Cylindrical secondary battery

By using a positive electrode active material containing lithium-containing composite oxide with sulfonic acid compounds attached to its surface in large batteries, and by optimizing the positive electrode flux layer and lead connection, the problem of reduced output characteristics caused by insufficient electrolyte in large batteries has been solved, achieving a balance between high capacity and high output characteristics.

CN118891746APending Publication Date: 2024-11-01PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028026.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-14
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously improve battery capacity and output characteristics per unit volume in large-scale batteries.

Method used

The positive electrode active material is made by attaching sulfonic acid compounds to the surface of lithium-containing composite oxide, and the battery structure is improved by setting the unit area weight of the positive electrode agent layer to above 250g/m2 and combining it with an appropriate positive electrode lead connection method.

Benefits of technology

This achieves high capacity per unit volume and improved output characteristics, thereby enhancing the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891746A_ABST
    Figure CN118891746A_ABST
Patent Text Reader

Abstract

This cylindrical secondary battery is provided with: an electrode body in which a belt-shaped positive electrode and a belt-shaped negative electrode are wound with a separator therebetween; a bottomed cylindrical exterior body that accommodates the electrode body, is connected to the negative electrode, and has an outer diameter of 25 mm or more; the positive electrode has a positive electrode current collector and a positive electrode mixture layer formed on the surface of the positive electrode current collector, and the positive electrode mixture layer contains a positive electrode active material and a sulfonic acid compound represented by general formula (I). The positive electrode active material contains a lithium-containing composite oxide having a layered rock salt structure, the weight per unit area of the positive electrode mixture layer is 250 g / m2 or more, and three or more positive electrode leads are led out from the electrode body. (In the formula, A is a group 1 element or a group 2 element, R is a hydrocarbon group, and n is 1 or 2. > # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a cylindrical secondary battery. Background Art

[0002] In recent years, as a high-output, high-capacity secondary battery, a non-aqueous electrolyte secondary battery having a positive electrode, a negative electrode and a non-aqueous electrolyte, which moves Li ions between the positive electrode and the negative electrode for charging and discharging, has been widely used. Patent document 1 discloses a cylindrical secondary battery, which improves the output characteristics of the battery by configuring a collector component above and below an electrode body with multiple tabs protruding, and suppresses the cost of the collector component. In addition, patent document 2 discloses a positive electrode active material having a lithium sulfonate salt compound attached to the surface of lithium titanate, and records that the positive electrode active material has excellent high-temperature storage characteristics.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent No. 5747082

[0006] Patent Document 2: Japanese Patent Application Publication No. 2018-6164 Summary of the invention

[0007] However, in recent years, the enlargement of batteries has been studied for the purpose of improving the battery capacity per unit volume. The present inventors have conducted in-depth research and found that even if the technologies described in Patent Documents 1 and 2 are combined, it is impossible to improve the battery capacity per unit volume and improve the output characteristics in a large battery. The technologies described in Patent Documents 1 and 2 do not study the enlargement of batteries, and there is still room for improvement.

[0008] An object of the present disclosure is to provide a cylindrical secondary battery having improved battery capacity per unit volume and improved output characteristics.

[0009] A cylindrical secondary battery as one embodiment of the present invention is characterized in that it comprises: an electrode body formed by winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator interposed therebetween; an outer casing having an outer diameter of 25 mm or more and a bottomed cylindrical shape that accommodates the electrode body and is connected to the negative electrode; and a sealing body that seals the opening at the upper end of the outer casing and is connected to the positive electrode, wherein the positive electrode comprises a positive electrode collector and a positive electrode mixture layer formed on the surface of the positive electrode collector, the positive electrode mixture layer contains a positive electrode active material, the positive electrode active material comprises a lithium-containing composite oxide having a layered rock salt structure and a sulfonic acid compound present on the surface of the lithium-containing composite oxide, the sulfonic acid compound is represented by the following general formula (I), and the unit area weight of the positive electrode mixture layer is 250 g / m 2 As described above, three or more positive electrode leads are led out from the electrode body.

[0010]

[0011] (In the formula, A is a Group 1 element or a Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0012] A cylindrical secondary battery as another embodiment of the present invention is characterized in that it comprises: an electrode body formed by winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator interposed therebetween; an outer casing having an outer diameter of 25 mm or more and a bottomed cylindrical shape that accommodates the electrode body and is connected to the negative electrode; and a sealing body that seals the opening at the upper end of the outer casing and is connected to the positive electrode, wherein the positive electrode comprises a positive electrode collector and a positive electrode mixture layer formed on the surface of the positive electrode collector, the positive electrode mixture layer contains a positive electrode active material, the positive electrode active material comprises a lithium-containing composite oxide having a layered rock salt structure and a sulfonic acid compound present on the surface of the lithium-containing composite oxide, the sulfonic acid compound is represented by the following general formula (I), and the unit area weight of the positive electrode mixture layer is 250 g / m 2 In the above, the positive electrode protruding upward from the negative electrode and the separator in the electrode assembly is connected to the positive electrode current collecting member, and the positive electrode current collecting member and the sealing body are connected via the positive electrode lead.

[0013]

[0014] (In the formula, A is a Group 1 element or a Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0015] According to the cylindrical secondary battery which is one embodiment of the present disclosure, it is possible to achieve both high capacity per unit volume and improved output characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a longitudinal cross-sectional view of a cylindrical secondary battery as an example of an embodiment.

[0017] Figure 2 The structure is shown in the expanded state Figure 1 A front view of a positive electrode and a negative electrode of an electrode body included in a cylindrical secondary battery.

[0018] Figure 3 The diagrams are plan views showing the positions of positive electrode leads arranged on the upper surface of the electrode body. (a) shows an example in which positive electrode leads are arranged substantially in a row in the radial direction, and (b) shows an example in which positive electrode leads are arranged at substantially equal angles.

[0019] Figure 4 It is a longitudinal cross-sectional view of a cylindrical secondary battery as another example of the embodiment.

[0020] Figure 5 yes Figure 31 is a perspective view of an electrode assembly of a cylindrical secondary battery, showing the structure of a positive electrode, a negative electrode, and a separator in a state where the vicinity of a rolled outer end portion is unfolded. DETAILED DESCRIPTION

[0021] In recent years, the enlargement of batteries has been studied for the purpose of improving the battery capacity per unit volume. However, compared with conventional batteries, the electrolyte in the large-scale battery is easily insufficient in the winding center of the electrode body, so the output characteristics are easily reduced. In order to solve this problem, the present inventors have conducted in-depth research and found that by using a positive electrode active material having a sulfonic acid compound represented by the following general formula I attached to the surface of a lithium-containing composite oxide, the output characteristics are improved. It is speculated that this is because the effect of the sulfonic acid compound promotes the movement of Li between the positive electrode active material and the electrolyte even if the electrolyte is small. Therefore, by setting the outer diameter of the battery to more than 25 mm and setting the unit area weight of the positive electrode mixture layer to 250 g / m 2 As described above, by setting the connection between the positive electrode and the sealing body in a predetermined manner, the capacity per unit volume of the secondary battery can be increased, and by using the above-mentioned positive electrode active material, the output characteristics of the secondary battery can be improved.

[0022]

[0023] (In the formula, A is a Group 1 element or a Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0024] Below, refer to Figure 1 to Figure 3 , while describing in detail an example of an embodiment of the cylindrical secondary battery disclosed in the present invention. In the following description, specific shapes, materials, numerical values, directions, etc. are examples used to make the present invention easy to understand, and can be appropriately changed according to the specifications of the cylindrical secondary battery. In addition, in the following description, when multiple embodiments and variations are included, it is envisaged from the beginning that these characteristic parts will be used in appropriate combination. In addition, in this specification, when the term "approximately" is used, it is used in the same meaning as the term "approximately", and the condition of "approximately to" can be satisfied as long as it is substantially the same.

[0025] Figure 1 It is a longitudinal cross-sectional view of a cylindrical secondary battery 10 as an example of an embodiment. Figure 1In the secondary battery 10 shown, the electrode body 14 and the electrolyte (not shown) are contained in the outer body 15. The electrode body 14 has a winding structure in which a strip-shaped positive electrode 11 and a strip-shaped negative electrode 12 are wound across a separator 13. As a non-aqueous solvent (organic solvent) of the electrolyte, carbonates, lactones, ethers, ketones, esters, etc. can be used, and these solvents can be mixed with two or more. When two or more solvents are mixed, it is preferred to use a mixed solvent containing cyclic carbonates and chain carbonates. For example, as cyclic carbonates, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used, and as chain carbonates, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC), etc. can be used. As an electrolyte salt of the electrolyte, LiPF6, LiBF4, LiCF3SO3, etc. and mixtures thereof can be used. The amount of the electrolyte salt dissolved in the nonaqueous solvent may be, for example, 0.5 mol / L to 2.0 mol / L. In the following, for convenience of description, the sealing body 16 side is referred to as "upper" and the bottom side of the outer body 15 is referred to as "lower".

