Novel composite material for anode electrode
The energy density, cost and performance challenges of the anode electrode are solved by using composite materials of silicon-based nanostructures attached to carbon-based substrates in the anode electrodes of lithium-ion batteries, achieving high efficiency Anode electrode preparation, suitable for large-scale production.
Patent Information
- Application Number
- CN202280092336.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-12-22
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, when manufacturing silicon-based anode electrodes for lithium-ion batteries, it is difficult to achieve high energy density, low cost and good mechanical and electrical properties. At the same time, there is a problem of excessive use of adhesives or uneven dispersion, which affects the anode layer. Uniformity and adhesion.
A composite material with multiple silicon-based nanostructures attached to a carbon-based substrate and a monomer unit polymer formed of styrene and allyl alcohol is used to form a composite material by mixing and drying to prepare an improved processing performance and uniformity. Highly capable anode electrode.
Achieved a low inactive material to active material ratio, improved uniformity and silicon distribution of the anode layer, promoted the prelithiation process, was suitable for large-scale production, and showed good capacity retention and Initial Coulomb efficiency.
Smart Images

Figure CN118891747A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of U.S. Provisional Application No. 63 / 293,442, filed on December 23, 2021, under 35 USC ξ119(e), the entire contents of which are incorporated herein by reference. Technical Field
[0003] The technology described herein relates to a composite material for a battery anode electrode, and an anode electrode and a battery (e.g., a lithium-ion battery) comprising the composite material, and a method of making the same. More particularly, the technology described herein relates to a composite material comprising a carbon-based substrate attached to a
[0004] Composite materials of silicon-based nanostructures (such as carbon-based powders). Background Art
[0005] A great deal of effort has been devoted to reducing the cost and improving the performance of energy storage devices, and the goal of widespread adoption of electric vehicles (EVs) has greatly motivated this effort. Many have explored strategies ranging from adopting new anode active materials to improve performance (e.g., silicon-carbon anode materials) to applying new cell manufacturing processes to reduce costs (e.g., dry electrode coating or pre-lithiation), but the results have been uncertain, driven primarily by the challenging trade-offs of combining new materials with large-scale production methods while reducing costs.
[0006] The manufacture of high energy density anode electrodes for EV cell batteries requires mixing active materials such as silicon and graphite with inactive materials such as binders and conductive additives. Since inactive materials do not contribute to the reversible storage of lithium and electrons in the anode, there is a trend to reduce the weight ratio of inactive materials to active materials to increase the energy density of EV cell batteries while reducing their overall weight. In addition, incorporating larger amounts of silicon, which has a higher specific capacity and a slightly higher voltage platform than graphite, into the anode generally enables thinner anode electrodes that can be charged faster. However, the volume change associated with the alloying of lithium ions and silicon (up to 300%) is much larger than the volume change associated with the embedding of lithium ions into graphite (typically less than 10%). This poses a significant challenge to selecting a polymer binder that can maintain the mechanical and electrical integrity of the anode layer and its adhesion to the current collector foil while safely achieving higher silicon anode contents and reducing manufacturing costs.
[0007] Some of the main binders used in the aqueous electrode manufacturing of silicon-based anode electrodes are carboxymethyl cellulose (CMC) and polyacrylic acid (PAA). These binders are soluble in water and exhibit high mechanical rigidity and stiffness. However, CMC and PAA as the only binders require higher binder content (e.g., about 8 wt%) in the silicon-graphite anode electrode layer, which can increase anode rigidity and stiffness and may have a negative impact on the electrode winding process and other key production processes.
[0008] Another strategy currently being adopted is to use styrene butadiene rubber (SBR) as a binder to improve flexibility, bond strength, adhesion, and cohesion. However, SBR is difficult to disperse evenly in the electrode slurry, which may have a negative impact on the electrode performance.
[0009] Elsewhere, efforts to advance silicon as a viable anode material for lithium-ion cells generally involve one of the following approaches: (a) mixing small amounts of silicon oxide additives (e.g., SiOx, where x approaches a value of 1) with graphite particles, and / or (b) embedding silicon particles within a carbon shell comprising amorphous carbon, hard carbon, and / or pyrolyzed polymers. In both approaches, the anode is formed by mixing the anode active material with a polymer binder to provide a slurry, which is then used to form an anode layer on a copper current collector foil. However, these approaches have several disadvantages. For example, strategies according to approach (a) are technically complex and relatively expensive, meaning that they are limited to formulations containing only small amounts of silicon, resulting in anodes that exhibit first cycle efficiencies of less than 90%, which require expensive cathode materials to compensate. Strategies according to approach (b) require silicon precursors to form the silicon particles and carbon precursors to form the shell. The cost of producing these carbon shells is high, as is the low conversion rate of the silicon precursors to reversible silicon capacity in the anode. Furthermore, the new materials and particles involved in the strategies according to both approaches can significantly affect the rheology of the anode slurry, which in turn can compromise the uniformity of the anode coating, the uniformity of the silicon distribution within the anode layer, and the adhesion of the anode layer on the current collector foil. Summary of the invention
[0010] Aspects of the present disclosure relate to improved silicon-based anode materials that: have a low ratio of inactive material to active material; provide improved processing performance; have improved slurry uniformity and silicon distribution in the anode layer; can facilitate the pre-lithiation process; and / or are suitable for large-scale production at a competitive cost using current and future unit cell production equipment.
[0011] According to a first aspect, a composite material is provided, comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol.
[0012] According to a second aspect, there is provided a method for preparing a composite material, the method comprising: mixing a plurality of silicon-based nanostructures attached to a carbon-based substrate with a solution of a polymer to form a mixture, the polymer comprising monomer units formed of styrene and allyl alcohol; and drying the mixture.
[0013] According to a third aspect, there is provided a composite material obtained, directly obtained or obtainable by the method of the second aspect.
[0014] According to a fourth aspect, there is provided an anode electrode comprising a first anode layer comprising a binder and a composite material as described herein.
[0015] According to a fifth aspect, there is provided a method for preparing an anode electrode, the method comprising: mixing a composite material as described herein and a binder; applying an anode layer of the mixture resulting from the mixing.
[0016] According to a sixth aspect, there is provided an anode electrode obtained, directly obtained or obtainable by the method of the fifth aspect.
[0017] According to a seventh aspect, there is provided a battery comprising the composite material and / or the anode electrode as described herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to describe the manner in which the above disclosure and its advantages and features can be obtained, a more specific description of the above principles will be presented by reference to specific examples shown in the accompanying drawings. These drawings depict only exemplary aspects of the present disclosure and therefore should not be considered to limit its scope. These principles are described and explained with additional specificity and detail through the use of the following drawings:
[0019] Figure 1A is a SEM (scanning electron microscope) photograph showing silicon-based nanowires attached to the surface of uncoated natural graphite particles used in composite materials of various aspects of the present invention.
[0020] Figure 1B and 1C 1 is a SEM photograph (1C is an enlarged view of a rectangular portion of 1B) showing a cross section of an uncoated natural graphite particle used for a composite material of various aspects of the present invention. The particle was cut using a FIB (focused ion beam) cutting technique to reveal the inner wall surface of the pores in the graphite particle and the silicon-based nanowires attached thereto.
[0021] Figure 2A is a flow chart illustrating a method for preparing a composite material according to aspects of the present invention.
[0022] Figure 2B is a flow chart illustrating a method for preparing a composite material according to aspects of the present invention.
[0023] Figure 3 is a flow chart illustrating a method for preparing an anode electrode according to aspects of the present invention.
[0024] Figure 4 Graphs showing the performance of a half cell according to aspects of the present invention are shown.
[0025] Figure 5 Graphs showing the cycling performance of an anode in a full cell according to aspects of the present invention are shown.
[0026] Figure 6 A curve showing a half-cell according to aspects of the present invention is shown. Figure 6 The A-6C is Figure 6 Detailed view of the portion of the curve shown in .
[0027] Fig. 7A and 7B TEM images of silicon nanowires and graphite particles coated by a uniform PSAA carbonized layer according to aspects of the present invention are shown.
[0028] Figure 8 The cycling performance between a battery cell of a baseline battery and a battery cell according to aspects of the present invention using a first cycling protocol is shown.
[0029] Fig. 9 Cycling performance between cells of a baseline battery using a second cycling regimen different from the first cycling regimen and cells of a battery according to aspects of the present invention is shown.
[0030] Fig.10 The specifications, first charge capacity, and first discharge capacity of four groups of electrochemical anode material composites containing different combinations of SiNW-carbon and PSAA are shown.
[0031] Fig.11 The specific discharge capacity over hundreds of cycles is shown for two types of electrochemical cells, the first type comprising anode composites prepared using a single surface treatment and the second type comprising anode composites prepared using dual surface treatments.
[0032] Fig.12 The % capacity retention over hundreds of cycles is shown for two types of electrochemical cells, the first type comprising anode composites prepared using a single surface treatment and the second type comprising anode composites prepared using dual surface treatments. DETAILED DESCRIPTION
[0033] definition
[0034] " nanostructure " used herein is a structure with at least one region or characteristic size, and the region or characteristic size have less than about 500nm, for example, less than about 200nm, less than about 100nm, less than about 50nm or even less than the size of about 20nm.Usually, this region or characteristic size will be along the minimum axis of this structure.The example of this type of structure includes nanowire, nanorod, nanotube, nanofiber, nanoparticle etc.Nanostructure can be, for example, substantially crystalline, substantially monocrystalline, polycrystalline, amorphous or its combination.In certain embodiments, each dimension in the three-dimensional of this nanostructure has less than about 500nm, for example, less than about 200nm, less than about 100nm, less than about 50nm or even less than the size of about 20nm.
[0035] As used herein, "aspect ratio" is the length of a first axis of a nanostructure divided by the average of the lengths of a second axis and a third axis of the nanostructure, where the second axis and the third axis are the two axes whose lengths are most nearly equal to each other. For example, the aspect ratio of a perfect rod would be the length of its major axis divided by the diameter of a cross section perpendicular (normal) to the major axis.
[0036] As used herein, the "diameter" of a nanostructure refers to the diameter of a cross-section perpendicular to a first axis of the nanostructure, where the first axis has the largest length difference relative to a second axis and a third axis (the second axis and the third axis being the two axes whose lengths are most nearly equal to each other). The first axis is not necessarily the longest axis of the nanostructure; for example, for a disk-shaped nanostructure, the cross-section will be a substantially circular cross-section orthogonal to the short longitudinal axis of the disk. When the cross-section is not circular, the diameter is the average of the major axis and the minor axis of the cross-section. For elongated or high aspect ratio nanostructures, such as nanowires, the diameter is measured across a cross-section perpendicular to the longest axis of the nanowire. For spherical nanostructures, the diameter is measured from one side to the other through the center of the sphere.
[0037] As used herein, the term "crystalline" or "substantially crystalline" when used with respect to a nanostructure refers to the fact that the nanostructure generally exhibits long-range order in one or more dimensions of the structure. It will be understood by those skilled in the art that the term "long-range order" will depend on the absolute size of the particular nanostructure, since the order of a single crystal cannot extend beyond the boundaries of the crystal. In such cases, "long-range order" will mean a substantial order in at least most dimensions of the nanostructure. In some cases, the nanostructure may be provided with an oxide or other coating, or may consist of a core and at least one shell. In such cases, it will be understood that the oxide, shell or other coating need not exhibit such order (e.g., it may be amorphous, polycrystalline, etc.). In such cases, the phrase "crystalline", "substantially crystalline", "substantially single crystal" or "single crystal" refers to the central core of the nanostructure (excluding any coating or shell). As used herein, the term "crystalline" or "substantially crystalline" is also intended to encompass structures containing various defects, stacking faults, atomic substitutions, etc., as long as the structure exhibits substantial long-range order (e.g., ordered over at least about 80% of the length of at least one axis of the nanostructure or its core). Furthermore, it should be understood that the interface between the core and the exterior of the nanostructure or between the core and an adjacent shell or between a shell and a second adjacent shell may contain non-crystalline regions and may even be amorphous. This does not prevent the nanostructure from being crystalline or substantially crystalline as defined herein.
[0038] As used herein, the term "single crystal" when used with respect to a nanostructure means that the nanostructure is substantially crystalline and comprises substantially a single crystal. When used with respect to a nanostructure heterostructure comprising a core and one or more shells, "single crystal" means that the core is substantially crystalline and comprises substantially a single crystal.
