, thickener sodium carboxymethyl cellulose (CMC), and binder styrene butadiene rubber (SBR) are added to solvent water in a mass ratio of 91.2:4.8:2:1:1, mixed evenly, and formed into a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil, dried at 85°C, and then cold pressed to form a lithium-ion battery negative electrode sheet, wherein the percentage content of the silicon active material is 5%.

[0159] diaphragm

[0160] A polyethylene microporous film is used as a porous diaphragm substrate, and inorganic alumina powder, polyvinylpyrrolidone, and acetone solvent are evenly mixed in a weight ratio of 3:1.5:5.5 to form a slurry, which is then coated on one side of the substrate and dried to obtain a diaphragm.

[0161] electrolyte

[0162] Lithium hexafluorophosphate is dissolved in a mixed solvent of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate (the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:2:1) to obtain a lithium ion battery electrolyte.

[0163] Secondary battery 100

[0164] The positive electrode sheet, negative electrode sheet and separator are wound to obtain an electrode assembly 20, which is then packaged, injected, formed, and vented to obtain a secondary battery 100. The designed charging NP of the secondary battery 100 is 1.08, and the designed capacity of the secondary battery 100 is 100.9 ampere hours (Ah). The storage capacity of the battery accounts for 70%.

[0165] Example 2

[0166] The battery is basically the same as Example 1, except that the coating weight of the positive electrode is kept constant and the coating weight of the negative electrode is reduced. The battery has a designed charge NP of 1.024 and a storage ratio of 50%.

[0167] Example 3

[0168] The battery is basically the same as Example 1, except that the coating weight of the positive electrode is kept constant and the coating weight of the negative electrode is reduced. The battery has a design charge NP = 1.00. The storage ratio of the battery is 80%.

[0169] Example 4

[0170] It is basically the same as Example 1, except that: the coating weight of the positive electrode is kept unchanged, and the coating weight of the negative electrode is reduced. The design charging NP of the battery is 1.05, and the storage ratio of the battery is 55%.

[0171] Example 5

[0172] It is basically the same as Example 1, except that the coating weight of the positive electrode is kept unchanged and the coating weight of the negative electrode is reduced. The design charging NP of the battery is 1.03, and the storage ratio of the battery is 60%.

[0173] Blank comparison

[0174] The method is basically the same as Example 1, except that the battery is designed to have a charging NP of 1.10.

[0175] Comparative Example 1

[0176] The method is basically the same as Example 1, except that the battery is designed to have a charging NP of 1.21.

[0177] Comparative Example 2

[0178] The method is basically the same as Example 2, except that the battery is designed to have a charging NP of 1.21.

[0179] Comparative Example 3

[0180] The method is basically the same as Example 3, except that the battery is designed to have a charging NP of 1.10.

[0181] Comparative Example 4

[0182] The method is basically the same as Example 3, except that the coating weight of the positive electrode is kept unchanged and the coating weight of the negative electrode is increased. The design charging NP of the battery is 1.20.

[0183] Comparative Example 5

[0184] The method is basically the same as Example 4, except that the coating weight of the positive electrode is kept unchanged and the coating weight of the negative electrode is increased. The design charge NP of the battery is 1.20.

[0185] Comparative Example 6

[0186] The method is basically the same as Example 5, except that the coating weight of the positive electrode is kept unchanged and the coating weight of the negative electrode is increased. The design charge NP of the battery is 1.20.

[0187] according to Calculation is performed, where n = 200, a = 0.00017, and Y0 is set according to the NP range of 1.03-1.20 for conventional silicon-free cells. The calculated Y 0,S Please refer to Table 1 for the range values.

[0188] Table 1

[0189]

[0190] The performance test of the secondary battery 100 will be described below.

[0191] The battery capacity of the secondary battery 100 in the above embodiment and comparative example, as well as the extreme storage and extreme cycling (for specific methods, please refer to the above methods and will not be repeated here) are measured. The data of N1 (number of days) and N2 (number of cycles) are obtained respectively. For specific parameters, please refer to Table 2.

[0192] Battery capacity test of the secondary battery 100:

[0193] At 25°C, charge at 0.5C to the full charge voltage; then charge at constant voltage at the full charge voltage until the current is ≤ 0.05C, let it stand for 30 minutes, and then discharge at 1C to the full discharge voltage; record the capacity value at the end of discharge.

[0194] Comparing Example 1 with Comparative Example 1, Example 2 with Comparative Example 2, Example 3 with Comparative Example 3 and Comparative Example 4, Example 4 with Comparative Example 5, and Example 5 with Comparative Example 6, it can be seen that the initial (e.g., first charge or first discharge, etc.) NP designed according to the above formula reduces the NP value design of the secondary battery 100, and the battery capacity of the secondary battery 100 obtained is higher; at the same time, under the same cycle ratio, the lifespan of the secondary battery 100 achieved during storage and cycling is consistent. In this way, determining the design of the NP value based on the storage ratio is conducive to achieving a balance between high energy density and long life.