[0026] The opening at the upper end of the outer body 15 is sealed by the sealing body 16, and the interior of the secondary battery 10 is sealed. Insulating plates 17 and 18 are respectively provided above and below the electrode body 14. The positive lead 19 extends up and down through the through hole of the insulating plate 17, connecting the bottom plate of the sealing body 16, that is, the perforated metal plate 22, to the positive electrode 11 contained in the electrode body 14. Thus, the positive electrode 11 is connected to the sealing body 16, and in the secondary battery 10, the top plate of the sealing body 16, that is, the cover 26, which is electrically connected to the perforated metal plate 22, becomes the positive terminal. The positive lead 19 is, for example, an aluminum lead. On the other hand, the negative lead 20 extends on the bottom side of the outer body 15 through the through hole of the insulating plate 18 and is welded to the bottom inner surface of the outer body 15. Thus, the negative electrode 12 is connected to the outer body 15, and in the secondary battery 10, the outer body 15 becomes the negative terminal. The negative lead 20 is, for example, a nickel lead.

[0027] In the electrode body 14, three positive leads 19 are led out. The number of positive leads 19 led out from the electrode body 14 may be three or more. Thus, the connection resistance between the positive electrode 11 and the sealing body 16 can be suppressed, so the output characteristics of the secondary battery 10 can be improved. The more the number of positive leads 19, the more the connection resistance is suppressed, but the cost of the secondary battery 10 increases. Therefore, from the perspective of both the suppression effect of the connection resistance and the cost, the number of positive leads 19 is preferably 3 to 10, more preferably 3 to 8, and particularly preferably 3 to 6. It should be noted that the three or more positive leads 19 led out from the electrode body 14 can be directly connected to the sealing body 16, or can be connected to the sealing body 16 by a known current collecting member. In addition, there is no particular limitation on the connection method between the negative electrode 12 and the outer body 15, and multiple negative leads 20 can be used for connection.

[0028] The outer body 15 is a bottomed cylindrical shape with an outer diameter of 25 mm or more. The outer diameter of the outer body 15 is preferably 30 mm or more, and more preferably 35 mm or more. In addition, the outer diameter of the outer body 15 can be 38 mm or more, 40 mm or more, 45 mm or more, or 50 mm or more. The outer diameter of the outer body 15 can be, for example, 60 mm or less. If it is within this range, the battery capacity per unit volume of the secondary battery 10 can be improved. The thickness of the outer body 15 is, for example, 0.1 mm to 2 mm, and the inner diameter of the outer body 15 is preferably 24 mm or more, more preferably 29 mm or more, and particularly preferably 34 mm or more. In addition, the inner diameter of the outer body 15 can be 37 mm or more, 39 mm or more, 44 mm or more, or 49 mm or more. The outer body 15 is, for example, a metal outer can. A gasket 27 is provided between the outer body 15 and the sealing body 16 to ensure the airtightness of the interior of the secondary battery 10. The outer casing 15 has a groove 21 formed by pressing the side surface from the outside, for example, to support the sealing body 16. The groove 21 is preferably formed in an annular shape along the circumferential direction of the outer casing 15, and supports the sealing body 16 on its upper surface.

[0029] The sealing body 16 has a perforated metal plate 22, a lower valve core 23, an insulating member 24, an upper valve core 25 and a cover 26 stacked in sequence from the electrode body 14 side. The components constituting the sealing body 16 have, for example, a disc shape or a ring shape, and the components except the insulating member 24 are electrically connected to each other. The lower valve core 23 and the upper valve core 25 are connected to each other at their respective central portions, and an insulating member 24 is sandwiched between their respective peripheral portions. If the internal pressure of the battery rises due to abnormal heat release, for example, the lower valve core 23 breaks, whereby the upper valve core 25 expands toward the cover 26 side and leaves the lower valve core 23, thereby disconnecting the electrical connection between the two. When the internal pressure rises further, the upper valve core 25 breaks, and the gas is discharged from the opening 26a of the cover 26.

[0030] Next, refer to Figure 2 The connection method between the positive electrode 11 and the positive electrode lead 19 will be described. Figure 2 The structure is shown in the expanded state Figure 1 The front view of the positive electrode 11 and the negative electrode 12 of the electrode body 14 of the secondary battery 10 is shown. The positive electrode 11 has a positive electrode collector 30 and a positive electrode mixture layer 32 formed on the surface of the positive electrode collector 30, and the negative electrode 12 has a negative electrode collector 40 and a negative electrode mixture layer 42 formed on the surface of the negative electrode collector 40.

[0031] like Figure 2 As shown, the positive electrode 11 has a plurality of positive electrode collector exposed portions 34 at the upper end along the length direction, where the positive electrode collector 30 is exposed, and there is a positive electrode mixture layer 32 between the positive electrode collector exposed portions 34. The positive electrode collector exposed portions 34 are respectively connected to one of the positive electrode leads 19. By connecting the positive electrode lead 19 to the positive electrode 11 in this way, the area of ​​the positive electrode mixture layer 32 can be increased, so that the output characteristics of the secondary battery 10 can be improved. On the other hand, the negative electrode 12 has a negative electrode collector exposed portion 44 at the inner end of the roll in the length direction, where the negative electrode collector 40 is exposed. The negative electrode collector exposed portion 44 is connected to the negative electrode lead 20.

[0032] Next, refer to Figure 3 (a) and Figure 3 The arrangement of the positive electrode lead 19 will be described in the following (b). Figure 3 (a) and Figure 3 (b) are all plan views showing the position where the positive electrode lead 19 is arranged on the upper surface of the electrode body 14 .

[0033] like Figure 3 As shown in (a), the positive electrode lead 19 can be arranged in a substantially straight line in the radial direction. This makes it easy to bundle the positive electrode lead 19 and to join the positive electrode lead 19 to the perforated metal plate 22. Figure 3 In (a), all positive electrode leads 19 are arranged on one side relative to the center of electrode body 14, but positive electrode leads 19 may be arranged on both sides relative to the center of electrode body 14. In addition, the positive electrode lead 19 may be joined to the perforated metal plate 22 at multiple locations.

[0034] like Figure 3 As shown in (b), the positive electrode leads 19 can be arranged at substantially equal angles. Thus, each of the plurality of positive electrode leads 19 can be easily joined to the perforated metal plate 22 without being obstructed by other positive electrode leads 19 .

[0035] Below, refer to Figure 4 and Figure 5Another embodiment of the cylindrical secondary battery disclosed in the present invention will be described in detail. Figure 1 The same structures as in the embodiment shown are labeled Figure 1 The same reference numerals as those in the embodiments shown in the drawings are used and the description thereof is omitted. Figure 1 Description of the same effects and modifications as those of the embodiment shown.

[0036] Figure 4 In another example of the implementation mode Figure 1 The corresponding figure. Figure 4 As shown, the positive electrode 11 included in the electrode body 14 is connected to the positive electrode collector component 50, and the positive electrode collector component 50 is connected to the sealing body 16 through the positive electrode lead 19. Thus, the positive electrode 11 is connected to the sealing body 16, and in the secondary battery 10, the top plate of the sealing body 16 electrically connected to the perforated metal plate 22, that is, the cover 26 becomes the positive terminal. In addition, the negative electrode 12 included in the electrode body 14 is connected to the negative electrode collector component 52, and the negative electrode collector component 52 is connected to the outer body 15 through the negative electrode lead 20. Thus, the negative electrode 12 is connected to the outer body 15, and in the secondary battery 10, the outer body 15 becomes the negative terminal. It should be noted that there is no particular limitation on the connection method between the negative electrode 12 and the outer body 15. For example, it can be connected to Figure 1 The embodiment shown is likewise connected using a negative lead 20 .

[0037] As long as the positive electrode current collecting member 50 can be connected to the positive electrode 11 and the sealing body 16, the material, shape, etc. are not particularly limited, for example, it can be a disc-shaped member made of aluminum. In addition, from the perspective of the circulation of the electrolyte, the positive electrode current collecting member 50 can have a single or multiple holes at any position. As long as the negative electrode current collecting member 52 can be connected to the negative electrode 12 and the outer body 15, the material, shape, etc. are not particularly limited, for example, it can be a disc-shaped member made of nickel. In addition, from the perspective of the circulation of the electrolyte, the negative electrode current collecting member 52 can have a single or multiple holes at any position.