[0039] " nanoparticle " used herein is wherein each dimension (for example each dimension in the three-dimensional of this nanostructure) is less than about 500nm, for example less than about 200nm, less than about 100nm, less than about 50nm or even less than about 20nm nanostructure.Nanoparticle can have any shape, and comprises for example nanocrystal, substantially spherical particle (having the aspect ratio of about 0.8 to about 1.2) and irregular shape particle.Nanoparticle optionally has the aspect ratio of less than about 1.5.Nanoparticle can be amorphous, crystalline, monocrystalline, partially crystalline, polycrystalline etc.Nanoparticle can be substantially uniform in material property, or can be inhomogeneous (for example heterogeneous structure) in certain embodiments.Nanoparticle can be made of one or more materials of substantially any convenience (convenient), for example, this nanoparticle can comprise " pure " material, substantially pure material, doped material etc.
[0040] A "nanowire" is a nanostructure whose major axis is longer than the other two major axes. Thus, a nanowire has an aspect ratio greater than 1; the nanowires of the present invention typically have an aspect ratio greater than about 1.5 or greater than about 2. Short nanowires (sometimes referred to as nanorods) typically have an aspect ratio of about 1.5 to about 10. Longer nanowires have an aspect ratio greater than about 10, greater than about 20, greater than about 50, or greater than about 100, or even greater than about 10,000. The diameter of the nanowire is typically less than about 500nm, preferably less than about 200nm, more preferably less than about 150nm, most preferably less than about 100nm, about 50nm, or about 25nm, or even less than about 10nm or about 5nm. The nanowire may be substantially uniform in material properties, or in certain embodiments may be non-uniform (e.g., nanowire heterostructures). The nanowire may be made of substantially any conventional material or materials, the nanowire may comprise "pure" materials, substantially pure materials, doped materials, etc., and may include insulators, conductors, and semiconductors. Nanowires are generally substantially crystalline and / or substantially monocrystalline, but may be, for example, polycrystalline or amorphous. In some cases, nanowires may be provided with oxides or other coatings, or may include a core and at least one shell. In such cases, it should be understood that oxides, shells or other coatings do not need to exhibit such order (e.g., they may be amorphous, polycrystalline, etc.). Nanowires may have a variable diameter or may have a substantially uniform diameter, i.e., a diameter that exhibits a variation of less than about 20% (e.g., less than about 10%, less than about 5%, or less than about 1%) in a region with maximum variability and in a linear dimension of at least 5 nm (e.g., at least 10 nm, at least 20 nm, or at least 50 nm). Typically, the diameter is evaluated away from the end of the nanowire (e.g., at the center 20%, 40%, 50%, or 80% of the nanowire). Nanowires may be straight over the entire length of their major axis or a portion thereof, or may be, for example, curved or bent. In certain embodiments, nanowires or a portion thereof may exhibit two-dimensional or three-dimensional quantum confinement. In some embodiments, nanowires may specifically exclude carbon nanotubes, and in certain embodiments exclude "whiskers" or "nanowhiskers," particularly whiskers having a diameter greater than 100 nm, or greater than about 200 nm.
[0041] As used herein, "silicon-based" when used with respect to a nanostructure means that the nanostructure comprises at least about 50% silicon by mass. Suitably, the silicon-based nanostructure comprises at least about 60% silicon, at least about 70% silicon, at least about 80% silicon, at least about 90% silicon, at least about 95% silicon, or about 100% silicon, including 100% silicon, by mass.
[0042] " Carbon-based substrate " used herein refers to a porous substrate comprising at least about 50% carbon by mass. Suitably, the carbon-based substrate comprises at least about 60% carbon, at least about 70% carbon, at least about 80% carbon, at least about 90% carbon, at least about 95% carbon or about 100% carbon by mass, including 100% carbon. The carbon-based substrate can be in the form of sheet or separate particles and cross-linked structures. The carbon-based substrate particularly excludes metallic materials, such as steel, including stainless steel. Typically, the carbon-based substrate is graphite powder (such as artificial graphite powder or natural graphite powder). Graphite powder can be coated (such as carbon coated) or uncoated. The carbon-based substrate particles can have substantially any desired shape, such as spherical or substantially spherical, elongated, oval / elliptical, plate-like (such as plate, thin slice or sheet) and / or similar shapes. Similarly, the carbon-based substrate (such as graphite particles) can have substantially any size and porosity. Typically, the carbon-based substrate (eg, graphite particles) has a D of about 0.5 μm to about 50 μm. 50 It should be understood that D 50 refers to the median particle size corresponding to the 50th percentile of the cumulative undersize distribution. The measurement method used is laser diffraction according to ISO Standard No. 13320. Thus, when, for example, the carbon-based substrate is graphite powder, it is understood that a D of 0.5 μm to 50 μm 50 It means that a sample of graphite powder has a D of not less than 0.5 μm and not more than 50 μm when measured by laser diffraction according to ISO#13320. 50 This measurement is commonly used in the specifications of commercial carbon-based substrates (e.g., graphite powder) used by lithium-ion battery manufacturers and is therefore well known to those skilled in the art. The carbon-based substrate may alternatively have a D of, for example, about 0.5 μm to about 2 μm, about 2 μm to about 10 μm, about 2 μm to about 5 μm, about 5 μm to about 50 μm, about 10 μm to about 30 μm, about 10 μm to about 20 μm, about 15 μm to about 25 μm, about 15 μm to about 20 μm, or about 20 μm. 50 . The graphite powder (e.g., coated or uncoated natural graphite powder or artificial graphite powder) may comprise particles comprising a plurality of pores disposed therein and a surface area comprising the inner wall surfaces of the pores defining the plurality of pores. As is well known to those skilled in the art, the porosity of graphite particles can be estimated by various types of measurements, such as: gas adsorption surface area according to the "BET" or "SSA" standards; direct FIB SEM imaging; mercury porosimetry. The standard definition of porosity found in ASTM Standard C709 (which has definitions of terms relating to manufactured carbon and graphite) is "the percentage of the total volume of the material occupied by pores." When calculating the apparent density of a material, the pore volume is included in the calculation. This results in a value of 2.26 g / cm 3When compared to the theoretical density of graphite, the typical apparent density of synthetic graphite is 1.6 g / cm 3 Up to 1.90g / cm 3 (The specific volume of graphite is the inverse of the specific density.) The difference between the apparent density (weight of the particle divided by the volume of the particle including the pore volume) and the theoretical density (weight per unit volume in the absence of pores) is a measure of the total pore volume per unit mass. Thus, porosity can be defined as the ratio of the pore volume per unit mass divided by the sum of the specific volume and the pore volume per unit mass. Typical natural graphite for anode applications has an apparent (bulk) density of 1.2 g / cm2, while natural graphite porosity falls within the range of about 5%-50%. 3 -2.14g / cm 3 within the range.
[0043] As used herein, the term "about" refers to a value of a given amount that varies by + / - 10% of that value, or optionally by + / - 5% of that value, or in some embodiments by + / - 1% of that value.
[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those of ordinary skill in the art to which the present invention belongs. The following definitions supplement those in the art and are for this application, and should not be attributed to any relevant or irrelevant situation, such as any jointly owned patent or application. Although any methods and materials similar or equivalent to those described herein can be used in practice, certain materials and methods are described herein. Therefore, the terms used herein are only used for the purpose of describing specific embodiments, and are not intended to be limiting.
[0045] Throughout the description and claims of this specification, when the term "comprise" (or "comprises" or "comprising") is used herein to describe subject matter, the same subject matter described using the terms "consist of" (or "consists of" or "consisting of") or "consist essentially of" (or "consists essentially of" or "consisting essentially of") is also contemplated.
[0046] Throughout the description and claims of this specification, the singular encompasses the plural, unless the context otherwise requires. In particular, where the indefinite article is used, the specification is to be understood as contemplating plurality as well as singularity, unless the context otherwise requires.
[0047] Features described in conjunction with a particular aspect, embodiment or example (and their relative applicability) are to be understood to be applicable to any other aspect, embodiment or example described herein, unless incompatible therewith. All features disclosed in this specification (including any accompanying claims, abstract and drawings) and / or all steps of any method or process so disclosed may be combined in any combination, except combinations in which at least some of such features and / or steps are mutually exclusive. The invention is not limited to the details of any particular embodiment described herein. The invention extends to any novel one or any novel combination of the features disclosed in this specification (including any accompanying claims, abstract and drawings), or to any novel one or any novel combination of the steps of any method or process so disclosed.
[0048] Unless otherwise specified, when the amount or concentration of a particular component of a given product is specified as a weight percentage (mass %, wt% or %w / w), the weight percentage refers to the percentage of the component by weight relative to the total weight of the product as a whole. It will be appreciated by those skilled in the art that the sum of the weight percentages of all components of a product will add up to 100 weight %. However, when all components are not listed (e.g., when a product is referred to as "comprising" one or more particular components), the weight percentage surplus can be optionally supplemented to 100 weight % by unspecified ingredients.
[0049] When a range is provided, the value can be any value or range of values within the range, unless otherwise stated.
[0050] Composite materials and their preparation
[0051] In one aspect, an embodiment provides a composite material comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol.
[0052] As a result of painstaking research, the inventors surprisingly discovered that applying a polymerization comprising a monomer portion formed by styrene and allyl alcohol to a silicon-based nanostructure attached to a carbon-based substrate greatly enhances the dispersibility and bonding capabilities of the resulting composite material, allowing the composite material to be directly and inexpensively processed with other active and inactive materials (e.g., adhesives, conductive additives, etc.) to form a highly uniform anode material. In particular, the inventors have determined that the properties of the polymers disposed on the silicon-based nanostructure and the carbon-based substrate produce favorable bonding interactions with those materials that are typically used as adhesives in the preparation of battery anode materials. This improved interaction between the components of the anode slurry allows the use of wet and dry processing techniques to prepare anode materials with a high ratio of active material to inactive material, and also allows for longer cycle life, i.e., the ability to provide a higher anode reversible capacity in more charge / discharge cycles, even when charging or discharging includes higher currents. In addition, the polymer comprising a monomer portion formed by styrene and allyl alcohol is able to form a more stable interface between the silicon-based nanostructure and the semi-solid / solid electrolyte, demonstrating an improved ability to withstand volume changes that occur in the silicon-based nanostructure during charge / discharge cycles. For the reasons stated above, batteries incorporating the composite materials described herein provide improved electronic properties (eg, specific capacity and / or initial coulombic efficiency (ICE) and / or capacity retention over many charge / discharge cycles, even at high C-rates).
[0053] The composite material is suitable for an anode electrode, in particular an anode electrode of a lithium ion battery.
[0054] With respect to the polymers disposed on the plurality of silicon-based nanostructures and the carbon-based substrate, it is understood that a monomer unit formed from styrene refers to a repeating unit whose repetition will produce a polystyrene chain (regardless of the end groups). Similarly, it is understood that a monomer unit formed from allyl alcohol (i.e., prop-2-en-1-ol) refers to a repeating unit whose repetition will produce a poly(allyl alcohol) chain (regardless of the end groups). The monomer unit formed from styrene and allyl alcohol is depicted below:
[0055]
[0056] Without wishing to be bound by theory, the inventors hypothesize that the structure and / or properties of the polymer comprising monomer units formed by styrene and allyl alcohol promote improved interactions with other anode slurry components, which in turn imparts improved dispersibility to the silicon-based nanostructures attached to the carbon-based substrate, resulting in a more uniform anode material. In particular, the functional groups / structural motifs present on the polymer are free to participate in intermolecular interactions with the functional groups / structural motifs that may be present on the binder contained in the slurry. For example, the hydroxyl groups of the polymer may participate in hydrogen bonding with the groups present on the binder (e.g., the hydroxyl groups present on the carboxymethyl cellulose) and / or the phenyl groups of the polymer may participate in π-π stacking with the groups present on the binder (e.g., the phenyl groups present on the styrene-butadiene rubber). When the anode material is prepared by dry coating techniques, for example, a solid mixture of silicon-based nanostructures attached to a carbon-based substrate is dispersed in a thermoplastic polymer binder (e.g., polytetrafluoroethylene) under solvent-free conditions and then laminated to a current collector as a film, the improved dispersibility of the silicon-based nanostructures attached to the carbon-based substrate is particularly important.
[0057] The polymer comprising monomer units formed from styrene and allyl alcohol can form a coating (eg, a partial or complete coating) on the silicon-based nanostructures and the carbon-based substrate. Suitably, the polymer is disposed (eg, coated) on the silicon-based nanostructures and the carbon-based substrate in a substantially uniform manner.