[0195] Table 2

[0196]

[0197] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, rather than to limit them. Although this application has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of this application, and they should all be included in the scope of the claims and description of this application. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. An electrode assembly, comprising: a positive electrode sheet and a negative electrode sheet; The condition satisfied between NP and S when the current capacity retention rate of the electrode assembly is not less than m is: 1.17 - 0.35S ≤ NP ≤ -0.41S + 1.36, 50% ≤ S ≤ 80%, and m ≥ 99%; Wherein, NP is the ratio of the capacity per unit area of the negative electrode sheet to the capacity per unit area of the positive electrode sheet; S is the storage ratio of the electrode assembly. The number of storage days that the electrode assembly can reach when its capacity retention rate is 80% under extreme storage is denoted as N1, and the number of charge-discharge cycles that the electrode assembly can reach when its capacity retention rate is 80% under extreme charge-discharge cycling is denoted as N2, S = 5N1 / (5N1 + N2); The extreme storage means that the electrode assembly is stored at a temperature of 60°C in a 100% SoC state; The extreme cycling means that the electrode assembly is charged at a rate of 0.5C and discharged at a rate of 1C at 25°C, and continuously cycled within the range of 0% - 100% SoC; The current capacity retention rate of the electrode assembly is the ratio of the current capacity T1 of the electrode assembly to the initial capacity T2 of the electrode assembly.

2. The electrode assembly according to claim 1, wherein When the storage ratio S is 50% - 80%, the NP value of the electrode assembly is: 0.89~1.16; Optionally, when the storage ratio S is 70% - 80%, the NP value of the electrode assembly is: 0.95~1.07。 3. The electrode assembly according to claim 1 or 2, wherein: The unit area capacity of the negative electrode sheet is recorded as P1, and the unit area capacity of the positive electrode sheet is recorded as P2. The conditions satisfied by P1 and P2 are: 2.3 mAh / cm 2 ≤P1≤8.6mAh / cm 2 ; 1.5mAh / cm 2 ≤P2≤6.8mAh / cm 2 .

4. The electrode assembly according to any one of claims 1 to 3, wherein: The coating weight per unit area of ​​the negative electrode sheet is in the range of 3.9 mg / cm 2 ~13mg / cm 2 Optionally, the coating weight per unit area of ​​the negative electrode sheet is in the range of 3.9 mg / cm 2 ~10mg / cm 2 and / or, The coating weight per unit area of ​​the positive electrode sheet is in the range of 6.5 mg / cm 2 ~29mg / cm 2 Optionally, the coating weight per unit area of ​​the positive electrode sheet is in the range of 9 mg / cm 2 ~21mg / cm 2 .

5. The electrode assembly according to any one of claims 1 to 4, wherein: The negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes at least one of a silicon material and a carbon material.

6. The electrode assembly according to claim 5, wherein: The silicon material includes at least one of Si and SiOz (0 < z < 2); and / or, The carbon material includes at least one of natural graphite, artificial graphite, mesophase microcarbon beads, hard carbon, and soft carbon; Optionally, the carbon material includes natural graphite and artificial graphite.

7. The electrode assembly according to claim 5, characterized in that The weight percentage of the silicon material in the negative electrode active material is 3% - 50%; Optionally, the weight percentage of the silicon material in the negative electrode active material is 3% - 25%.

8. The electrode assembly according to any one of claims 1 to 7, wherein: The NP of the electrode assembly during the first charge or first discharge is recorded as Y 0,S , Y 0,S The conditions satisfied between S are: Wherein, Y0 refers to the NP value set for the reference electrode assembly during the first charge or first discharge, and 1.03≤Y0≤1.2, and a refers to the capacity loss value caused by each cycle of charge and discharge of the reference electrode assembly.

9. The electrode assembly according to claim 8, wherein Y 0,S The conditions satisfied between S are:

10. The electrode assembly according to claim 8 or 9, wherein: Y0 also satisfies the condition: 1.05 ≤ Y0 ≤ 1.

15.

11. The electrode assembly according to claim 8 or 9, wherein: a satisfies the condition: 0.00016 ≤ a ≤ 0.00026; Optionally, a also satisfies the condition: 0.00018 ≤ a ≤ 0.00024.

12. The electrode assembly according to any one of claims 1 to 11, wherein: The positive electrode sheet includes a positive electrode active material, and the positive electrode active material is an active substance capable of intercalating and deintercalating lithium ions.

13. The electrode assembly according to claim 12, wherein: The positive electrode active material includes one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide; and compounds obtained from transition metals or non-transition metals; Optionally, the positive electrode active material includes a lithium-containing transition metal composite oxide, wherein the transition metal includes at least one selected from nickel, cobalt, manganese, and aluminum.

14. A secondary battery, comprising: a housing; The electrode assembly according to any one of claims 1 - 13, housed in the housing; an electrolyte, filled in the housing.

15. An electrical device, comprising the secondary battery according to claim 14.