[0038] Next, refer to Figure 5 The structure of the electrode body 14 will be described. Figure 5 yes Figure 4 The three-dimensional view of the electrode body 14 in the secondary battery 10 shown in FIG. 1 is a view showing the structure of the positive electrode 11, the negative electrode 12 and the separator 13 in a state where the outer end of the roll is unfolded. In the electrode body 14, the positive electrode 11 protrudes upward more than the negative electrode 12 and the separator 13. Thus, the positive electrode 11 is connected to the positive electrode current collecting member 50. Figure 5As shown, the positive electrode 11 may have a positive electrode collector exposed portion 34 at the upper end where the positive electrode collector 30 is exposed. Thus, the positive electrode 11 can be more reliably connected to the positive electrode collector member 50. On the other hand, the negative electrode 12 protrudes downward more than the positive electrode 11 and the separator 13. Thus, the negative electrode 12 is connected to the negative electrode collector member 52. Figure 5 As shown, the negative electrode 12 may have a negative electrode current collector exposed portion 44 at the lower end portion where the negative electrode current collector 40 is exposed. This allows the negative electrode 12 and the negative electrode current collecting member 52 to be connected more reliably.

[0039] Hereinafter, the positive electrode 11, the negative electrode 12 and the separator 13 constituting the electrode body 14, in particular the positive electrode 11 will be described in detail. It should be noted that the positive electrode 11, the negative electrode 12 and the separator 13 described below can be applied to any of the above-mentioned embodiments.

[0040] [positive electrode]

[0041] The positive electrode 11 includes a positive electrode current collector 30 and a positive electrode mixture layer 32 formed on the surface of the positive electrode current collector 30. The positive electrode mixture layer 32 is preferably formed on both sides of the positive electrode current collector 30. The positive electrode current collector 30 can be made of a foil of a metal such as aluminum or an aluminum alloy that is stable within the potential range of the positive electrode 11, or a thin film having the metal disposed on the surface.

[0042] The positive electrode mixture layer 32 contains a positive electrode active material. In addition, the positive electrode mixture layer 32 may further contain a conductive agent, a binder, etc. The positive electrode mixture layer 32 can be produced, for example, by applying a positive electrode slurry containing a positive electrode active material, a conductive agent, a binder, etc. on the surface of the positive electrode collector 30, drying the coating film, and then rolling it.

[0043] As the conductive agent contained in the positive electrode mixture layer 32, carbon materials such as carbon black (CB), acetylene black (AB), Ketjen black, carbon nanotubes (CNT), graphene, and graphite can be listed. They can be used alone or in combination of two or more. The content of the conductive agent in the positive electrode mixture layer 32 is preferably 0.01% by mass to 5% by mass, and more preferably 0.05% by mass to 3% by mass relative to the total mass of the positive electrode mixture layer 31.

[0044] As the binder contained in the positive electrode mixture layer 32, for example, fluorine resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyimide resins, acrylic resins, polyolefin resins, polyacrylonitrile (PAN), etc. can be listed. They can be used alone or in combination of two or more. The content of the binder in the positive electrode mixture layer 32 is preferably 0.1% by mass to 5% by mass, and more preferably 0.5% by mass to 3% by mass relative to the total mass of the positive electrode mixture layer 32.

[0045] The weight per unit area of ​​the positive electrode mixture layer 32 is 250 g / m 2 As a result, the cost of the secondary battery 10 can be reduced. The weight per unit area of ​​the positive electrode mixture layer 32 can be 400 g / m 2 The thickness of the positive electrode mixture layer 32 is, for example, 10 μm to 150 μm on one side of the positive electrode current collector 30 .

[0046] The positive electrode active material contained in the positive electrode mixture layer 32 includes a lithium-containing composite oxide having a layered rock salt structure and a sulfonic acid compound present on the surface of the lithium-containing composite oxide. The lithium-containing composite oxide includes, for example, secondary particles formed by aggregation of primary particles. Here, the surface of the lithium-containing composite oxide refers to the surface of the secondary particles of the lithium-containing composite oxide, or the interface where the primary particles are in contact with each other. That is, the sulfonic acid compound is present on the surface of the secondary particles of the lithium-containing composite oxide, or the interface where the primary particles are in contact with each other.

[0047] The particle size of the primary particles constituting the secondary particles of the lithium-containing composite oxide is, for example, 0.02 μm to 2 μm. The particle size of the primary particles is measured as the diameter of the circumscribed circle in the particle image observed using a scanning electron microscope (SEM). The average particle size of the secondary particles of the lithium-containing composite oxide is, for example, 2 μm to 30 μm. Here, the average particle size refers to the median particle size (D50) based on volume. D50 refers to the particle size at which the accumulation of frequencies from the smaller particle size in the volume-based particle size distribution reaches 50%, also known as the median diameter. The particle size distribution of the secondary particles of the lithium-containing composite oxide can be measured using a laser diffraction particle size distribution measuring device (e.g., MT3000II manufactured by MicrotracBEL Corp.) using water as the dispersion medium.

[0048] The lithium-containing composite oxide may be a mixture of particles having a D50 of 10 μm or more and particles having a D50 of 6 μm or less. This can increase the packing density of the positive electrode active material in the positive electrode mixture layer 32, thereby increasing the battery capacity. The particles having a D50 of 10 μm or more and the particles having a D50 of 6 μm or less are, for example, secondary particles.

[0049] The layered rock salt structure of the lithium-containing composite oxide belongs to, for example, space group R-3m, space group C2 / m, etc. In terms of high capacity and stability of the crystal structure, the lithium-containing composite oxide preferably has a layered rock salt structure belonging to space group R-3m. The layered rock salt structure of the lithium-containing composite oxide may include a transition metal layer, a Li layer, and an oxygen layer. The charge and discharge reaction of the battery is carried out by reversibly entering and exiting the Li ions present in the Li layer.

[0050] The lithium-containing composite oxide contains Ni, for example, and the content of Ni in the lithium-containing composite oxide can be 70 mol% to 95 mol% relative to the total molar number of metal elements other than Li. Thus, a high-capacity battery is obtained. The ratio of Ni in the lithium-containing composite oxide to the total molar number of metal elements other than Li is preferably 80 mol% or more. Thus, a higher-capacity battery is obtained.

[0051] The lithium-containing composite oxide may be of the general formula Li a Ni x Co y Al z Mn w M1 v O 2-b (wherein, 0.95≤a≤1.05, 0.7≤x≤0.95, 0≤y≤0.15, 0≤z≤0.1, 0≤w≤0.3, 0≤v≤0.1, 0≤b≤0.05, x+y+z+w+v=1, M1 contains at least one element selected from Fe, Ti, Si, Nb, Zr, Mo, W and Zn). It should be noted that the positive electrode active material may contain lithium-containing composite oxides or other compounds other than those shown in the above general formula within the scope of not impairing the purpose of the present disclosure. The molar fraction of the metal element contained in the entire particle of the lithium-containing composite oxide is determined by inductively coupled plasma (ICP) emission spectroscopy.

[0052] The sulfonic acid compound present on the surface of the lithium-containing composite oxide is represented by the following general formula I.

[0053]

[0054] (In the formula, A is a Group 1 element or a Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0055] In the general formula I, A is preferably a Group 1 element, more preferably Li. This can further improve the initial charge and discharge efficiency. It should be noted that when A is a Group 1 element, n=1.

[0056] In the general formula I, R is preferably an alkyl group. R is more preferably an alkyl group having 5 or less carbon atoms, further preferably an alkyl group having 3 or less carbon atoms, and particularly preferably a methyl group. In addition, in R, a portion of the hydrogen bonded to the carbon may be replaced by fluorine. However, in R, the hydrogen bonded to the carbon may not be completely replaced by fluorine. The smaller the molecular weight of R, the more the reaction resistance can be reduced.

[0057] Examples of the sulfonic acid compound include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, magnesium methanesulfonate, and lithium fluoromethanesulfonate.

[0058] The amount of the sulfonic acid compound present on the surface of the lithium-containing composite oxide is preferably 0.1% by mass to 1% by mass, and more preferably 0.3% by mass to 0.8% by mass, based on the mass of the lithium-containing composite oxide.

[0059] The presence of sulfonic acid compounds on the surface of the lithium-containing composite oxide can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode active material can be detected at 1238 cm -1 、1175cm -1 、1065cm -1 、785cm -1 At least one or more locations nearby have an absorption peak.

[0060] In the infrared absorption spectrum obtained by FT-IR, for example, the positive electrode active material containing lithium methanesulfonate has an absorption spectrum at 1238 cm -1 、1175cm -1 、1065cm -1 、785cm -1 There is an absorption peak near 1238cm -1 、1175cm -1 、1065cm -1 The nearby peak is the absorption peak caused by the SO stretching vibration of lithium methanesulfonate. -1 The nearby peak is an absorption peak derived from the CS stretching vibration of lithium methanesulfonate.

[0061] For the positive electrode active material containing a sulfonic acid compound other than lithium methanesulfonate, the absorption peak derived from the sulfonic acid compound contained in the positive electrode active material can be identified in the same manner as the positive electrode active material containing lithium methanesulfonate. It should be noted that the presence of the sulfonic acid compound on the surface of the lithium-containing composite oxide can also be confirmed by ICP, atomic absorption spectrometry, X-ray photoelectron spectroscopy (XPS), synchrotron radiation XRD measurement, TOF-SIMS, etc.