[0058] The polymer comprising monomer units formed from styrene and allyl alcohol suitably has a softening point below 200°C. Such polymers generally show better compatibility with binders used in anode slurries. More suitably, the polymer has a softening point of 50°C to 100°C. Most suitably, the polymer has a softening point of 60°C to 90°C.
[0059] A polymer comprising monomer units formed from styrene and allyl alcohol may have a molecular weight of 800 gmol -1 Up to 5000 g mol -1 The molecular weight (M) was determined by gas permeation chromatography (GPC). n ). Suitably, the polymer has a 1000 g mol -1 Up to 3000 g mol -1 The molecular weight (M n ). Most suitably, the polymer has 1200 g mol -1 Up to 2000 g mol -1 The molecular weight (M n ).
[0060] The polymer comprising the monomer unit formed by styrene and allyl alcohol is suitably soluble in alcoholic solvents, particularly ethanol. The polymer showing these solubility characteristics promotes the drying of the resulting composite material. Compared with using water-soluble polymers, the solution of a polymer soluble in, for example, ethanol can be directly dried at a lower temperature without leaving any solvent residue (the solvent residue can have a negative impact on battery performance) on the silicon-based nanostructure. More suitably, the polymer is insoluble in water. Polymer can be insoluble in carbonate-based electrolytes, such as those used to prepare lithium-ion batteries. Suitably, ethanol can be recovered and reused in the drying process, which results in lower cost and waste.
[0061] The polymer comprising the monomeric unit formed by styrene and allyl alcohol can include at least 20 mol % (e.g., 20 mol % to 50 mol %) of the monomeric unit formed by allyl alcohol. Suitably, the polymer comprises 25 mol % to 45 mol % of the monomeric unit formed by allyl alcohol. Most suitably, the polymer comprises 30 mol % to 36 mol % of the monomeric unit formed by allyl alcohol. In addition, the polymer can include at least 50 mol % of the monomeric unit formed by styrene.
[0062] In a particular embodiment, the polymer comprising monomer units formed from styrene and allyl alcohol is poly(styrene-co-allyl alcohol) (PSAA). The polymer may have any of the above properties. PSAA is a cheap, environmentally friendly and non-toxic polymer that is readily soluble in ethanol.
[0063] The composite material may have 0.1 wt% to 10 wt% of a polymer comprising monomer units formed from styrene and allyl alcohol (eg PSAA). Suitably, the composite material comprises 0.5 wt% to 5 wt% (eg 0.7 wt% to 2 wt%) of the polymer.
[0064] Silicon-based nanostructures are attached to carbon-based substrates so that they are electrically connected to each other. Typically, silicon-based nanostructures are attached to the outer surface of carbon-based substrates. However, when the carbon-based substrate is porous (e.g., porous graphite powder), silicon-based nanostructures can be attached to the inner surface (those surfaces that define pores) and the outer surface of the carbon-based substrate. This can be achieved by many techniques known in the art. For example, silicon-based nanostructures (e.g., silicon nanowires) can be grown from catalyst particles deposited on carbon-based substrates (e.g., graphite particles) via gas-liquid-solid (VLS) or gas-solid-solid (VSS) chemical vapor deposition techniques. Alternatively, silicon-based nanostructures (e.g., silicon nanowires) can be electrochemically deposited on carbon-based substrates (e.g., graphite particles). With reference to U.S. Patents 10,243,207 or 9,812,699, which are incorporated herein by reference in their entirety. In some embodiments, the silicon-based nanostructures are mechanically attached to carbon-based substrates. In some embodiments, the silicon-based nanostructures are attached to the carbon-based substrate so that they are in electrical communication with each other without the need to use a conductive polymer to achieve mechanical and electrical connection. In some embodiments, the electrical communication is via a low electrical impedance path during cycling.
[0065] In a particular embodiment, the silicon-based nanostructure is suitably a carbon-based nanowire, such as a silicon nanowire. The dimensions of the silicon-based nanostructure (e.g., silicon nanowire) are described above. Suitably, the silicon-based nanowire (e.g., silicon nanowire) has a diameter of 10 nm to 200 nm. The silicon-based nanostructure may comprise a single crystal core and a shell, wherein the shell comprises amorphous silicon, polycrystalline silicon, or a combination thereof.
[0066] The carbon-based substrate is provided as a plurality of particles, wherein silicon-based nanostructures are attached to those particles (e.g., attached to the surface of those particles). Some particles may have more silicon-based nanostructures attached thereto than other particles. The carbon-based substrate may be selected from graphite powder (e.g., artificial graphite powder or natural graphite powder), which may be coated (e.g., carbon-coated) or uncoated, mesophase carbon microbead powder (also referred to as "MCMB" in industrial applications), or a combination thereof. Most suitably, the carbon-based substrate is graphite powder. The dimensions of the carbon-based substrate are described above. Suitably, the carbon-based substrate (e.g., graphite powder) has a D of about 5 μm to about 50 μm measured according to industry standard practices and equipment. 50 Suitably, the carbon-based substrate (e.g., graphite powder) has a porosity of about 10% to 30% as measured by methods known in the art and described above. In the examples provided herein, the Brunauer-Emmett-Teller (BET) measurement method and direct FIB SEM imaging method were used to measure the pores and visualize the nanowires and PSAA coatings, as shown in the accompanying drawings.
[0067] The plurality of silicon-based nanostructures (eg, silicon nanowires) and the carbon-based substrate (eg, graphite powder) may together account for ≥ 90% by weight of the composite material. Suitably, the plurality of silicon-based nanostructures and the carbon-based substrate may together account for ≥ 95% by weight of the composite material.
[0068] In an embodiment, the silicon-based nanostructures are silicon nanowires having a diameter of 10 nm to 200 nm. Suitably, the silicon nanowires and the carbon-based powder comprise ≥ 90 wt% of the composite material.
[0069] A plurality of silicon-based nanostructures (e.g., silicon nanowires) attached to a carbon-based substrate (e.g., graphite powder) may contain 1 wt% to 40 wt% silicon. Suitably, a plurality of silicon-based nanostructures attached to a carbon-based substrate contain 2.5 wt% to 25 wt% silicon. Most suitably, a plurality of silicon-based nanostructures attached to a carbon-based substrate contain 5 wt% to 15 wt% silicon (e.g., 8 wt% to 11 wt% silicon).
[0070] In an embodiment, the silicon-based nanostructure is a silicon nanowire having a diameter of 10 nm to 200 nm, and the carbon-based substrate is a silicon nanowire having a diameter of 5 μm to 50 μm. 50 Suitably, the silicon nanowires attached to the graphite powder comprise 1 wt % to 40 wt % (eg 5 wt % to 15 wt %) silicon.
[0071] In an embodiment, the composite material comprises a plurality of silicon-based nanostructures (e.g., silicon nanowires) and a carbon-based substrate (e.g., graphite powder) of ≥90% by weight, and a polymer (e.g., PSAA) of a monomer unit comprising styrene and allyl alcohol of 0.1% to 10% by weight. Suitably, the composite material comprises a plurality of silicon-based nanostructures and a carbon-based substrate of ≥95% by weight, and a polymer of a monomer unit comprising styrene and allyl alcohol of 0.5% to 5% by weight (e.g., 0.7% to 2% by weight). Silicon can account for 2% to 40% by weight (e.g., 5% to 15% by weight) of a plurality of silicon-based nanostructures attached to a carbon-based substrate.
[0072] In certain embodiments, a polymer (e.g., PSAA) comprising monomer units formed from styrene and allyl alcohol may be provided as an outer coating (partially or completely) on a plurality of silicon-based nanostructures and a carbon-based substrate. In such embodiments, a plurality of silicon-based nanostructures and a carbon-based substrate may further comprise a conductive carbon coating provided as an inner coating. The inner coating is located between the plurality of silicon-based nanostructures and the carbon-based substrate and the outer coating. The conductive carbon coating may be formed by carbonizing a polymer coating pre-set on the silicon-based nanostructure and the carbon-based substrate (e.g., at a temperature of 200° C. to 750° C.), wherein the polymer coating may be a polymer (e.g., PSAA) comprising monomer units formed from styrene and allyl alcohol.
[0073] In some embodiments, the composite material comprises a carbon-based substrate having a polymer comprising monomer units formed from styrene and allyl alcohol directly disposed thereon and a community of silicon-based nanostructures, and a carbon-based substrate having a polymer comprising monomer units formed from styrene and allyl alcohol indirectly disposed thereon via an intermediate conductive carbon coating and a community of silicon-based nanostructures.
[0074] The composite material may further include a conductive additive. Conductive additives that can be used to prepare battery anode materials are well known to those skilled in the art and include carbon black particles, carbon nanofibers, carbon nanotubes, graphite particles, graphene particles, mesophase carbon microsphere particles, and combinations of two or more thereof. "Carbon black" as used herein refers to materials produced by incomplete combustion of petroleum products. Carbon black is a form of amorphous carbon with an extremely high surface area to volume ratio. "Graphene" refers to a single atomic carbon layer formed into a sheet and can be prepared as graphene powder. Reference is made to U.S. Patent Nos. 5,677,082, 6,303,266, and 6,479,030, the disclosures of each of which are incorporated herein by reference in their entirety. A particularly suitable conductive additive is carbon black. When a conductive additive is present, it may be disposed on a polymer (e.g., PSAA) comprising a monomer unit formed of styrene and allyl alcohol or dispersed throughout the polymer. In some embodiments, the use of a conductive carbon coating formed of carbonized PSAA may eliminate the need for additional conductive additives.
[0075] The composite material is suitably provided as a plurality of particles. The exact form of the composite material will depend on the character of the silicon-based nanostructure and the carbon-based substrate. For example, the composite material can be provided as a powder (e.g., a free-flowing powder). The presence of a polymer comprising the monomeric units formed by styrene and allyl alcohol on the outer surface of the silicon-based nanostructure and the carbon-based substrate causes very little (if any) agglomeration between the single composite particles at room temperature or at a temperature lower than the polymer softening temperature.
[0076] In a second aspect, the embodiment provides a method for preparing a composite material. The method is shown, for example, in Figure 2A In. Figure 2A As shown in , the method (100) includes mixing a plurality of silicon-based nanostructures attached to a carbon-based substrate with a solution of a polymer to form a mixture (104), wherein the polymer includes monomer units formed from styrene and allyl alcohol; and drying the mixture (108).
[0077] It should be appreciated that those features of the second aspect also described above in relation to the first aspect may have any of the above definitions.
[0078] The silicon-based nanostructures attached to the carbon-based substrate can be prepared by growing the silicon-based nanostructures (e.g., silicon nanowires) from catalyst particles deposited on the surface of the carbon-based substrate via VLS or VSS chemical vapor deposition techniques. In some embodiments, the carbon-based substrate is a graphite powder (e.g., natural graphite powder or artificial graphite powder) comprising a plurality of graphite particles, each graphite particle comprising a plurality of pores, wherein the silicon-based nanostructures (e.g., silicon nanowires) are grown from catalyst particles (e.g., catalyst nanoparticles comprising copper, copper compounds, and / or copper alloys) deposited on the outer and inner surfaces (i.e., those surfaces defining the pores) of the graphite particles by VLS or VSS chemical vapor deposition techniques, thereby providing silicon-based nanostructures attached to the outer and inner surfaces of the graphite particles. Figures 1A to 1C Shown is an SEM photograph of uncoated natural graphite particles comprising silicon-based nanowires attached to the surfaces of the graphite particles, including silicon nanowires attached to the interior surfaces (ie, those surfaces defining the pores).
[0079] The solution of the polymer (e.g., PSAA) may comprise a polymer and ethanol. Compared with the use of water-soluble polymers, ethanol-soluble polymers may be dried directly at lower temperatures and / or pressures below atmospheric pressure without leaving any solvent residues on the silicon-based nanostructures (which may have a negative impact on battery performance). The ethanol removed during the drying process may be recovered and recycled into the process. Suitably, the solution comprises <5% by weight of water. More suitably, the solution is water-free.
[0080] The solution of the polymer may comprise 0.05 to 10 wt% polymer (for example 0.05 to 10 wt% polymer in ethanol). Suitably, the solution comprises 0.1 to 3 wt% polymer.
[0081] Drying may be carried out at a temperature of 20° C. to 150° C., at ambient pressure or under reduced pressure (eg under vacuum). Suitably, drying is carried out at a temperature of 30° C. to 130° C. Step (b) may be carried out under an inert gas (eg nitrogen).