[0062] The average particle size of the sulfonic acid compound is preferably less than 10 μm, more preferably less than 5 μm, and further preferably less than 3 μm. By making the average particle size of the sulfonic acid compound preferably less than 10 μm, more preferably less than 5 μm, and further preferably less than 3 μm, it can be more evenly attached to the entire positive electrode active material powder, and the effect of the sulfonic acid compound can be more significantly manifested. The lower limit of the average particle size of the sulfonic acid compound is, for example, 0.1 μm. Here, the average particle size of the sulfonic acid compound can be obtained by observing the sulfonic acid compound attached to the surface of the lithium-containing composite oxide with a SEM. Specifically, after determining the outer shape of 50 randomly selected particles, the long diameter (longest diameter) of each of the 50 particles is obtained, and their average value is taken as the average particle size of the sulfonic acid compound.

[0063] Metal compounds may be present on the surface of the lithium-containing composite oxide. The metal compound, for example, contains one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earths and Al. As compounds containing Sr, SrO, Sr(OH)2, and SrCO3 can be exemplified. As compounds containing Ca, CaO, Ca(OH)2, and CaCO3 can be exemplified. As compounds containing W, WO3 can be exemplified. As compounds containing Al, Al2O3 can be exemplified. As compounds containing Zr, ZrO2, Zr(OH)4, Zr(CO3)2, and Zr(SO4)2·4H2O can be exemplified. As compounds containing rare earths, oxides, hydroxides, carbonates, sulfates, nitrates, and phosphates of rare earths can be exemplified. In addition, the metal compound may contain a plurality of these metal elements, and SrAlO4 and CaAlO4 can be exemplified. The metal compound may also contain Li, and lithium tungstate can be exemplified.

[0064] A non-metal compound may exist on the surface of the lithium-containing composite oxide. For example, the non-metal compound contains one or more non-metal elements selected from the group consisting of P and B. Examples of the compound containing P include Li 3-x H x PO4 (0≤x≤3). Examples of the compound containing B include H3BO3, Li3BO3, and Li2B4O7.

[0065] For the positive electrode active material, in the case of the filtrate of the aqueous dispersion obtained by dispersing 1g of the positive electrode active material in 70ml of pure water with hydrochloric acid titration, the acid consumption until the first inflection point of the pH curve is set to Xmol / g, and the acid consumption until the second inflection point is set to Ymol / g, and the value of YX is preferably 130μmol / g or less, more preferably 100μmol / g or less, and further preferably 60μmol / g or less. In addition, the value of X-(YX) is preferably 130μmol / g or less, more preferably 100μmol / g or less, and further preferably 60μmol / g or less. That is, the positive electrode active material may slightly contain a water-soluble alkaline component titrated with acid. When the amount of the alkaline component contained in the positive electrode active material is small, the stability of the slurry is improved and the productivity is improved.

[0066] The positive electrode active material contains only an alkali component equivalent to the amount of the above-mentioned acid consumption. As an alkali component, for example, lithium hydroxide (LiOH), lithium carbonate (Li2CO3) and the like can be listed. Lithium carbonate and lithium hydroxide can exist on the interface of each primary particle and the surface of the secondary particles formed by the aggregation of primary particles inside the particles of the composite oxide. They are preferably present uniformly rather than unevenly on a part of the surface of the primary particles.

[0067] The specific quantitative method of the water-soluble alkaline component extracted from the positive electrode active material is as follows. The following titration method is generally called the Warder method.

[0068] (1) 1 g of the positive electrode active material was added to 30 ml of pure water and stirred to prepare a suspension in which the active material was dispersed in water.

[0069] (2) The suspension is filtered and pure water is added to make the volume 70 ml to obtain a filtrate containing a water-soluble alkaline component dissolved from the active substance.

[0070] (3) While measuring the pH of the filtrate, hydrochloric acid is added dropwise to the filtrate, and the amount of hydrochloric acid consumed until the first inflection point of the pH curve (near pH 8) (titration) X mol / g and the amount of hydrochloric acid consumed until the second inflection point (near pH 4) Y mol / g are calculated. It should be noted that the inflection point is the peak position of the differential value relative to the titration.

[0071] The positive electrode mixture layer 31 may contain other positive electrode active materials in addition to the positive electrode active material of the present embodiment described above. Examples of other positive electrode active materials include lithium-containing composite oxides having no sulfonic acid compound on the surface.

[0072] Next, an example of a method for producing a positive electrode active material according to the present embodiment is described. The method for producing a positive electrode active material includes, for example, a synthesis step, a washing step, a drying step, and an adding step.

[0073] In the synthesis process, for example, a metal oxide containing 70 mol% to 95 mol% of Ni, 0 mol% to 15 mol% of Co, 0 mol% to 10 mol% of Al, 0 mol% to 30 mol% of Mn, and 0 mol% to 10 mol% of M1 (M1 contains at least one element selected from Fe, Ti, Si, Nb, Zr, Mo, W and Zn) is mixed with a Li compound and calcined to obtain a lithium-containing composite oxide.

[0074] The metal oxide can be obtained, for example, by stirring a solution of a metal salt containing Ni and any metal element (Co, Al, Mn, Fe, etc.), while dropping an alkaline solution such as sodium hydroxide, adjusting the pH to the alkaline side (e.g., 8.5 to 12.5), thereby precipitating (coprecipitating) a composite hydroxide containing Ni and any metal element, and heat-treating the composite hydroxide to obtain the above-mentioned metal oxide. The heat treatment temperature is not particularly limited, for example, in the range of 300° C. to 600° C.

[0075] As the Li compound, for example, Li2CO3, LiOH, Li2O2, Li2O, LiNO3, LiNO2, Li2SO4, LiOH·H2O, LiH, LiF, etc. can be listed. From the viewpoint of easily adjusting the above parameters to the above-mentioned specified range, the mixing ratio of the metal oxide and the Li compound is preferably set to a ratio in which the molar ratio of the metal element other than Li: Li is in the range of 1:0.98 to 1:1.1. It should be noted that when the metal oxide is mixed with the Li compound, other metal raw materials can be added as needed. Here, other metal raw materials refer to oxides of metal elements other than the metal elements constituting the metal oxide, etc.

[0076] The mixture of metal oxide and Li compound is calcined, for example, in an oxygen atmosphere. The calcination conditions may be a temperature rise rate of more than 450°C and less than 680°C in a range of more than 1.0°C / min and less than 5.5°C / min, and a maximum temperature of more than 700°C and less than 980°C. The temperature rise rate from more than 680°C to the maximum temperature may be, for example, 0.1°C / min to 3.5°C / min. In addition, the holding time to the maximum temperature may be more than 1 hour and less than 10 hours. In addition, the calcination process may be a multi-stage calcination, and a plurality of the first temperature rise rate and the second temperature rise rate may be set in each temperature region as long as they are within the above-specified range.

[0077] In the washing step, the lithium-containing composite oxide obtained in the synthesis step is washed with water and dehydrated to obtain a filter cake-like composition. The washing and dehydration can be performed by known methods and conditions. It can be performed within a range that does not cause lithium to dissolve from the lithium-containing composite oxide and deteriorate the battery characteristics. It should be noted that the positive electrode active material of this embodiment has less residual alkali components because it is washed with water.

[0078] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step can be performed in a vacuum atmosphere. The drying conditions are, for example, 150° C. to 400° C. and 0.5 to 15 hours.

[0079] In the adding process, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the filter cake-like composition obtained in the washing process or the powdered composition obtained in the drying process. Thus, the sulfonic acid compound can be attached to the surface of the lithium-containing composite oxide. Preferably, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the filter cake-like composition. Li compounds remain in the filter cake-like composition, and the residual Li compounds are dissolved in the water contained in the filter cake-like composition, so even when a sulfonic acid solution is added, a sulfonic acid compound containing Li is formed. The amount of the sulfonic acid compound or sulfonic acid added is preferably 0.1% to 1% by mass, and more preferably 0.3% to 0.8% by mass, relative to the mass of the lithium-containing composite oxide. The concentration of the sulfonic acid solution is, for example, 0.5% to 40% by mass.

[0080] A metal compound containing one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earths and Al, and a non-metal compound containing one or more non-metal elements selected from the group consisting of P and B can be attached to the surface of the lithium-containing composite oxide by adding the raw materials of the metal compound and the non-metal compound in any one of the synthesis process, after the synthesis process, in the cleaning process, after the cleaning process, in the drying process, after the drying process or in the addition process. As Sr raw materials, Sr(OH)2, Sr(OH)2·8H2O, SrO, SrCo3, SrSO4, Sr(NO3)2, SrCl2, SrAlO4, etc. can be listed. As Ca raw materials, Ca(OH)2, CaO, CaCO3, CaSO4, Ca(NO3)2, CaCl2, CaAlO4, etc. can be listed. Examples of Zr raw materials include Zr(OH)4, ZrO2, Zr(CO3)2, and Zr(SO4)2·4H2O. Examples of rare earth raw materials include oxides, hydroxides, and carbonates of rare earths. Examples of W raw materials include tungsten oxide (WO3), lithium tungstate (Li2WO4, Li4WO5, and Li6W2O9). It should be noted that, as a W raw material, a solution containing W may also be used. In addition, as an Al raw material, Al2O3, Al(OH)3, and Al2(SO4)3 may be used, and Al derived from a lithium-containing composite oxide may also be used. Examples of P raw materials include Li 3-x H x PO4 (0≤x≤3), etc. Examples of B raw materials include H3BO3, Li3BO3, and Li2B4O7.

[0081] The positive electrode mixture layer 32 may further contain Li2NiO2. Li2NiO2 contains a large amount of Li and functions as a Li filler for supplying Li ions to the negative electrode 12 during initial charge. Li2NiO2 may have a structure identified as a space group Immm.

[0082] When the mass of Li2NiO2 contained in the positive electrode mixture layer 32 is set to 100 parts by mass of the positive electrode active material contained in the positive electrode mixture layer 32, it can be 1 part by mass to 10 parts by mass. If the mass of Li2NiO2 contained in the positive electrode mixture layer 32 is 1 part by mass or more, a sufficient amount of Li ions can be supplied to the negative electrode. In addition, as described later, at least a part of Li2NiO2 changes to a compound represented by the general formula Li a Ni 2-a O2 (0 < a ≤ 0.5). When the mass of Li2NiO2 contained in the positive electrode mixture layer 32 exceeds 10 parts by mass, the contribution of the compound represented by the general formula Li a Ni 2-a O2 (0 < a ≤ 0.5) to the charge-discharge capacity is less than that of the lithium-containing composite oxide, so the battery capacity decreases.

[0083] After the first charge and discharge, a part or all of Li2NiO2 changes to a compound represented by, for example, the general formula Li a Ni 2-a O2 (0 < a ≤ 0.5). That is, the positive electrode mixture layer 32 may further contain a compound represented by the general formula Li a Ni 2-a O2 (0 < a ≤ 0.5). The compound represented by Li a Ni 2-a O2 (0 < a ≤ 0.5) releases and stores Li ions during charge and discharge and functions as a positive electrode active material.

[0084] When the mass of the compound represented by Li a Ni 2-a O2 (0 < a ≤ 0.5) contained in the positive electrode mixture layer 32 is set to 100 parts by mass of the positive electrode active material contained in the positive electrode mixture layer 32, it can be 0.1 part by mass to 5 parts by mass. If the mass of the compound represented by the general formula Li a Ni 2-a O2 (0 < a ≤ 0.5) contained in the positive electrode mixture layer 32 is 0.1 part by mass or more, a sufficient amount of Li ions can be supplied to the negative electrode. In addition, when the mass of the compound represented by the general formula Li a Ni 2-a O2 (0 < a ≤ 0.5) contained in the positive electrode mixture layer 32 exceeds 5 parts by mass, the contribution of the compound represented by the general formula Li a Ni 2-a O2 (0 < a ≤ 0.5) to the charge-discharge capacity is less than that of the lithium-containing composite oxide, so the battery capacity decreases.

[0085] [Negative electrode]

[0086] The negative electrode 12 has a negative electrode current collector 40 and a negative electrode mixture layer 42 formed on the surface of the negative electrode current collector 40. The negative electrode mixture layer 42 is preferably formed on both sides of the negative electrode current collector 40. The negative electrode current collector 40 can be a foil of a metal such as copper or a copper alloy that is stable within the potential range of the negative electrode 12, a thin film having such a metal disposed on its surface, or the like. The negative electrode mixture layer 42 can contain a negative electrode active material, a binder, and the like. The negative electrode 12 can be produced, for example, by coating a negative electrode paste containing a negative electrode active material, a binder, and the like on the surface of the negative electrode current collector 40, drying the coating film, and then performing rolling to form the negative electrode mixture layer 42 on both sides of the negative electrode current collector 40.

[0087] As the negative electrode active material contained in the negative electrode mixture layer 42, there is no particular limitation as long as it can reversibly occlude and release lithium ions, and carbon materials such as graphite are usually used. The graphite can be any of natural graphite such as flake graphite, massive graphite, and earthy graphite, artificial massive graphite, graphitized mesophase carbon microbeads, and other artificial graphite. In addition, as the negative electrode active material, metals alloyed with Li such as Si and Sn, metal compounds containing Si, Sn, etc., lithium titanium composite oxides, etc. can also be used. In addition, a negative electrode active material provided with a carbon coating film thereon can also be used. For example, a Si-containing compound represented by SiO x (0.5 ≤ x ≤ 1.6), or a Si-containing compound obtained by dispersing fine particles of Si in a lithium silicate phase represented by Li 2y SiO (2+y) (0 < y < 2) can be used in combination with graphite.

[0088] Similar to the case of the positive electrode 11, as the binder contained in the negative electrode mixture layer 42, a fluororesin, a polyimide resin, an acrylic resin, a polyolefin resin, PAN, etc. can also be used, and styrene-butadiene rubber (SBR) is preferably used. In addition, CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc. can be contained in the negative electrode mixture layer 42.

[0089] [Separator]

[0090] The separator 13 uses, for example, a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. As the material of the separator, polyolefins such as polyethylene and polypropylene, cellulose, etc. are preferred. The separator 13 can have a single-layer structure or a laminated structure. In addition, a resin layer having high heat resistance such as an aromatic polyamide resin or a filler layer containing a filler of an inorganic compound can be provided on the surface of the separator 13.

[0091] Examples

[0092] Hereinafter, the present disclosure will be further described by way of examples and comparative examples, but the present disclosure is not limited to the following examples.

[0093] [Preparation of positive electrode active material]

[0094] <Example 1>

[0095] The [Ni 0.90 Co 0.05 Al 0.05 The composite hydroxide represented by ](OH)2 was calcined at 500°C for 8 hours to obtain a composite oxide (Ni 0.90 Co 0.05 Al 0.05 Next, LiOH and the composite oxide were mixed so that the molar ratio of Li to the total amount of Ni, Co and Al was 1.03:1 to obtain a mixture. The mixture was heated under an oxygen flow with an oxygen concentration of 95% (per 10 cm 3 2mL / min and 5L / min flow rate per 1kg of mixture), calcined from room temperature to 650°C at a heating rate of 2.0°C / min, and then calcined from 650°C to 780°C at a heating rate of 0.5°C / min to obtain a lithium-containing composite oxide (synthesis process). Water is added to the lithium-containing composite oxide to make the slurry concentration 1500g / L, stirred for 15 minutes, and filtered to obtain a filter cake-like composition (cleaning process). Powdered lithium methanesulfonate is added to the filter cake-like composition (addition process). The amount of lithium methanesulfonate added is 0.1% by mass relative to the total mass of the lithium-containing composite oxide. After the addition process, a drying process is performed under vacuum atmosphere at 180°C for 2 hours to obtain the positive electrode active material of Example 1. It should be noted that the presence of lithium sulfonate on the surface of the positive electrode active material was confirmed by Fourier transform infrared spectroscopy (FT-IR). In addition, the value of YX of the positive electrode active material is 52μmol / g, and the value of X-(YX) is 43μmol / g. The average particle size (D50) of the positive electrode active material (lithium-containing composite oxide) was 11 μm.

[0096] [Production of positive electrode]

[0097] 92 parts by mass of the above positive electrode active material, 5 parts by mass of acetylene black (AB) and 3 parts by mass of polyvinylidene fluoride (PVDF) were mixed, and the mixture was further mixed with N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode slurry. Next, the slurry was mixed with a unit area weight of 250 g / m 2The positive electrode current collector formed of an aluminum foil having a thickness of 15 μm is coated with the coating film in a manner, and after the coating film is dried, the coating film is rolled using a calendering roller and cut into a predetermined electrode size that can be accommodated in an outer casing having an outer diameter of φ50 mm, thereby obtaining a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode current collector. It should be noted that an exposed portion where the surface of the positive electrode current collector is exposed is provided at the upper end of the positive electrode.

[0098] [Production of negative electrode]

[0099] Natural graphite is used as the negative electrode active material. The negative electrode active material, sodium carboxymethyl cellulose (CMC-Na) and styrene-butadiene rubber (SBR) are mixed in an aqueous solution at a solid content mass ratio of 100:1:1 to prepare a negative electrode slurry. The negative electrode slurry is applied to both sides of a negative electrode collector formed of copper foil, and after the coating film is dried, the coating film is rolled using a calendering roller and cut into a specified electrode size to obtain a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode collector. It should be noted that an exposed portion where the surface of the negative electrode collector is exposed is provided at the inner end of the negative electrode roll.

[0100] [Preparation of non-aqueous electrolyte]

[0101] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed at a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent at a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.