[0082] In another aspect, embodiments provide methods for preparing composite materials, such as e.g. Figure 2B As shown in Figure 2B As shown in , the method (150) includes mixing a plurality of silicon-based nanostructures attached to a carbon-based substrate with a solution of a polymer to form a mixture (154), wherein the polymer includes monomer units formed from styrene and allyl alcohol; and drying the mixture (158).
[0083] In an embodiment, the plurality of silicon-based nanostructures and the carbon-based substrate have a conductive carbon coating disposed thereon. The coating may be partial or complete. The conductive carbon coating may be formed by carbonizing a polymer coating previously disposed on the plurality of silicon-based nanostructures and the carbon-based substrate (162), such as Figure 2B As shown in . The polymer coating may include monomer units formed from styrene and allyl alcohol (e.g., PSAA). The polymer coating may be pre-set on multiple silicon-based nanostructures and carbon-based substrates by mixing multiple silicon-based nanostructures and carbon-based substrates with a solution of a polymer material (e.g., a solution of PSAA in ethanol, such as a 5-10 wt % solution of PSAA in ethanol). Subsequently, the polymer material pre-set on multiple silicon-based nanostructures and carbon-based substrates is carbonized by heating the multiple silicon-based nanostructures and carbon-based substrates having the polymer material set thereon to a temperature of 200° C. to 750° C. (e.g., 500° C. to 750° C.), preferably in an inert atmosphere (e.g., under nitrogen). Therefore, in some embodiments, the composite material obtained by drying may include PSAA set on a carbonized PSAA coating, and the carbonized PSAA coating is set on the silicon-based nanostructures and the carbon-based substrate.
[0084] The composite material resulting from drying is suitably a powder (eg a free-flowing powder).The use of a polymer comprising monomer units formed from styrene and allyl alcohol (particularly PSAA) results in little or no agglomeration between the composite material particles.
[0085] like Figure 2B As shown in , the method (150) may further include mixing the carbon-coated Si-based nanostructures attached to the carbon-based substrate with a solution of a polymer comprising monomer units formed from styrene and allyl alcohol (166), and drying the mixture to obtain a composite material (170) comprising a polymer coating disposed on the carbon-coated Si-based nanostructures attached to the carbon-based substrate.
[0086] In a third aspect, embodiments provide a composite material obtained, directly obtained or obtainable by the method of the second aspect.
[0087] Anode electrode and its preparation
[0088] In a fourth aspect, embodiments provide an anode electrode comprising a first anode layer including a binder and a composite material as described herein.
[0089] The anode electrode described herein (which comprises a polymer comprising a monomeric portion formed of styrene and allyl alcohol disposed on a silicon-based nanostructure attached to a carbon-based substrate) has those advantageous properties discussed above, including improved uniformity, ease of processing according to wet or dry electrode coating techniques, improved ability to accommodate volume changes, and excellent adhesion to other anode components (including current collectors and any additional anode layers). Therefore, batteries incorporating the anode electrode of the present invention provide improved electronic properties (e.g., specific capacity and / or initial coulombic efficiency (ICE)).
[0090] It will be appreciated that those features of the fourth aspect also described above in relation to the first, second or third aspect may have any of the above definitions.
[0091] The first anode layer comprises a binder and a composite material of the first aspect, suitably a close and substantially uniform mixture. Any suitable binder can be used in the first anode layer. Suitably, the binder is selected from styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), poly (vinylidene fluoride) (PVDF), poly (acrylic acid) (PAA), poly (acrylonitrile) (PAN), poly (acrylamide-to-diallyl dimethyl ammonium) (PAADAA), poly (tetrafluoroethylene) (PTFE) and a combination of two or more thereof. In a particular embodiment, the binder is a mixture of styrene butadiene rubber and carboxymethyl cellulose. For example, the binder can be a mixture of styrene butadiene rubber and carboxymethyl cellulose, comprising 30% to 70% by weight of styrene butadiene rubber and 30% to 70% by weight of carboxymethyl cellulose, more suitably comprising 40% to 60% by weight of styrene butadiene rubber and 40% to 60% by weight of carboxymethyl cellulose. In other embodiments, the binder is poly (tetrafluoroethylene), which is particularly useful when the first anode layer is prepared by dry coating technology.
[0092] The first anode layer may suitably additionally comprise a conductive additive in an amount of 0.2 wt % to 5 wt %. Suitable conductive additives are described above. A particularly suitable conductive additive is carbon black. The conductive additive may be dispersed throughout the binder, and / or the composite material, binder and conductive additive may form a close and substantially uniform mixture within the first anode layer. A polymer comprising monomer units formed from styrene and allyl alcohol (e.g., PSAA) may be disposed on the conductive additive.
[0093] The first anode layer suitably comprises ≥ 90 wt % of the composite material. As described above, the plurality of silicon-based nanostructures attached to the carbon-based substrate present in the composite material may comprise 1 wt % to 40 wt % of silicon. Also as described above, the composite material may comprise 0.1 wt % to 10 wt % of a polymer (e.g., PSAA) comprising monomeric units formed from styrene and allyl alcohol.
[0094] The presence of a polymer comprising monomeric units formed from styrene and allyl alcohol in the composite material of the first aspect can allow the preparation of an anode electrode with a reduced amount of binder, so that the anode electrode has a low ratio of inactive material to active material. For example, the first anode layer may comprise 0.5 wt % to 10 wt % of binder. Suitably, the first anode layer comprises 1 wt % to 6 wt % of binder.
[0095] The first anode layer can include 0.5 wt % to 10 wt % of a binder and 90 wt % to 99.5 wt % of this composite material. Suitably, the first anode layer includes 1 wt % to 6 wt % of a binder and 94 wt % to 99 wt % of this composite material. In this composite material, a plurality of silicon-based nanostructures attached to a carbon-based substrate can include 1 wt % to 40 wt % of silicon. This composite material can include 0.1 wt % to 10 wt % of a polymer (such as PSAA) comprising a monomer unit formed by styrene and allyl alcohol.
[0096] In some embodiments, the first anode layer comprises 0.5% to 10% by weight of a binder and 90% to 99.5% by weight of the composite material, wherein the composite material comprises 0.1% to 10% by weight (e.g., 0.5% to 5% by weight) of a polymer (e.g., PSAA) comprising monomer units formed from styrene and allyl alcohol. Suitably, the binder is a mixture of styrene butadiene rubber and carboxymethyl cellulose (e.g., 30% to 70% by weight of styrene butadiene rubber and 30% to 70% by weight of carboxymethyl cellulose). The first anode layer may further comprise 0.2% to 5% by weight of a conductive additive (e.g., carbon black).
[0097] In some embodiments, the first anode layer comprises 1 wt % to 6 wt % of a binder and 94 wt % to 99 wt % of the composite material, wherein the composite material may comprise 0.1 wt % to 10 wt % (e.g., 0.5 wt % to 3 wt %) of a polymer (e.g., PSAA) comprising monomer units formed from styrene and allyl alcohol. Suitably, the binder is a mixture of carboxymethyl cellulose and styrene butadiene rubber (e.g., 40 wt % to 60 wt % of styrene butadiene rubber and 40 wt % to 60 wt % of carboxymethyl cellulose). The first anode layer may further comprise 0.2 wt % to 5 wt % of a conductive additive (e.g., carbon black).
[0098] The anode electrode may be a single layer anode electrode such that the first anode layer is the only anode layer.
[0099] Alternatively, the anode electrode can be a multilayer anode electrode such that it includes one or more additional anode layers. Each additional anode layer can independently include an active material and a binder, which is suitably a close and substantially uniform mixture. Any one or more of the above-mentioned binders can be used. The active material can be selected from graphite powder, a plurality of silicon-based nanostructures attached to a carbon-based substrate, a composite material of the first aspect, and a combination of two or more thereof. Each additional anode layer can optionally include one or more conductive additives described herein. The multilayer anode electrode can be described as a stack of anode layers (e.g., a first anode layer and one or more additional anode layers). In a multilayer anode, one or more of the anode layers can include different carbon-based substrates and different amounts of silicon-based nanostructures attached to the carbon-based substrate. Each of the multiple layers can also include a plurality of conductive nanostructures having different D 50 Each of the multiple layers may also have a different porosity. A polymer comprising monomer units formed from styrene and allyl alcohol (eg, PSAA) may be applied to the silicon-based nanostructures and the carbon-based substrate in all layers or only in some layers.
[0100] The anode electrode may further comprise a current collector. Any suitable current collector may be used in the anode electrode of the present invention. Suitably, the current collector is a copper foil or a carbon-coated copper foil.
[0101] The first anode layer and any additional anode layers are intended to be in electrical communication with a current collector so that current can flow from the electrolyte to the current collector.The current collector may form part of the anode electrode.
[0102] In certain embodiments, the first anode layer comprises a first surface configured to contact (or be in contact with) a current collector, and a second surface in contact with one or more additional anode layers. The second surface of the first anode layer may comprise metallic lithium disposed thereon. The metallic lithium may be selected from lithium metal foil, stable lithium metal powder, and combinations thereof.
[0103] In other embodiments, the anode electrode comprises one or more additional anode layers described herein positioned between the first anode layer and the current collector.
[0104] The first anode layer and any additional anode layers may be substantially free of (e.g., free of) solvent residues and / or may each be provided as a self-supporting film. Such anode layers may be formed, for example, by dry coating techniques (e.g., by extrusion and / or calendering). In an embodiment, the anode electrode is a multilayer anode electrode, wherein all anode layers are substantially free of (e.g., free of) solvent residues (e.g., have been formed by dry coating techniques).
[0105] The polymer (e.g., PSAA) comprising monomeric units formed from styrene and allyl alcohol present in the composite material exhibits favorable interactions with binders (e.g., poly(tetrafluoroethylene)) commonly used to form anode layers according to dry coating techniques. Composite materials comprising polymers (e.g., PSAA) are typically provided as powders at room temperature with little or no agglomeration of particles. The composite material (e.g., composite powder) can be directly mixed with a binder to provide a compact and substantially uniform powder with little or no agglomeration. A moderate increase in temperature (e.g., to 50° C. to 200° C., or 60° C. to 180° C.) softens the polymer (e.g., PSAA) of the composite material and promotes adhesion to the binder particles, allowing the dried anode layer (e.g., extruded and / or calendered) to be formed into a film, such as a self-supporting film.
[0106] In an embodiment, the binder of the first anode layer is poly(tetrafluoroethylene), wherein the first anode layer is substantially free of (e.g., free of) solvent residues. The anode electrode can be a single-layer anode electrode. Alternatively, the anode electrode can be a multi-layer anode electrode, wherein one or more additional anode layers further comprise poly(tetrafluoroethylene) as a binder. The multi-layer anode electrode can be such that all anode layers are substantially free of (e.g., free of) solvent residues.
[0107] The first anode layer and any additional anode layers may have a -3 Up to 1.7 g cm -3 Suitably, the first anode layer and any additional anode layers may have a density of 1.3 g cm -3 Up to 1.5 g cm -3 density.
[0108] In a fifth aspect, embodiments provide a method (200) for preparing an anode electrode, such as Figure 3 as shown in . Figure 3 The method includes mixing: a composite material as described herein and a binder to form a mixture (204); and applying a layer of the mixture (208).
[0109] It will be appreciated that those features of the fifth aspect also described above in relation to the first, second, third or fourth aspects may have any of the above definitions. For example, it will be appreciated that the composite material of the fifth aspect may first be prepared according to the steps outlined in the second aspect.
[0110] The components mixed during the mixing process may further include a conductive additive. Suitable conductive additives are described above. A particularly suitable conductive additive is carbon black. A polymer comprising monomer units formed from styrene and allyl alcohol (e.g. PSAA) may be provided on the conductive additive. The amount of the conductive additive may be from 0.2% to 5% by weight relative to the mass of the composite material and the (dry) adhesive.
[0111] The applied layer is configured to be in contact with the current collector. For example, applying the layer of the mixture may include applying the layer of the mixture so that it is in electrical communication with the current collector.
[0112] In certain embodiments, the mixture is provided as a wet slurry, and the method further comprises drying the applied layer. For example, the binder can be provided as a solution (e.g., an aqueous solution). The dried layer can then be calendered onto a current collector.
[0113] In other embodiments, the mixture is provided as a solid. In such embodiments, the applied layer may include a layer (e.g., a film) of a shaped (e.g., by extrusion and / or calendering) solid mixture. Before forming, the solid mixture may be heated to a temperature of 50°C to 200°C (e.g., 60°C to 180°C), which may promote adhesion of the composite material to the adhesive, thereby producing a more uniform layer. The shaped (e.g., extruded and / or calendered) layer may be a self-supporting film, which is optionally free of solvent residues. The shaped (e.g., extruded and / or calendered) layer (e.g., a self-supporting film) may then be laminated to the current collector.