[0102] [Production of test battery cells]

[0103] like Figure 3 As shown in (a), 6 aluminum leads are sandwiched around the center of the electrode body, and 3 of them are arranged roughly in a row in the radial direction of the electrode body, and the aluminum leads are installed on the exposed portion of the above-mentioned positive electrode at roughly equal intervals. In addition, a nickel lead is installed on the exposed portion of the above-mentioned negative electrode. The positive electrode and the negative electrode are wound into a spiral shape through a separator made of polyolefin to produce a wound electrode body. The electrode body is accommodated in the interior of an outer body with an outer diameter of 50 mm, and after the above-mentioned non-aqueous electrolyte is injected, the opening at the upper end of the outer body is sealed with a sealing body to obtain a test battery cell.

[0104] [Evaluation of battery capacity per unit volume]

[0105] For the above test battery cell, under a temperature environment of 25°C, constant current charging was performed at 0.1C until the battery voltage reached 4.2V, constant voltage charging was performed at 4.2V until the current value reached 0.01C, and then constant current discharge was performed at 0.1C until the battery voltage reached 2.5V. Furthermore, for the test battery cell, under a temperature environment of 25°C, constant current charging was performed at 0.1C until the battery voltage reached 4.2V, constant voltage charging was performed at 4.2V until the current value reached 0.01C, and then constant current discharge was performed at 0.3C until the battery voltage reached 2.5V, and the discharge capacity at this time was taken as the initial discharge capacity. The initial discharge capacity was divided by the volume of the test battery cell to calculate the battery capacity per unit volume. It should be noted that in the above-mentioned charging and discharging, a 10-minute rest period was set when transitioning from charging to discharging.

[0106] [Evaluation of output characteristics]

[0107] For the above test battery cell, under a temperature environment of 25°C, constant current charging was performed at 0.2C until the battery voltage reached 4.2V, and constant voltage charging was performed at 4.2V until the current value reached 0.02C. After resting for 1 hour, constant current discharge was performed at 0.2C until the battery voltage reached 2.5V. Furthermore, for the above test battery cell, under a temperature environment of 25°C, constant current charging was performed at 0.2C until the battery voltage reached 4.3V, constant voltage charging was performed at 4.3V until the current value reached 0.02C, constant current discharge was performed at 0.5C until the battery voltage reached 2.5V, and after resting for 10 minutes, discharge was performed at 0.02C until the battery voltage reached 2.5V. The output characteristics were calculated from the discharge capacity at 0.5C and the discharge capacity at 0.02C by the following formula.

[0108] Output characteristic (%) = discharge capacity at 0.5C / (discharge capacity at 0.5C+discharge capacity at 0.02C)×100

[0109] <Example 2>

[0110] A test cell was prepared and evaluated in the same manner as in Example 1 except that the amount of lithium methanesulfonate added was 0.3 mass % relative to the total mass of the lithium-containing composite oxide in the adding step of preparing the positive electrode active material.

[0111] <Example 3>

[0112] A test cell was prepared and evaluated in the same manner as in Example 1 except that the amount of lithium methanesulfonate added was 0.5 mass % relative to the total mass of the lithium-containing composite oxide in the adding step of preparing the positive electrode active material.

[0113] <Example 4>

[0114] A test cell was prepared and evaluated in the same manner as in Example 1 except that the amount of lithium methanesulfonate added was 0.8 mass % relative to the total mass of the lithium-containing composite oxide in the adding step of preparing the positive electrode active material.

[0115] <Example 5>

[0116] A test cell was prepared and evaluated in the same manner as in Example 1 except that the amount of lithium methanesulfonate added was 1 mass % relative to the total mass of the lithium-containing composite oxide in the adding step of preparing the positive electrode active material.

[0117] <Example 6>

[0118] A test cell was prepared and evaluated in the same manner as in Example 1 except that powdery sodium methanesulfonate was added in place of lithium methanesulfonate in an amount of 0.5 mass % relative to the total mass of the lithium-containing composite oxide in the addition step of preparing the positive electrode active material.

[0119] <Example 7>

[0120] In the addition process of the preparation of the positive electrode active material, a methanesulfonic acid solution is added instead of the powdered lithium methanesulfonate, and the addition amount of methanesulfonic acid is 0.48% by mass relative to the total mass of the lithium-containing composite oxide. Otherwise, a test battery cell is prepared in the same manner as in Example 1 and evaluated. It should be noted that the concentration of the added methanesulfonic acid solution is 10% by mass, and the methanesulfonic acid solution is added in the manner described above with the addition amount of methanesulfonic acid. It should be noted that the presence of lithium sulfonate on the surface of the positive electrode active material was confirmed by Fourier transform infrared spectroscopy (FT-IR). In addition, the concentration of the methanesulfonic acid solution used below is 10% by mass.

[0121] <Comparative Example 1>

[0122] A test cell was produced and evaluated in the same manner as in Example 1 except that the addition step was not performed in the production of the positive electrode active material.

[0123] <Comparative Example 2>

[0124] A test cell was prepared and evaluated in the same manner as in Example 1 except that powdery lithium succinate was added instead of lithium methanesulfonate in an amount of 0.5 mass % relative to the total mass of the lithium-containing composite oxide in the addition step of preparing the positive electrode active material.

[0125] <Comparative Example 3>

[0126] A test cell was prepared and evaluated in the same manner as in Example 1 except that powdery lithium oxalate was added instead of lithium methanesulfonate in an amount of 0.5 mass % relative to the total mass of the lithium-containing composite oxide in the addition step of preparing the positive electrode active material.

[0127] <Comparative Example 4>

[0128] In the addition step of preparing the positive electrode active material, the addition amount of lithium methanesulfonate was set to 0.5 mass % relative to the total mass of the lithium-containing composite oxide. In the preparation of the test cell, the test cell was prepared and evaluated in the same manner as in Example 1 except that the number of aluminum leads was changed to 1.

[0129] <Comparative Example 5>

[0130] In the addition step of preparing the positive electrode active material, the amount of lithium methanesulfonate added was 0.5% by mass relative to the total mass of the lithium-containing composite oxide. In the preparation of the positive electrode, the weight per unit area was 190 g / m 2 A test battery cell was prepared and evaluated in the same manner as in Example 1 except that the positive electrode slurry was applied in the manner of .

[0131] <Comparative Example 6>

[0132] In the addition process for preparing the positive electrode active material, the addition amount of lithium methanesulfonate relative to the total mass of the lithium-containing composite oxide is set to 0.5 mass %. In the preparation of the positive electrode, the positive electrode is obtained by cutting into a specified electrode size that can be accommodated in an outer body with an outer diameter of φ20 mm. In the preparation of the test battery cell, the number of aluminum leads is changed to 1, and the electrode body is accommodated in an outer body with an outer diameter of φ20 mm. Except for this, the test battery cell is prepared in the same manner as Example 1 and evaluated.

[0133] <Comparative Example 7>

[0134] In the addition process of preparing the positive electrode active material, the addition amount of lithium methanesulfonate relative to the total mass of the lithium-containing composite oxide is set to 0.5 mass %. In the preparation of the positive electrode, the positive electrode is obtained by cutting into a specified electrode size accommodated in an outer body with an outer diameter of φ20 mm. In the preparation of the test battery cell, the electrode body is accommodated in an outer body with an outer diameter of φ20 mm. Except for this, the test battery cell is prepared and evaluated in the same manner as Example 1.

[0135] The battery capacity per unit volume and output characteristics of the test cells of Examples 1 to 7 and Comparative Examples 1 to 7 are shown in Table 1. In addition, Table 1 also shows the composition (ratio of each metal element to the total number of moles of metal elements other than Li) and average particle size (D50) of the lithium-containing composite oxide, the type, method and amount of the added sulfonic acid compound, the outer diameter of the battery, the unit area weight of the positive electrode mixture layer, and the current collection method and number of aluminum leads of the positive electrode. The battery capacity per unit volume shown in Table 1 is a relative evaluation based on Example 1. The case of 5% or more greater than Example 1 is set as ◎, the case of the same as Example 1 (less than ±5% relative to Example 1) is set as 0, the case of 5% or more less than Example 1 and less than 10% is set as △, the case of 10% or more less than Example 1 is set as ×, and the case of 20% or more less than Example 1 is set as ××. In addition, the output characteristics of the Examples and Comparative Examples shown in Table 1 are values ​​relatively expressed with the output characteristics of the test cell of Comparative Example 1 being set as 100.

[0136] [Table 1]

[0137]

[0138] <Example 8>

[0139] In the preparation of the positive electrode active material, the composition of the lithium-containing composite oxide is LiNi 0.80 Al 0.055 Mn 0.145 O2, the amount of lithium methanesulfonate added to the total mass of the lithium-containing composite oxide was 0.5 mass %, and in the preparation of the positive electrode, the weight per unit area was 325 g / m 2 The positive electrode slurry was applied in a manner and cut into a predetermined electrode size to be accommodated in an outer casing with an outer diameter of φ40 mm to obtain a positive electrode. In the production of a test battery cell, Figure 3 A test battery cell was prepared and evaluated in the same manner as in Example 1 except that three aluminum leads were arranged at substantially equal angles and the electrode assembly was housed in an outer casing having an outer diameter of 40 mm as shown in (b).