[0114] Applying the mixture layer may include applying a layer of the mixture to a current collector. The anode electrode may be a single-layer anode electrode, such that the applied layer is the only anode layer. Alternatively, the anode electrode may be a multilayer anode electrode, such that the method further includes the step of applying one or more additional anode layers to the applied layer, wherein the one or more additional anode layers independently comprise active materials and a binder. Applying one or more additional anode layers to the layer may be described as forming a stack of anode layers.
[0115] In an additional aspect, an embodiment provides a method for preparing an anode electrode, the method comprising: mixing a plurality of silicon-based nanostructures attached to a carbon-based substrate, a polymer comprising monomer units formed from styrene and allyl alcohol, and a binder to form a mixture; and applying a layer of the mixture.
[0116] It should be appreciated that those features of this additional aspect also described above in relation to the first, second, third, fourth or fifth aspect may have any of the above definitions.
[0117] In a sixth aspect, embodiments provide an anode electrode obtained, directly obtained, or obtainable by any of the methods for preparing an anode electrode described hereinbefore.
[0118] Battery
[0119] In a seventh aspect, embodiments provide a battery comprising a composite material and / or an anode electrode as described herein.
[0120] A battery whose anode comprises a polymer comprising a monomeric moiety formed of styrene and allyl alcohol disposed on a silicon-based nanostructure attached to a carbon-based substrate has those advantageous properties discussed above, including improved anode uniformity, improved ability to accommodate volume changes, and excellent integrity of the anode assembly. Thus, the battery described herein provides improved electronic properties (e.g., specific capacity and / or initial coulombic efficiency (ICE)).
[0121] Most suitably, the battery is a lithium ion battery.
[0122] Numbered statements
[0123] The following numbered statements 1-64 are not claims, but rather describe certain aspects and embodiments.
[0124] 1. A composite material comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol.
[0125] 2. The composite material of claim 1, wherein the polymer has a softening point below 200°C.
[0126] 3. The composite material of claim 1 or 2, wherein the polymer is insoluble in water.
[0127] 4. The composite material of claim 1, 2 or 3, wherein the polymer is soluble in alcohol (eg, ethanol).
[0128] 5. The composite material of any preceding statement, wherein the polymer is poly(styrene-co-allyl alcohol).
[0129] 6. The composite material of any of the preceding statements, wherein the polymer comprises at least 25 mol % of monomer units formed from allyl alcohol.
[0130] 7. The composite material of any preceding statement, wherein the composite material comprises from 0.1 wt% to 10 wt% of the polymer.
[0131] 8. The composite material of any preceding statement, wherein the composite material comprises 0.5 wt% to 5 wt% of the polymer.
[0132] 9. The composite material of any of the preceding statements, wherein the plurality of silicon-based nanostructures are silicon nanowires, silicon nanoparticles, or a combination thereof.
[0133] 10. The composite material of any preceding statement, wherein the plurality of silicon-based nanostructures are silicon nanowires.
[0134] 11. The composite material of claim 10, wherein the silicon nanowires have a diameter of 10 nm to 200 nm.
[0135] 12. The composite material of any of the preceding statements, wherein the plurality of silicon-based nanostructures comprises a single crystalline core and a shell layer, wherein the shell layer comprises amorphous silicon, polycrystalline silicon, or a combination thereof.
[0136] 13. The composite material of any of the preceding statements, wherein the composite material comprises ≥ 90 wt. % of silicon-based nanostructures attached to a carbon-based substrate.
[0137] 14. The composite material of any of the preceding statements, wherein the composite material comprises > 95 wt. % of silicon-based nanostructures attached to a carbon-based substrate.
[0138] 15. The composite material of any preceding statement, wherein the carbon-based substrate is a carbon-based powder.
[0139] 16. The composite material of claim 15, wherein the carbon-based powder has a D 50 .
[0140] 17. The composite material of any of the preceding statements, wherein the carbon-based substrate is selected from graphite powder, mesocarbon microbead powder or a combination thereof.
[0141] 18. The composite material of any preceding statement, wherein the carbon-based substrate is graphite powder.
[0142] 19. The composite material of any of the preceding statements, wherein the carbon-based substrate is a graphite powder comprising a plurality of graphite particles, each particle comprising a plurality of pores disposed therein, wherein the silicon-based nanostructures are attached to a surface defining said pores.
[0143] 20. The composite material of any preceding statement, wherein the carbon-based substrate is a graphite powder comprising uncoated natural graphite particles.
[0144] 21. The composite material of any preceding statement, wherein the plurality of silicon-based nanostructures attached to the carbon-based substrate comprises 1 wt% to 40 wt% silicon.
[0145] 22. The composite material of any preceding statement, wherein the plurality of silicon-based nanostructures attached to the carbon-based substrate comprises 2.5 wt% to 25 wt% silicon (eg, 5 wt% to 15 wt% silicon).
[0146] 23. The composite material of any of the preceding statements, wherein the plurality of silicon-based nanostructures and the carbon-based substrate further comprise a conductive carbon coating (e.g., carbonized PSAA), wherein a polymer comprising monomer units formed from styrene and allyl alcohol (e.g., PSAA) is disposed on the conductive carbon coating.
[0147] 24. The composite material of claim 23, wherein the conductive carbon coating (e.g., carbonized PSAA) is provided as an inner coating on a plurality of silicon-based nanostructures and a carbon-based substrate, and a polymer comprising monomer units formed from styrene and allyl alcohol (e.g., PSAA) is provided as an outer coating on a plurality of silicon-based nanostructures and a carbon-based substrate.
[0148] 25. A method for preparing a composite material, the method comprising:
[0149] mix:
[0150] a plurality of silicon-based nanostructures attached to a carbon-based substrate, and
[0151] a solution of a polymer comprising monomer units formed from styrene and allyl alcohol to form a mixture; and
[0152] The mixture was dried.
[0153] 26. The method of claim 25, wherein the solution of the polymer comprises the polymer and an alcohol solvent (eg, ethanol).
[0154] 27. The method of claim 25 or 26, wherein the solution of the polymer does not contain water.
[0155] 28. The method of claim 25, 26 or 27, wherein the solution comprises 0.05 wt % to 10 wt % of the polymer.
[0156] 29. The method of any one of claims 25 to 28, wherein the solution comprises 0.1 wt% to 3 wt% of the polymer (eg, 0.5 wt% to 1.5 wt%).
[0157] 30. The method of any one of claims 25 to 29, wherein the drying is carried out at a temperature of 20°C to 150°C, under ambient pressure or reduced pressure (eg, under vacuum).
[0158] 31. The method of any one of claims 25 to 30, wherein the drying is carried out at a temperature of 30°C to 130°C, optionally under an inert gas (eg, nitrogen).
[0159] 32. The method of any one of claims 25 to 31, wherein the plurality of silicon-based nanostructures attached to the carbon-based substrate comprises a conductive carbon coating.
[0160] 33. The method of claim 32, wherein the conductive carbon coating is formed by carbonizing a polymer coating previously disposed on the silicon-based nanostructures and the carbon-based substrate.
[0161] 34. The method of claim 33, wherein the polymer coating pre-disposed on the silicon-based nanostructures and the carbon-based substrate is a polymer comprising monomer units formed from styrene and allyl alcohol.
[0162] 35. The method of claim 33 or 34, wherein carbonizing the polymer coating pre-disposed on the silicon-based nanostructures and the carbon-based substrate comprises heating the silicon-based nanostructures and the carbon-based substrate having the polymer coating pre-disposed thereon at a temperature of 200°C to 750°C (e.g., 500°C to 750°C), optionally in an inert atmosphere (e.g., under nitrogen).
[0163] 36. An anode electrode comprising a first anode layer comprising a binder and the composite material of any one of statements 1 to 24.
[0164] 37. The anode electrode of claim 36, wherein the binder is selected from the group consisting of styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), poly(vinylidene fluoride) (PVDF), poly(acrylic acid) (PAA), poly(acrylonitrile) (PAN), poly(acrylamide-co-diallyldimethylammonium) (PAADAA), poly(tetrafluoroethylene) (PTFE), and combinations of two or more thereof.
[0165] 38. The anode electrode of claim 36 or 37, wherein the binder is a mixture of styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC).
[0166] 39. The anode electrode of statement 38, wherein the binder comprises 30 wt % to 70 wt % of butadiene rubber (SBR) and 30 wt % to 70 wt % of carboxymethyl cellulose (CMC).
[0167] 40. The anode electrode of claim 36 or 37, wherein the binder is poly(tetrafluoroethylene) (PTFE).
[0168] 41. The anode electrode of any one of statements 36 to 40, wherein the first anode layer comprises 0.5 wt % to 10 wt % of the binder.
[0169] 42. The anode electrode of any one of statements 36 to 41, wherein the first anode layer comprises 1 wt % to 6 wt % of the binder.
[0170] 43. The anode electrode of any one of statements 36 to 42, wherein the first anode layer comprises ≥ 90 wt% of the composite material.
[0171] 44. The anode electrode of any one of statements 36 to 43, wherein the first anode layer further comprises a conductive additive.
[0172] 45. The anode electrode of claim 44, wherein the first anode layer comprises 0.2 wt % to 5 wt % of the conductive additive.
[0173] 46. The anode electrode of statement 44 or 45, wherein the conductive additive is selected from the group consisting of carbon black particles, carbon nanofibers, carbon nanotubes, and combinations of two or more thereof.
[0174] 47. The anode electrode of any one of statements 36 to 46, wherein the anode electrode further comprises a current collector.
[0175] 48. The anode electrode of claim 47, wherein the current collector is a copper foil or a carbon-coated copper foil.
[0176] 49. The anode electrode of any one of statements 36 to 48, further comprising one or more additional anode layers, each additional anode layer independently comprising an active material and a binder.
[0177] 50. The anode electrode of claim 49, wherein the first anode layer comprises a first surface configured to contact (or be in contact with) a current collector and a second surface in contact with one or more additional anode layers.
[0178] 51. The anode electrode of statement 50, wherein the second surface of the first anode layer comprises metallic lithium disposed thereon.
[0179] 52. The anode electrode of claim 51, wherein the metallic lithium is selected from the group consisting of lithium metal foil, stabilized lithium metal powder, and combinations thereof.
[0180] 53. The anode electrode of any one of statements 49 to 52, wherein the active material is selected from graphite powder, a plurality of silicon-based nanostructures attached to a carbon-based substrate, a composite material as in any one of statements 1 to 24, and a combination of two or more thereof.
[0181] 54. The anode electrode of claim 53, wherein at least one of the one or more additional anode layers further comprises a conductive additive, wherein the conductive additive is selected from the group consisting of carbon black particles, carbon nanofibers, carbon nanotubes, and combinations of two or more thereof.
[0182] 55. A method for preparing an anode electrode, the method comprising:
[0183] mix:
[0184] The composite material of any one of claims 1 to 24, and
[0185] a binder to form a mixture; and
[0186] Apply a layer of this mixture.
[0187] 56. The method of claim 55, wherein the layer is configured to contact a current collector.
[0188] 57. The method of claim 55 or 56, wherein the mixture is provided as a wet slurry, and the method further comprises drying the layer.
[0189] 58. The method of claim 55 or 56, wherein the mixture is provided as a solid, and the applying comprises forming a layer of the solid mixture.
[0190] 59. The method of any one of statements 55 to 58, wherein the applying comprises applying a layer of the mixture onto a current collector.
[0191] 60. The method of claim 59, further comprising applying one or more additional anode layers onto the layer, wherein the one or more additional anode layers each independently comprise an active material and a binder.
[0192] 61. The method of claim 60, wherein the active material is selected from the group consisting of graphite powder, a plurality of silicon-based nanostructures attached to a carbon-based substrate, a composite material as in any one of claims 1 to 24, and a combination of two or more thereof.
[0193] 62. The method of claim 61, wherein at least one of the one or more additional anode layers further comprises a conductive additive, wherein the conductive additive is selected from the group consisting of carbon black particles, carbon nanofibers, carbon nanotubes, and combinations of two or more thereof.
[0194] 63. A battery comprising: the composite material of any one of statements 1 to 24 and / or the anode electrode of any one of statements 36 to 54.
[0195] 64. The battery of claim 63, wherein the battery is a lithium ion battery.
[0196] Example
[0197] One or more embodiments of the present invention will now be described for purposes of illustration only with reference to the accompanying drawings:
[0198] Figure 4 The performance of half cells 1-3 described in Example 2 is shown.
[0199] Figure 5The cycling performance of the three anodes described in Example 2 is shown.
[0200] Figure 6 The performance of half cells 1-3 described in Example 2 is shown.
[0201] Fig. 7A , 7B A high magnification SEM picture of SiNW-carbon powder after PSAA carbonization in Example 3 is shown, showing a thin coating on the silicon and graphite surfaces.
[0202] Figure 8 The performance of the two NCA pouch cell batteries described in Example 4 is shown.
[0203] Fig. 9 The performance of the two NCA pouch cell batteries described in Example 5 is shown.
[0204] Fig.10 The specifications, first charge capacity, and first discharge capacity of four groups of electrochemical anode material composites containing different combinations of SiNW-carbon and PSAA are shown.
[0205] Fig.11 The specific discharge capacity over hundreds of cycles is shown for two types of electrochemical cells, the first type comprising anode composites prepared using a single surface treatment and the second type comprising anode composites prepared using dual surface treatments.
[0206] Fig.12 The % capacity retention over hundreds of cycles is shown for two types of electrochemical cells, the first type comprising anode composites prepared using a single surface treatment and the second type comprising anode composites prepared using dual surface treatments.
[0207] Example 1 - Preparation of composite materials
[0208] Assemble the following reagents:
[0209] 1 kg of silicon nanowires mechanically and conductively attached to graphite particles, wherein the Si weight % is equal to 9.7% (hereinafter referred to as SiNW-carbon powder), the silicon nanowires having a diameter of 20 nm to 100 nm (measured with FESEM), and the graphite particles are composed of D 50 = 14 microns of commercially available natural graphite. Silicon nanowires are grown onto graphite particles using the decomposition of a silane gas precursor in a CVD reactor due to a copper (I) oxide nanoparticle catalyst disposed on the graphite particles, as described in U.S. Pat. No. 10,243,207, the entire contents of which are incorporated herein by reference.
[0210] 20.2 g of a 50 wt% solution of PSAA in EtOH (10.1 g of calculated PSAA polymer content), obtained from Sigma-Aldrich with a molecular weight of M n ~1600.
[0211] 1000 g ethanol.
[0212] The composite material was prepared as follows:
[0213] a) 1000 grams of ethanol were mixed with 20.2 grams of a 50 wt% solution of PSAA in ethanol in a 5 liter stainless steel container by pushing for 5 minutes to obtain 1020.2 grams of a diluted PSAA solution containing -10.1 grams of PSAA polymer.
[0214] b) 1 kg of SiNW-carbon powder was immersed in the PSAA solution in a 5 liter container and mixed for 30 minutes to produce a mixture comprising SiNW-carbon powder with PSAA polymer uniformly disposed thereon.
[0215] c) The mixture in the 5 liter container was placed in an oven to dry at 40 to 120° C. under nitrogen for about 2 hours to produce 1010.1 grams of dry composite particles. The PSAA coated SiNW-carbon powder formed a powder of individual particles without any grinding or sieving.
[0216] Example 2 - Half-cell cell studies
[0217] Three half-unit cells were prepared according to the following general protocol:
[0218] a) 6.12 grams of 1.5 wt% CMC stock solution (in DI water) were gradually added to 3.97 grams of DI water in a planetary kneader vessel followed by mixing at 600 rpm for 15 minutes. The resulting mixture was maintained at 30°C.
[0219] b) 5.94 g of SiNW-carbon powder (with or without PSAA disposed thereon) were gradually added to the mixture obtained from step a).The resulting mixture was mixed in a planetary kneader vessel (non-bubbling kneader, NBK-1) at 400 rpm for 15 minutes.
[0220] c) 0.23 g of a 40 wt% SBR suspension was added to the mixture obtained from step b). The resulting mixture was then mixed at 400 rpm for 15 minutes.
[0221] d) The slurry obtained from step c) was placed in a 40°C bath for 2 minutes and then mixed again to reach a slurry temperature of 30°C.
[0222] e) The slurry obtained from step d) was then used to coat an anode electrode onto a copper foil using a doctor blade. The electrode was then dried at 90°C for 60 minutes.
[0223] f) After 60 minutes at room temperature, the electrode obtained from step e) is subsequently calendered to a temperature of 1-1.65 g cm -3 Density, 1.4gcm -3 The density of is used as an example.
[0224] Half cell 1 is used to build a 1.5 wt% CMC, 1.5 wt% SBR, 1 wt% Super Baseline performance of an anode containing 96 wt% SiNW-carbon powder (without PSAA) and a conductive additive (carbon black) containing 9.7 wt% Si. Lithium foil was used as the counter electrode. Figure 4 As shown in Table 1 (below), the observed first delithiation specific capacity was 629.03 mAh / g and the observed initial coulombic efficiency (ICE) was 90.00%.
[0225] Half-cell 2: by mixing 95.54 wt% SiNW-carbon powder (9.7 wt% Si), 1.5 wt% CMC, 1.5 wt% SBR, 1 wt% Super A water-based slurry was prepared by adding a conductive additive (carbon black) and 1 wt % PSAA (from a 50 wt % PSAA solution in EtOH). The anode electrode was coated onto a copper foil using the slurry. When 1 wt % PSAA was added to a slurry containing 1.5 wt % CMC, 1.5 wt % SBR, 1 wt % Super P and 95.54 wt % SiNW-carbon powder (9.7 wt % Si), the anode electrode was coated onto a copper foil. Figure 4 As shown in Table 1 (below), the resulting anode exhibited a first delithiation specific capacity of 633.08 mAh / g and an initial coulombic efficiency (ICE) of 90.13%. The results show that incorporating PSAA into the anode yields higher delithiation capacity and higher ICE relative to baseline anode half-cell 1.
[0226] Half-cell 3: Prepared by mixing 96 wt% SiNW-carbon powder (9.7 wt% Si) pretreated with 1 wt% PSAA according to the deposition method outlined in Example 1, 1.5 wt% CMC, 1.5 wt% SBR, and 1 wt% Super (carbon black) conductive additive to prepare a slurry. This slurry is used to coat the anode electrode on copper foil. When SiNW-carbon powder pretreated with 1 wt % PSAA is used, Figure 4As shown in Table 1 (below), the resulting anode exhibited a further improved first delithiation specific capacity of 634.89 mAh / g and a further improved ICE of 90.92%. The results indicate that the PSAA present on the SiNW-carbon powder can lead to favorable interactions with the CMC / SBR binder. These interactions lead to a more uniform anode, which allows lithium ions to better access the active materials (SiNW and graphite), thereby resulting in improved specific capacity and ICE.
[0227] The performance of the three anode half-cells is summarized in Table 1 and shown in Figure 4 middle.
[0228] Table 1 - Performance of half-cells 1-3
[0229]
[0230] like Figure 4 As shown in Table 1, the application of PSAA improves ICE by nearly 1%. Depending on the N / P ratio of the anode and cathode specific capacities (i.e., N / P=1.05), the approximately 1% higher anode ICE results in a savings of approximately 1% of cathode materials that are up to five times more expensive than graphite materials, providing significant savings to EV cell manufacturers.
[0231] The same slurry composition was used to form the three anodes used in its NCA pouch cells. The NCA material was purchased from BASF. The N / P ratio was 1.05. After completing the formation process with subsequent charge / discharge at C / 20 between 4.2V and 2.5V for one cycle, and charge / discharge at C / 10 and C / 5 between 4.2V and 3V for one cycle, the three cells were cycled at C / 3 charge and C / 2 discharge between 4.2V and 3V, as shown in FIG. Figure 5 As shown in Figure 5 The cycling performance was measured and compared as outlined in .
[0232] Cycling performance was established using a baseline anode of 1.5 wt% CMC / 1.5 wt% SBR, 1 wt% Super P, and SiNW-carbon powder (9.7 wt% Si). Figure 5 As shown in , when 1 wt % PSAA is added to the slurry, the resulting anode shows some improvement in NCA full cell cycling performance over the baseline NCA cell. Figure 5 Further improvements were achieved using anodes containing SiNW-carbon powder pretreated with 1 wt % PSAA, as shown in . The results indicate that pretreatment of SiNW-carbon powder with PSAA can significantly improve the full cell performance of SiNW-carbon anodes, especially in anodes using low levels of CMC / SBR binder.
[0233] Example 3 - PSAA Carbonization Study
[0234] Assemble the following reagents:
[0235] 1 kg of silicon nanowires mechanically and conductively attached to graphite particles, wherein the Si weight % is equal to 9.7% (hereinafter referred to as SiNW-carbon powder), the silicon nanowires having a diameter of 20 nm to 100 nm (measured with FESEM), and the graphite particles are composed of D 50 = 14 microns of commercially available natural graphite. Silicon nanowires are grown onto graphite particles using the decomposition of a silane gas precursor in a CVD reactor due to a copper (I) oxide nanoparticle catalyst disposed on the graphite particles, as described in U.S. Pat. No. 10,243,207, the entire contents of which are incorporated herein by reference.
[0236] 160.0 g of a 50 wt% solution of PSAA in EtOH (80.0 g of calculated PSAA polymer content), obtained from Sigma-Aldrich with a molecular weight of M n ~1600.
[0237] 1000 g ethanol.
[0238] The composite material was prepared as follows:
[0239] a) 1000 grams of ethanol were mixed with 160.0 grams of a 50 wt% solution of PSAA in ethanol in a 5 liter stainless steel container by pushing for 5 minutes to obtain 560.0 grams of a diluted PSAA solution containing 80.0 grams of PSAA polymer.
[0240] b) 1 kg of SiNW-carbon powder was immersed in the PSAA solution in a 5 liter container and mixed for 30 minutes to produce a mixture comprising SiNW-carbon powder with PSAA polymer uniformly disposed thereon.
[0241] c) The mixture in the 5 liter container was placed in an oven to dry at 40 to 120° C. under nitrogen for about 2 hours to produce 1080.0 grams of dry composite particles. The PSAA coated SiNW-carbon powder formed a powder of individual particles without any grinding or sieving.
[0242] The PSAA on SiNW-carbon powder can be carbonized at 700 °C for one hour under nitrogen.
[0243] For comparison, amorphous carbon coating on the same SiNW-carbon powder was prepared using acetylene / nitrogen (1:1) gas at 700 °C for 1 h.
[0244] Three half-unit cells were prepared according to the following general protocol:
[0245] a) 6.12 grams of 1.5 wt% CMC stock solution (in DI water) were gradually added to 3.97 grams of DI water in a planetary kneader vessel followed by mixing at 600 rpm for 15 minutes. The resulting mixture was maintained at 30°C.
[0246] b) 5.94 g of SiNW-carbon powder (with or without PSAA disposed thereon) were gradually added to the mixture obtained from step a).The resulting mixture was mixed in a planetary kneader vessel (non-bubbling kneader, NBK-1) at 400 rpm for 15 minutes.
[0247] c) 0.23 g of a 40 wt% SBR suspension was added to the mixture obtained from step b). The resulting mixture was then mixed at 400 rpm for 15 minutes.
[0248] d) The slurry obtained from step c) was placed in a 40°C bath for 2 minutes and then mixed again to reach a slurry temperature of 30°C.
[0249] e) The slurry obtained from step d) was then used to coat an anode electrode onto a copper foil using a doctor blade. The electrode was then dried at 90°C for 60 minutes.
[0250] f) After 60 minutes at room temperature, the electrode obtained from step e) is subsequently calendered to a temperature of 1-1.65 g cm -3 The density is 1.4 g cm -3 The density of is used as an example.
[0251] Half-cell 1 was used to establish baseline performance of an anode having 1.5 wt% CMC, 1.5 wt% SBR, and 97 wt% SiNW-carbon powder (without PSAA) containing 9.7 wt% Si. Lithium foil was used as the counter electrode. The observed first delithiation specific capacity was 648.27 mAh / g, and the observed initial coulombic efficiency (ICE) was 92.41%.
[0252] Half-cell 2: A water-based slurry was prepared by mixing 97 wt% SiNW-carbon powder with an amorphous carbon layer (9.7 wt% Si), 1.5 wt% CMC, and 1.5 wt% SBR. The slurry was used to coat the anode electrode on a copper foil. The resulting anode exhibited a first delithiation specific capacity of 632.46 mAh / g and an initial coulombic efficiency (ICE) of 91.78%, indicating that the amorphous carbon-coated SiNW-carbon powder anode had a slightly lower delithiation capacity and, therefore, a lower ICE than the uncoated SiNW-carbon powder in half-cell 1.