[0140] <Example 9>

[0141] A test cell was prepared and evaluated in the same manner as in Example 8 except that powdery sodium methanesulfonate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0142] <Example 10>

[0143] A test cell was prepared and evaluated in the same manner as in Example 8 except that a methanesulfonic acid solution was added in place of powdered lithium methanesulfonate in an amount of 0.48 mass % relative to the total mass of the lithium-containing composite oxide in the addition step of preparing the positive electrode active material.

[0144] <Comparative Example 8>

[0145] A test cell was produced and evaluated in the same manner as in Example 8 except that the addition step was not performed in the production of the positive electrode active material.

[0146] <Comparative Example 9>

[0147] A test cell was prepared and evaluated in the same manner as in Example 8 except that powdery lithium succinate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0148] <Comparative Example 10>

[0149] A test cell was prepared and evaluated in the same manner as in Example 8 except that powdery lithium oxalate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0150] The battery capacity per unit volume and output characteristics of the test battery cells of Examples 8 to 10 and Comparative Examples 9 and 10 are shown in Table 2. In addition, in Table 2, each condition is shown together in the same manner as in Table 1. The battery capacity per unit volume and output characteristics shown in Table 2 are the results of evaluation in the same manner as in Table 1, based on Comparative Example 8.

[0151] [Table 2]

[0152]

[0153] <Example 11>

[0154] In the preparation of the positive electrode active material, the composition of the lithium-containing composite oxide is LiNi 0.80 Co 0.045 Al 0.055 Mn 0.10 O2, the amount of lithium methanesulfonate added to the total mass of the lithium-containing composite oxide was 0.5 mass %, and in the preparation of the positive electrode, the weight per unit area was 275 g / m 2 The positive electrode slurry was applied in a manner and cut into a predetermined electrode size to be accommodated in an outer casing with an outer diameter of φ40 mm to obtain a positive electrode. In the production of a test battery cell, Figure 3 A test battery cell was prepared and evaluated in the same manner as in Example 1 except that three aluminum leads were arranged at substantially equal angles and the electrode assembly was housed in an outer casing having an outer diameter of 40 mm as shown in (b).

[0155] <Example 12>

[0156] A test cell was prepared and evaluated in the same manner as in Example 11 except that powdery sodium methanesulfonate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0157] <Example 13>

[0158] A test cell was prepared and evaluated in the same manner as in Example 11 except that a methanesulfonic acid solution was added in place of powdered lithium methanesulfonate in an amount of 0.48 mass % relative to the total mass of the lithium-containing composite oxide in the addition step of preparing the positive electrode active material.

[0159] <Comparative Example 11>

[0160] A test cell was produced and evaluated in the same manner as in Example 11 except that the addition step was not performed in the production of the positive electrode active material.

[0161] <Comparative Example 12>

[0162] A test cell was prepared and evaluated in the same manner as in Example 11 except that powdery lithium succinate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0163] <Comparative Example 13>

[0164] A test cell was prepared and evaluated in the same manner as in Example 11 except that powdery lithium oxalate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0165] The battery capacity per unit volume and output characteristics of the test battery cells of Examples 11 to 13 and Comparative Examples 12 and 13 are shown in Table 3. In addition, in Table 3, each condition is shown together in the same manner as in Table 1. The battery capacity per unit volume and output characteristics shown in Table 3 are the results of evaluation in the same manner as in Table 1, based on Comparative Example 11.

[0166] [Table 3]

[0167]

[0168] <Example 14>

[0169] In the preparation of the positive electrode active material, the composition of the lithium-containing composite oxide is LiNi 0.80 Co 0.10 Mn 0.10O2, the amount of lithium methanesulfonate added to the total mass of the lithium-containing composite oxide is 0.5 mass %. In the preparation of the positive electrode, the electrode is cut into a predetermined electrode size that can be accommodated in an outer body with an outer diameter of φ45 mm to obtain a positive electrode. In the preparation of the test battery cell, as shown in FIG. Figure 4 As shown, the positive electrode and the sealing body were connected by the positive electrode current collecting member, the negative electrode and the outer casing were connected by the negative electrode current collecting member, and the electrode body was housed in an outer casing with an outer diameter of 45 mm. A test battery cell was prepared and evaluated in the same manner as in Example 1.

[0170] <Example 15>

[0171] A test cell was prepared and evaluated in the same manner as in Example 14 except that powdery sodium methanesulfonate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0172] <Example 16>

[0173] A test cell was prepared and evaluated in the same manner as in Example 14 except that a methanesulfonic acid solution was added in place of powdered lithium methanesulfonate in an amount of 0.48 mass % relative to the total mass of the lithium-containing composite oxide in the addition step of preparing the positive electrode active material.

[0174] <Comparative Example 14>

[0175] A test cell was produced and evaluated in the same manner as in Example 14 except that the addition step was not performed in the production of the positive electrode active material.

[0176] <Comparative Example 15>

[0177] A test cell was prepared and evaluated in the same manner as in Example 14 except that powdery lithium succinate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0178] <Comparative Example 16>

[0179] A test cell was prepared and evaluated in the same manner as in Example 14 except that powdery lithium oxalate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0180] <Comparative Example 17>

[0181] In the production of the positive electrode, the weight per unit area is 190g / m 2 A test battery cell was prepared and evaluated in the same manner as in Example 14 except that the positive electrode slurry was applied in the manner of .

[0182] <Comparative Example 18>

[0183] In the preparation of the positive electrode active material, the adding process is not carried out. In the preparation of the positive electrode, the positive electrode is obtained by cutting into a specified electrode size that can be accommodated in an outer body with an outer diameter of φ20 mm. In the preparation of the test battery cell, the electrode body is accommodated in an outer body with an outer diameter of φ20 mm. Except for this, the test battery cell is prepared in the same manner as Example 14 and evaluated.

[0184] <Comparative Example 19>

[0185] In the production of the positive electrode, the positive electrode was obtained by cutting it into a specified electrode size that could be accommodated in an outer body with an outer diameter of φ20 mm. In the production of the test battery cell, the electrode body was accommodated in an outer body with an outer diameter of φ20 mm. Otherwise, the test battery cell was produced in the same manner as Example 14 and evaluated.

[0186] The battery capacity per unit volume and output characteristics of the test battery cells of Examples 14 to 16 and Comparative Examples 15 to 19 are shown in Table 4. In Table 4, the conditions are shown together in the same manner as in Table 1. The battery capacity per unit volume and output characteristics shown in Table 3 are the results of evaluation in the same manner as in Table 1, based on Comparative Example 14.

[0187] [Table 4]

[0188]

[0189] <Example 17>

[0190] In the preparation of the positive electrode active material, the composition of the lithium-containing composite oxide is LiNi 0.70 Al 0.05 Mn 0.25 O2, the amount of lithium methanesulfonate added to the total mass of the lithium-containing composite oxide was 0.5 mass %, and in the preparation of the positive electrode, the weight per unit area was 325 g / m 2 The positive electrode slurry was applied in a manner and cut into a specified electrode size that could be accommodated in an outer casing with an outer diameter of φ30 mm to obtain a positive electrode. In the preparation of the test battery cell, the number of aluminum leads was changed to 3 and the electrode body was accommodated in an outer casing with an outer diameter of φ30 mm. Otherwise, the test battery cell was prepared in the same manner as in Example 1 and evaluated.

[0191] <Example 18>

[0192] A test cell was prepared and evaluated in the same manner as in Example 17 except that powdery sodium methanesulfonate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0193] <Example 19>

[0194] A test cell was prepared and evaluated in the same manner as in Example 17 except that a methanesulfonic acid solution was added in place of powdered lithium methanesulfonate in an amount of 0.48 mass % relative to the total mass of the lithium-containing composite oxide in the addition step of preparing the positive electrode active material.

[0195] <Comparative Example 20>

[0196] A test cell was produced and evaluated in the same manner as in Example 17 except that the addition step was not performed in the production of the positive electrode active material.

[0197] <Comparative Example 21>

[0198] A test cell was prepared and evaluated in the same manner as in Example 17 except that powdery lithium succinate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0199] <Comparative Example 22>

[0200] A test cell was prepared and evaluated in the same manner as in Example 17 except that powdery lithium oxalate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0201] The battery capacity per unit volume and output characteristics of the test battery cells of Examples 17 to 19 and Comparative Examples 21 and 22 are shown in Table 5. In addition, in Table 5, each condition is shown together in the same manner as in Table 1. The battery capacity per unit volume and output characteristics shown in Table 5 are the results of evaluation in the same manner as in Table 1, based on Comparative Example 20.