[0253] Half-cell 3: A slurry was prepared by mixing 97 wt% SiNW-carbon powder (9.7 wt% Si) pretreated with PSAA and carbonized at 700°C under nitrogen. The binder was 1.5 wt% CMC and 1.5 wt% SBR. The anode electrode was coated onto copper foil using the slurry. The resulting anode showed a first delithiation specific capacity of 638.69 mAh / g and an ICE of 91.89%. The lithiation was similar to that of the amorphous carbon-coated SiNW-carbon powder anode from acetylene decomposition in the CVD process. However, the delithiation was better than the amorphous carbon-coated SiNW-carbon powder anode, which resulted in a higher ICE.
[0254] exist Figure 6 In FIG. 1 , the X-axis is the capacity % normalized by the fully lithiation capacity, and the lithiation curves of the three half-unit cells of Example 3 are shown. Figure 6 As shown in , the lithiation curve of carbonized PSAA is similar to that of thermal decomposition of acetylene into an amorphous carbon coating on SiNW-carbon powder. Figure 6 As shown in Figure A, the carbonized PSAA-coated SiNW-carbon anode and the amorphous carbon-coated SiNW-carbon anode are equally promoted by the carbonized layer relative to the uncoated SiNW-carbon anode for their lithiation. Figure 6 As shown in Figure B, the delithiation of the carbonized PSAA-coated SiNW-carbon anode occurs at a lower potential than that of the amorphous carbon-coated SiNW-carbon anode and the uncoated SiNW-carbon anode. Figure 6 As shown in C, the carbonized PSAA-coated SiNW-carbon anode maintains good initial Coulombic efficiency. Figure 6 As shown in , the PSAA-derived carbon coating is more uniform and easier to apply with less waste compared to the more traditional method of acetylene gas thermal decomposition, leading to facilitated delithiation of SiNWs.
[0255] Example 4 - Cycling of a full electrochemical cell (single-sided NCA cathode + single surface treatment without and with PSAA) Single-layer SiNW-carbon powder anode)
[0256] The following reagents are provided:
[0257] 0.0973 kg of silicon nanowires mechanically and conductively attached to uncoated natural graphite particles in 1 kg of Si-C composite material, wherein the Si weight % is equal to 9.73% (hereinafter referred to as SiNW-carbon powder in the examples), the silicon nanowires having a diameter of 20 nm to 100 nm (measured with FESEM), and the graphite particles are composed of D 50= 14 microns of commercially available uncoated natural graphite. Silicon nanowires were grown onto graphite particles using a copper (I) oxide nanoparticle catalyst disposed onto the graphite particles in a CVD reactor using the decomposition of a silane gas precursor as described in U.S. Pat. No. 10,243,207, the entire contents of which are incorporated herein by reference.
[0258] 1000 g of a 11.111 wt % PSAA solution in EtOH (111.11 g of calculated PSAA polymer content), obtained from Sigma-Aldrich with a molecular weight of M n ~1600.
[0259] 888.89 g of ethanol.
[0260] Prepare the following mixture:
[0261] a) 888.89 grams of ethanol were mixed with 111.11 grams of a 11.111 wt % PSAA solution in ethanol in a 5 liter stainless steel container by pushing for 5 minutes to obtain 1000 grams of a diluted PSAA solution containing 111.11 grams of PSAA polymer.
[0262] b) 1 kg of SiNW-carbon powder was immersed in the PSAA solution in a 5 liter container and mixed for 30 minutes to produce a mixture comprising SiNW-carbon powder with PSAA polymer uniformly disposed thereon.
[0263] c) The mixture in the 5 liter container was placed in an oven to dry at a temperature of 40 to 120° C. under nitrogen for about 2 hours to produce 1111.11 grams of dried composite particles having 10% PSAA in the composite. The PSAA coated SiNW-carbon powder formed a powder of individual particles without any grinding or sieving.
[0264] Note that the PSAA content on the surface before the carbonization treatment may be 1 wt % to 80 wt %, or 5 wt % to 30 wt %. In this specific example, 10 wt % of PSAA is used.
[0265] The carbonization process can be carried out in an inert gas environment in a reactor (e.g., flowing N2 at 1.0 LPM / kg of SiNW-carbon powder containing 10% PSAA during the process of raising the reactor temperature to 700°C, then maintaining the temperature at 700°C for 1 hour to complete the carbonization of PSAA, then maintaining the N2 flow to cool the reactor to a temperature below 300°C, and then unloading the treated SiNW-carbon powder from the reactor). The carbonization temperature can be 450°C to 900°C. The carbonization time can be 30 minutes to 5 hours. The N2 flow rate can be varied from 0.1 LPM / kg of SiNW-carbon powder to 5 LPM / kg of SiNW-carbon powder. The purpose of the N2 flow is to remove air / O2 and decomposition gases from the reactor and prevent the carbonized surface coating from being oxidized.
[0266] Because PSAA can be easily and uniformly coated on the SiNW-carbon powder surface, i.e., on both the graphite and Si nanowire surfaces, the carbonized surface coating is also uniform, e.g. Fig. 7A and 7B In the TEM image of , a uniform 1.9 nm coating can be observed on both the Si nanowire surface and the graphite surface after the carbonization treatment, where the Si nanowire has a diameter of 20.7 nm.
[0267] Two groups of NCA pouch cells were prepared, the first group was treated with PSAA carbonization and the second group was not treated.
[0268] a) Add 100 grams of 4 wt% CMC stock solution (in DI water) to a planetary kneader vessel. Keep the vessel at 30°C.
[0269] b) 46 g of SiNW-carbon powder (with carbonized PSAA disposed thereon for the group treated with PSAA carbonization and without PSAA for the group not treated) were gradually added to the mixture obtained from step a). The resulting mixture was mixed in a planetary kneader vessel (non-bubbling kneader, NBK-1) at 400 rpm for 15 minutes.
[0270] c) The slurry obtained from step b) was placed in a 40°C bath for 2 minutes and then mixed again to reach a slurry temperature of 30°C.
[0271] d) For each of the two NCA cells, the slurry obtained from step c) was then used to coat the anode electrode onto a copper foil using a doctor blade, the first one with PSAA carbonization treatment and the second one without. The electrodes were then dried at 90°C for 60 minutes.
[0272] e) After 60 minutes at room temperature, the electrode obtained from step d) was subsequently calendered to 1.4 g cm -3Density (usually 1 to 1.65 g cm -3 density).
[0273] Two sets of electrochemical unit cells were constructed by matching the NCA cathode with a SiNW-carbon powder anode electrode. The SiNW-carbon powder anode electrode was coated with 8 wt% CMC and 92 wt% SiNW-carbon powder containing 9.73 wt% Si. The first set contained the SiNW-carbon powder with carbonized PSAA, and the second set contained the SiNW-carbon powder without any PSAA applied.
[0274] Use as Figure 8 and Fig. 9 The different cycling protocols shown in Figure 5 compare the cycling performance of two sets of electrochemical cells over 500 cycles.
[0275] The electrochemical cell was subjected to a simple formation protocol with C / 20 for the charge current between 0CV and 4.25V and C / 20 for the discharge current between 4.25V and 2.5V. The electrodes were not pre-lithiated. The cell was characterized at C / 10 for one cycle and at C / 5 for another cycle. Subsequently, as Figure 8 As shown in (first cycling scheme), the cells were cycled 500 times at C / 3 for charging and C / 3 for discharging. The cells using untreated anodes showed 71% capacity retention at the 500th cycle. The cells using treated anodes showed better cycling and 74% capacity retention at the 500th cycle. The treatment improved capacity retention during cycling, which resulted in slower capacity fade. Fig. 9 (Second Cycle Scheme), the cell was cycled at C / 3 charge and C / 2 discharge. Every 100 cycles, the cell was used at C / 10 to check its capacity, which resulted in a capacity spike, indicating that the Si nanowires were still electrochemically active, and full capacity was achieved at C / 10. The capacity check of two C / 10 cycles activated the Li ion diffusion channels, so there was a slow decay tail after the capacity spike. As a result, the cell using the untreated anode exhibited a capacity retention of 70.5% at the 500th cycle. The cell using the treated anode showed better cycling and a capacity retention of 75.5% at the 500th cycle. This again shows that the carbonized PSAA surface treatment improves the cycling behavior, which leads to slower capacity decay.
[0276] Example 5 - Cycling of Full Electrochemical Cells (Single-Sided NCA Cathode + Single and Double PSAA Surface Treatments Single-layer SiNW-carbon powder anode)
[0277] Silicon nanowires (wherein the Si weight % is equal to 9.73%) mechanically and conductively attached to commercially available uncoated natural graphite particles were first uniformly coated with 5-20% PSAA (e.g., 20% PSAA) and subsequently carbonized at a temperature of up to 700°C, following the steps described in Example 4. After the carbonization process, a second surface coating was uniformly applied on the carbonized SiNW-carbon powder by using 0.1-5% PSAA (double surface treatment). In this example, 0.3 wt% PSAA was used. The second PSAA coating was applied according to the same procedure described in the previous example, and without carbonization.
[0278] Four sets of electrochemical cells (full cells with SiNW-carbon powder anode and NCA cathode) were prepared to evaluate and compare the full cell performance of different types of anode material and PSAA coating combinations:
[0279] 1) Electrochemical cell using an anode having 8 wt% CMC and 92 wt% SiNW-carbon powder (without surface treatment) with 9.7 wt% Si
[0280] 2) An electrochemical cell using an anode having 8 wt% CMC and 92 wt% SiNW-carbon powder having a Si wt% equal to 9.7% and uniformly coated with a coating (single surface treatment) of 5-20% PSAA (e.g. 20% PSAA) carbonized at a temperature of up to 700°C
[0281] 3) Electrochemical cell using an anode having only 5 wt% CMC, 5 wt% C65 carbon black conductive additive (from IMERYS Graphite & Carbon) and 90 wt% SiNW-carbon powder having a Si wt% equal to 9.7% and uniformly coated with a coating (single surface treatment) of 5-20% PSAA (e.g. 20% PSAA) carbonized at a temperature of up to 700°C
[0282] 4) An electrochemical cell using an anode having only 5 wt% CMC, 5 wt% C65 carbon black conductive additive (from IMERYS Graphite & Carbon) and 90 wt% SiNW-carbon powder having a Si wt% equal to 9.7% and uniformly coated with a first coating of 5-20% PSAA (e.g. 20% PSAA) carbonized at a temperature of up to 700°C and subsequently uniformly coated with a second coating of uncarbonized 0.1-5% PSAA (e.g. 0.3 wt%) (double surface treatment).
[0283] Fig.10An overview of four groups of electrochemical cells is presented in , which summarizes the types of anode materials used in each group and the initial cell performance.
[0284] The electrochemical cell was subjected to a simple formation process at C / 20 for charging between OCV and 4.25V and C / 20 for discharging between 4.25V and 2.5V. There was no pre-lithiation of the anode and cathode. The cell was characterized at C / 10 for one cycle and at C / 5 for another cycle. The cell was cycled 500 times at C / 3 for charging and C / 3 for discharging. Fig.11 and 12 Included are two graphs comparing the specific discharge capacity and capacity retention between a third type of electrochemical cell (single surface treatment with carbonized surface, 5% CMC) and a fourth electrochemical cell (dual surface treatment with 0.3% PSAA coated on the carbonized surface, 5% CMC) as described in the previous paragraph.
[0285] The cycling performance was compared over 500 cycles using different cycling protocols. Fig.11 and 12 The graphs in show the discharge specific capacity and % capacity retention over 500 cycles for an electrochemical cell having a single surface treatment and an electrochemical cell having a dual surface treatment.
[0286] It can be inferred from the graph that the electrochemical cells with dual surface treatments exhibit more stable cycling performance than the electrochemical cells with single surface treatments. As shown in the graph, for those cells with single surface treatments, a reversible capacity of 400 mAh / g is reached after 200 cycles, and for those cells with dual surface treatments, this reversible capacity is reached after 400 cycles.
[0287] The dual surface treatment enables the use of less polymer binder (eg only 5% CMC), which results in improved cell performance stability. Without wishing to be bound by theory, the inventors hypothesize that the dual surface treatment reduces the surface area and stabilizes the interface between the material and the electrolyte.
[0288] These novel PSAA surface coatings according to various aspects of the present invention can be applied to silicon nanowires, graphite particles, or other types of particles (e.g., carbon, metals or their oxides or alloys). These coatings help to make the surfaces of silicon nanowires and graphite particles uniform. Greater surface uniformity improves SEI formation, contributing to better stability and cycle performance. The PSAA coatings according to various aspects of the present invention are inexpensive and provide a convenient way to apply a uniform surface treatment to SiNW-carbon powder materials without using an additional grinding process to break up the powder. According to various aspects of the present invention, the PSAA surface coating uniformly applied to both silicon nanowires and graphite particles can be optionally carbonized to generate a uniform carbon coating for the silicon nanowires and graphite particles, which reduces the need for conductive additives and enhances the interaction (affinity) with different binder polymers in electrode processing.
[0289] While specific embodiments of the invention have been described herein for purposes of reference and illustration, various modifications will become apparent to those skilled in the art without departing from the scope of the invention as defined in the appended claims.
[0290] The description of the embodiments of the present disclosure is not intended to be exhaustive or to limit the present disclosure to the precise form disclosed. Although the specific embodiments and examples of the present disclosure are described herein for the purpose of illustration, various equivalent modifications within the scope of the present disclosure are possible as will be appreciated by those skilled in the relevant art. For example, although method steps or functions are presented in a given order, alternative embodiments may perform functions in different orders, or may perform functions substantially simultaneously. The teachings of the present disclosure provided herein may be appropriately applied to other programs or methods. Various embodiments described herein may be combined to provide further embodiments. If necessary, aspects of the present disclosure may be modified to provide further embodiments of the present disclosure using the compositions, functions and concepts of the above-mentioned references and applications. According to the detailed description, these and other changes may be made to the present disclosure. All such modifications are intended to be included within the scope of the appended claims.
[0291] The specific elements of any of the foregoing embodiments may be combined or substituted for the elements in other embodiments. In addition, although the advantages associated with certain embodiments of the present disclosure have been described in the context of these embodiments, other embodiments may also exhibit such advantages, and not all embodiments must exhibit such advantages to fall within the scope of the present disclosure.
Claims
1. A composite material comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol.
2. The composite material of claim 1, wherein the polymer has a softening point below 200°C.
3. The composite material of claim 1, wherein the polymer is insoluble in water.
4. The composite material of claim 1, wherein the polymer is soluble in alcohol.
5. The composite material of claim 4, wherein the alcohol comprises ethanol.
6. The composite material of claim 1, wherein the polymer is poly(styrene-co-allyl alcohol).
7. The composite material of claim 1, wherein the polymer comprises at least 25 mol% of monomer units derived from allyl alcohol.
8. The composite material of claim 1, wherein said composite material comprises from 0.1 wt% to 10 wt% of said polymer.
9. The composite material of claim 1, wherein said composite material comprises 0.5 wt% to 5 wt% of said polymer.
10. The composite material of claim 1, wherein the plurality of silicon-based nanostructures are silicon nanowires, silicon nanoparticles, or a combination thereof.
11. The composite material of claim 1, wherein the plurality of silicon-based nanostructures are silicon nanowires.
12. The composite material of claim 10, wherein the silicon nanowires have a diameter of 10 nm to 200 nm.
13. The composite material of claim 1, wherein the plurality of silicon-based nanostructures comprises a single crystalline core and a shell layer, wherein the shell layer comprises amorphous silicon, polycrystalline silicon, or a combination thereof.
14. The composite material of claim 1, wherein the composite material comprises at least 90 weight percent silicon-based nanostructures attached to a carbon-based substrate.
15. The composite material of claim 1, wherein the composite material comprises at least 95% by weight of silicon-based nanostructures attached to a carbon-based substrate.
16. The composite material of claim 1, wherein the carbon-based substrate is a carbon-based powder.
17. The composite material of claim 15, wherein the carbon-based powder has a D 50 .
18. The composite material of claim 1, wherein the carbon-based substrate is selected from graphite powder, mesocarbon microbead powder, or a combination thereof.
19. The composite material of claim 1, wherein the carbon-based substrate is graphite powder.
20. The composite material of claim 1, wherein the carbon-based substrate is a graphite powder comprising a plurality of graphite particles, each particle comprising a plurality of pores disposed therein, wherein the silicon-based nanostructures are attached to a surface defining the pores.
21. The composite material of claim 1, wherein the carbon-based substrate is a graphite powder comprising uncoated natural graphite particles.
22. The composite material of claim 1, wherein the plurality of silicon-based nanostructures attached to the carbon-based substrate comprises 1 wt% to 40 wt% silicon.
23. The composite material of claim 1, wherein the plurality of silicon-based nanostructures attached to the carbon-based substrate comprises 2.5 wt% to 25 wt% silicon.
24. The composite material of claim 23, wherein the plurality of silicon-based nanostructures attached to the carbon-based substrate comprises 5 wt% to 15 wt% silicon.
25. The composite material of claim 1, wherein the plurality of silicon-based nanostructures and the carbon-based substrate further comprise a conductive carbon coating, wherein a polymer comprising monomer units formed from styrene and allyl alcohol is disposed on the conductive carbon coating.
26. The composite material of claim 25, wherein the conductive carbon coating comprises carbonized PSAA.
27. The composite material of claim 26, wherein the conductive carbon coating is provided as an inner coating on the plurality of silicon-based nanostructures and the carbon-based substrate, and a polymer comprising monomer units formed of styrene and allyl alcohol is provided as an outer coating on the plurality of silicon-based nanostructures and the carbon-based substrate.
28. A method for preparing a composite material, the method comprising: mix: a plurality of silicon-based nanostructures attached to a carbon-based substrate, and a solution of a polymer comprising monomer units formed from styrene and allyl alcohol; and The mixture resulting from said mixing is dried.
29. The method of claim 27, wherein the solution of the polymer comprises the polymer and an alcohol solvent.
30. The method of claim 29, wherein the alcohol solvent comprises ethanol.
31. The method of claim 27, wherein the solution of polymer does not contain water.
32. The method of claim 27, wherein the solution comprises 0.05 wt% to 10 wt% of the polymer.
33. The method of claim 27, wherein the solution comprises 0.1 wt% to 3 wt% of the polymer.
34. The method of claim 33, wherein the solution comprises (e.g., 0.5% to 1.5% by weight) of the polymer.
35. The method of claim 27, wherein the drying is carried out at a temperature of 20°C to 150°C, at ambient pressure or under reduced pressure (eg, under vacuum).
36. The method of claim 35, wherein the drying is performed under vacuum.
37. The method of claim 27, wherein the drying is performed at a temperature of 30°C to 130°C.
38. The method of claim 37, wherein the drying is performed under an inert gas.
39. The method of claim 38, wherein the drying is performed under nitrogen.
40. The method of claim 27, wherein the plurality of silicon-based nanostructures attached to the carbon-based substrate comprises a conductive carbon coating.
41. The method of claim 40, wherein the conductive carbon coating is formed by carbonizing a polymer coating previously disposed on the silicon-based nanostructures and the carbon-based substrate.
42. The method of claim 41, wherein the polymer coating pre-disposed on the silicon-based nanostructures and the carbon-based substrate is a polymer comprising monomer units formed from styrene and allyl alcohol.
43. The method of claim 41, wherein carbonizing the polymer coating pre-disposed on the silicon-based nanostructure and the carbon-based substrate comprises heating the silicon-based nanostructure and the carbon-based substrate having the polymer coating pre-disposed thereon at a temperature of 200°C to 750°C.
44. The method of claim 43, wherein the heating is performed at a temperature of 500°C to 750°C.
45. The method of claim 43, wherein the heating is performed under an inert gas.
46. The method of claim 45, wherein the heating is performed under nitrogen.
47. An anode electrode comprising a first anode layer comprising a binder and a composite material comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol.
48. The anode electrode of claim 47, wherein the binder is selected from styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), poly(vinylidene fluoride) (PVDF), poly(acrylic acid) (PAA), poly(acrylonitrile) (PAN), poly(acrylamide-co-diallyldimethylammonium) (PAADAA), poly(tetrafluoroethylene) (PTFE), and combinations of two or more thereof.
49. The anode electrode of claim 47, wherein the binder is a mixture of styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC).
50. The anode electrode of claim 49, wherein the binder comprises 30 to 70 wt% of butadiene rubber (SBR) and 30 to 70 wt% of carboxymethyl cellulose (CMC).
51. The anode electrode of claim 47, wherein the binder is poly(tetrafluoroethylene) (PTFE).
52. The anode electrode of claim 47, wherein the first anode layer comprises 0.5 wt% to 10 wt% of the binder.
53. The anode electrode of claim 47, wherein the first anode layer comprises 1 wt% to 6 wt% of the binder.
54. The anode electrode of claim 47, wherein said first anode layer comprises at least 90% by weight of said composite material.
55. The anode electrode of claim 47, wherein the first anode layer further comprises a conductive additive.
56. The anode electrode of claim 55, wherein the first anode layer comprises 0.2 wt% to 5 wt% of the conductive additive.
57. The anode electrode of claim 55, wherein the conductive additive is selected from the group consisting of carbon black particles, carbon nanofibers, carbon nanotubes, and combinations of two or more thereof.
58. The anode electrode of claim 47, wherein the anode electrode further comprises a current collector.
59. The anode electrode of claim 58, wherein the current collector is a copper foil or a carbon-coated copper foil.
60. The anode electrode of claim 47, further comprising one or more additional anode layers, each additional anode layer independently comprising an active material and a binder.
61. The anode electrode of claim 60, wherein the first anode layer comprises a first surface configured to contact (or be in contact with) a current collector and a second surface in contact with the one or more additional anode layers.
62. The anode electrode of claim 61, wherein the first anode layer comprises a first surface contacting a current collector.
63. The anode electrode of claim 61, wherein the second surface of the first anode layer comprises metallic lithium disposed thereon.
64. The anode electrode of claim 63, wherein the metallic lithium is selected from the group consisting of lithium metal foil, stabilized lithium metal powder, and combinations thereof.
65. The anode electrode of claim 60, wherein the active material is selected from graphite powder, a plurality of silicon-based nanostructures attached to a carbon-based substrate, a composite material comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol, and combinations of two or more thereof.
66. The anode electrode of claim 65, wherein at least one of the one or more additional anode layers further comprises a conductive additive, wherein the conductive additive is selected from the group consisting of carbon black particles, carbon nanofibers, carbon nanotubes, and combinations of two or more thereof.
67. A method for preparing an anode electrode, the method comprising: mix: A composite material comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol, and a binder to form a mixture; and A layer of the mixture is applied.
68. The method of claim 67, wherein the layer is configured to contact a current collector.
69. The method of claim 67, wherein the mixture is provided as a wet slurry and the method further comprises drying the layer.
70. The method of claim 67, wherein the mixture is provided as a solid and the applying comprises forming a layer of the solid mixture.
71. The method of claim 70, wherein said forming comprises extruding or calendering.
72. The method of claim 67, wherein said applying comprises applying a layer of said mixture onto a current collector.
73. The method of claim 72, further comprising applying one or more additional anode layers onto the layer, wherein the one or more additional anode layers each independently comprise an active material and a binder.
74. The method of claim 73, wherein the active material is selected from the group consisting of graphite powder, a plurality of silicon-based nanostructures attached to a carbon-based substrate, a composite material comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol, and combinations of two or more thereof.
75. The method of claim 74, wherein at least one of the one or more additional anode layers further comprises a conductive additive, wherein the conductive additive is selected from the group consisting of carbon black particles, carbon nanofibers, carbon nanotubes, and combinations of two or more thereof.
76. A battery comprising: A composite material comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol.
77. The battery of claim 76, wherein the battery is a lithium ion battery.
78. A battery comprising: An anode electrode comprising a first anode layer comprising a binder and a composite material comprising a plurality of silicon-based nanostructures attached to a carbon-based substrate, the plurality of silicon-based nanostructures and the carbon-based substrate having a polymer disposed thereon, wherein the polymer comprises monomer units formed from styrene and allyl alcohol.
79. The battery of claim 78, wherein the battery is a lithium ion battery.
Citation Information
Patent Citations
Nanostructured battery active materials and methods of producing same
US10243207B2
Compacted carbon for electrochemical cells
US5677082A
Resin useful for resist, resist composition and pattern forming process using the same
US6303266B1
Carbon electrode material
US6479030B1
Silicon nanostructure active materials for lithium ion batteries and processes, compositions, components and devices related thereto
US9812699B2