[0202] [Table 5]

[0203]

[0204] <Example 20>

[0205] In the preparation of the positive electrode active material, the composition of the lithium-containing composite oxide is LiNi 0.80 Mn 0.20 O2, the amount of lithium methanesulfonate added to the total mass of the lithium-containing composite oxide was 0.5 mass %, and in the preparation of the positive electrode, the weight per unit area was 325 g / m 2 A test battery cell was prepared and evaluated in the same manner as in Example 1 except that the positive electrode slurry was applied in the manner of .

[0206] <Example 21>

[0207] A test cell was prepared and evaluated in the same manner as in Example 20 except that powdery sodium methanesulfonate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0208] <Example 22>

[0209] A test cell was prepared and evaluated in the same manner as in Example 20 except that a methanesulfonic acid solution was added in place of powdered lithium methanesulfonate in an amount of 0.48 mass % relative to the total mass of the lithium-containing composite oxide in the addition step of preparing the positive electrode active material.

[0210] <Comparative Example 23>

[0211] A test cell was produced and evaluated in the same manner as in Example 20 except that the addition step was not performed in the production of the positive electrode active material.

[0212] <Comparative Example 24>

[0213] A test cell was prepared and evaluated in the same manner as in Example 20 except that powdery lithium succinate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0214] <Comparative Example 25>

[0215] A test cell was prepared and evaluated in the same manner as in Example 20 except that powdery lithium oxalate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0216] The battery capacity per unit volume and output characteristics of the test battery cells of Examples 20 to 22 and Comparative Examples 24 and 25 are shown in Table 6. In addition, in Table 6, each condition is shown together in the same manner as in Table 1. The battery capacity per unit volume and output characteristics shown in Table 6 are the results of evaluation in the same manner as in Table 1, based on Comparative Example 23.

[0217] [Table 6]

[0218]

[0219] <Example 23>

[0220] In the preparation of positive electrode active material, the synthetic composition is LiNi 0.90 Co 0.05 Mn 0.05 O2, two kinds of particles with a volume-based median particle size (D50) of 3 μm and 15 μm, are mixed in a mass ratio of 50:50, and the resulting mixture is used as a lithium-containing composite oxide, and the addition amount of lithium methanesulfonate relative to the total mass of the lithium-containing composite oxide is 0.5 mass %. Except for this, a test battery cell is prepared and evaluated in the same manner as in Example 1.

[0221] <Example 24>

[0222] A test cell was prepared and evaluated in the same manner as in Example 23 except that powdery sodium methanesulfonate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0223] <Example 25>

[0224] A test cell was prepared and evaluated in the same manner as in Example 23 except that a methanesulfonic acid solution was added in place of powdered lithium methanesulfonate in an amount of 0.48 mass % relative to the total mass of the lithium-containing composite oxide in the addition step of preparing the positive electrode active material.

[0225] <Example 26>

[0226] In the preparation of the positive electrode active material, two kinds of particles of 3 μm and 12 μm were synthesized and mixed at a mass ratio of 50:50 to use the obtained mixture as the lithium-containing composite oxide. A test cell was prepared and evaluated in the same manner as in Example 23.

[0227] <Example 27>

[0228] In the preparation of the positive electrode active material, two kinds of particles of 5 μm and 15 μm were synthesized and mixed at a mass ratio of 50:50 to use the obtained mixture as the lithium-containing composite oxide. A test cell was prepared and evaluated in the same manner as in Example 23.

[0229] <Comparative Example 26>

[0230] A test cell was produced and evaluated in the same manner as in Example 23 except that the addition step was not performed in the production of the positive electrode active material.

[0231] <Comparative Example 27>

[0232] A test cell was prepared and evaluated in the same manner as in Example 23 except that powdery lithium succinate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0233] <Comparative Example 28>

[0234] A test cell was prepared and evaluated in the same manner as in Example 23 except that powdery lithium oxalate was added instead of lithium methanesulfonate in the adding step of preparing the positive electrode active material.

[0235] The battery capacity per unit volume and output characteristics of the test battery cells of Examples 23 to 27 and Comparative Examples 27 and 28 are shown in Table 6. In addition, in Table 7, each condition is shown together in the same manner as in Table 1. The battery capacity per unit volume and output characteristics shown in Table 7 are the results of evaluation in the same manner as in Table 1, based on Comparative Example 26.

[0236] [Table 7]

[0237]

[0238] In any of Tables 1 to 7, the battery capacity per unit volume of the Examples was improved and the output characteristics were improved in all cases compared to the Comparative Examples.

[0239] Description of Reference Numerals

[0240] 10 secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 outer body, 16 sealing body, 17, 18 insulating plate, 19 positive electrode lead, 20 negative electrode lead, 21 groove portion, 22 perforated metal plate, 23 lower valve core, 24 insulating member, 25 upper valve core, 26 cover, 26a opening, 27 gasket, 30 positive electrode collector, 32 positive electrode mixture layer, 34 positive electrode exposed portion, 40 negative electrode collector, 42 negative electrode mixture layer, 44 negative electrode exposed portion, 50 positive electrode collector member, 52 negative electrode collector member

Claims

1. A cylindrical secondary battery comprising: An electrode body formed by winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator interposed therebetween; An outer casing having an outer diameter of 25 mm or more and a bottomed cylindrical shape that accommodates the electrode body and is connected to the negative electrode; and The upper opening of the outer body is sealed and connected to the positive electrode by a sealing body, The positive electrode comprises a positive electrode current collector and a positive electrode mixture layer formed on a surface of the positive electrode current collector. The positive electrode mixture layer contains a positive electrode active material. The positive electrode active material includes a lithium-containing composite oxide having a layered rock salt structure and a sulfonic acid compound present on the surface of the lithium-containing composite oxide. The sulfonic acid compound is represented by the following general formula (I): The unit area weight of the positive electrode mixture layer is 250 g / m 2 above, In the electrode body, three or more positive electrode leads are led out, In the formula, A is a Group 1 element or a Group 2 element, R is a hydrocarbon group, and n is 1 or 2.

2. The cylindrical secondary battery according to claim 1, wherein The positive electrode leads are arranged substantially in a row in the radial direction on the upper surface of the electrode body.

3. The cylindrical secondary battery according to claim 1, wherein The positive electrode leads are arranged at substantially equal angles on the upper surface of the electrode body.

4. The cylindrical secondary battery according to any one of claims 1 to 3, wherein The positive electrode has a plurality of positive electrode current collector exposed portions at the upper end portion along the length direction where the positive electrode current collector is exposed. The positive electrode mixture layer exists between the positive electrode current collector exposed portions. The exposed portions of the positive electrode current collector are respectively connected to one of the positive electrode leads.

5. A cylindrical secondary battery comprising: An electrode body formed by winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator interposed therebetween; An outer casing having an outer diameter of 25 mm or more and a bottomed cylindrical shape that accommodates the electrode body and is connected to the negative electrode; and The upper opening of the outer body is sealed and connected to the positive electrode by a sealing body, The positive electrode comprises a positive electrode current collector and a positive electrode mixture layer formed on a surface of the positive electrode current collector. The positive electrode mixture layer contains a positive electrode active material. The positive electrode active material includes a lithium-containing composite oxide having a layered rock salt structure and a sulfonic acid compound present on the surface of the lithium-containing composite oxide. The sulfonic acid compound is represented by the following general formula (I): The unit area weight of the positive electrode mixture layer is 250 g / m 2 above, The positive electrode protruding upward from the negative electrode and the separator in the electrode body is connected to a positive electrode current collecting member, and the positive electrode current collecting member is connected to the sealing body via a positive electrode lead. In the formula, A is a Group 1 element or a Group 2 element, R is a hydrocarbon group, and n is 1 or 2.

6. The cylindrical secondary battery according to any one of claims 1 to 5, wherein The A is a Group 1 element.

7. The cylindrical secondary battery according to any one of claims 1 to 5, wherein The A is Li.

8. The cylindrical secondary battery according to any one of claims 1 to 7, wherein The R is an alkyl group.

9. The cylindrical secondary battery according to any one of claims 1 to 7, wherein The R is a methyl group.

10. The cylindrical secondary battery according to any one of claims 1 to 9, wherein The positive electrode active material is a mixture of particles having a volume-based median particle size of 10 μm or more and particles having a volume-based median particle size of 6 μm or less.

11. The cylindrical secondary battery according to any one of claims 1 to 10, wherein The amount of the sulfonic acid compound present on the surface of the lithium-containing composite oxide is 0.1% by mass to 1% by mass relative to the mass of the lithium-containing composite oxide.

12. The cylindrical secondary battery according to any one of claims 1 to 11, wherein In the infrared absorption spectrum, at 1238cm -1 、1175cm -1 、1065cm -1 、785cm -1 At least one of the nearby regions has an absorption peak.