Preparation method of octenal liquid phase hydrogenation catalyst
Preparation by using specific ratios of Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, Al(NO3)3·9H2O and Na2CO3 and NaOH in the octenal liquid phase hydrogenation catalyst, the preparation of the drop funnel was prepared. The production of high-activity and high-selectivity catalyst precursors solves the problems of low activity and low selectivity of existing catalysts and achieves efficient preparation of octanol.
Patent Information
- Application Number
- CN202310497405.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-05-05
AI Technical Summary
The existing octenal liquid hydrogenation catalyst has low activity and low selectivity, and the impurity content of octanol products after hydrogenation is high.
Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, Al(NO3)3·9H2O, Na2CO3 and NaOH were prepared in a specific proportion. The solution was added dropwise to a constant temperature water bath through a dropping funnel to react and precipitate. After washing, calcining and reducing activation, catalyst precursors with high catalytic hydrogenation activity and high product selectivity were prepared.
The characteristics of high catalytic hydrogenation activity and high selectivity of product octanol are achieved, and the problems of low activity and low selectivity of existing catalysts are overcome.
Smart Images

Figure CN118892833A_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of catalyst preparation, and in particular to a method for preparing an octenal liquid phase hydrogenation catalyst. Background technology:
[0002] Chinese patents CN105080549A and CN105080549B disclose a catalyst for preparing 2-ethylhexanol by gas phase hydrogenation of octenal and its preparation method. A highly selective octenal hydrogenation catalyst prepared by distributed precipitation is proposed, which solves the problem of easy pulverization of the catalyst during use. The catalyst is mainly composed of 25% to 35% copper oxide, 45% to 60% zinc oxide, 2% to 10% aluminum oxide, 2% to 10% silicon dioxide, and 0.01% to 1% additive. The specific surface area of the catalyst is 30m 2 / g~60m 2 / g, pore volume is 0.17mL / g~0.30mL / g, and average pore radius is 5nm~10nm. The catalyst prepared by the inventive method has high activity and 2-ethylhexanol selectivity, and has better use strength and lower color number, and is suitable for the reaction process of octenal gas phase hydrogenation to 2-ethylhexanol.
[0003] Chinese patent CN114082421A discloses a hydrogenation catalyst and its preparation method and application in isooctene aldehyde hydrogenation. The hydrogenation catalyst comprises a carrier and an active component loaded on the carrier, wherein the carrier is alumina and / or phosphorus-modified alumina, and the active component is nickel; the specific surface area of the hydrogenation catalyst is 200 to 630 m 2 / g, pore volume is 2~4cm 3 / g, and the most probable pore size is 10-30nm. The hydrogenation catalyst is applied to the hydrogenation of isooctylaldehyde to isooctylaldehyde and isooctyl alcohol, which can improve the catalytic activity and selectivity.
[0004] Chinese patent CN105854919A discloses a low-temperature hydrogenation catalyst for α,β# unsaturated aldehydes and its preparation method and application. The catalyst described in the present invention is a hexagonal boron nitride-supported precious metal catalyst, which is prepared by impregnating an active precious metal salt on a pretreated carrier and reducing it. Through the fine control and effective combination of carrier pretreatment, impregnation and reduction treatment, the active component can be effectively dispersed on the carrier, and good performance is shown when the content of the precious metal active component is low.
[0005] Chinese patent CN1478596A discloses a process for preparing isooctyl alcohol by hydrogenating a mixture of isooctyl aldehyde and a catalyst used therein, and particularly relates to a process for preparing isooctyl alcohol by liquid phase hydrogenation of a mixture of isooctyl aldehyde and octenol using a novel catalyst and a catalyst used therein. The catalyst uses metal nickel as an active component, alkaline earth metal oxides and / or aluminum oxide as a promoter, and a silicon-containing compound as a carrier. The raw material of the carrier is a porous silicon-containing compound and / or a silicon-containing compound that is viscous in an aqueous solution; the active component nickel is loaded on the carrier in the form of coprecipitation, kneading, or coprecipitation-kneading with the carrier, and is prepared by roasting at 300-800°C. Summary of the invention:
[0006] The technical problem to be solved by the present invention is to provide a method for preparing an octenal liquid phase hydrogenation catalyst, wherein the method realizes that the prepared catalyst precursor is used for the octenal liquid phase hydrogenation to octanol reaction after reduction activation, and has the characteristics of high catalytic hydrogenation activity and high selectivity for the product octanol, thereby overcoming the shortcomings of the existing octenal liquid phase hydrogenation catalyst, such as low activity and selectivity, and high impurity content of the octanol product after hydrogenation.
[0007] The technical solution adopted by the present invention is: a method for preparing an octenal liquid phase hydrogenation catalyst, the method comprising the following steps:
[0008] Step 1: Ni(NO3)2·6H2O, Cu(NO3)2·3H2O and Al(NO3)3·9H2O are mixed uniformly according to the amount of substances to prepare solution a;
[0009] Step 2: Mix Na2CO3 and NaOH according to the amount of substance to prepare solution b;
[0010] Step 3: Place the prepared solution a and solution b in a dropping funnel respectively, and use the dropping funnel to drop the two solutions into a three-necked flask placed in a constant temperature water bath at 60°C to 80°C, and react under constant stirring;
[0011] Step 4: After aging for 2 h to 12 h, the precipitate is filtered and washed with distilled water, and then dried and calcined to obtain a catalyst precursor.
[0012] Furthermore, the molar ratio of Ni(NO3)2·6H2O, Cu(NO3)2·3H2O and Al(NO3)3·9H2O in step one is x:y:6, wherein x+y+6=10.
[0013] Furthermore, the molar ratio of Na2CO3 to NaOH in step 2 is 5:1 to 9:1.
[0014] Furthermore, after the solution a in step three reacts with the solution b, the pH value of the solution is controlled to be 9-10.
[0015] Furthermore, in the step 4, the precipitate after the reaction of solution a and solution b is filtered and washed until the upper layer of washing liquid is neutral.
[0016] Furthermore, in the step 4, the precipitate is filtered and washed with distilled water, dried in an oven at 120° C., and calcined in a muffle furnace at 500° C.
[0017] Furthermore, the reduction activation conditions of the prepared catalyst precursor are: reduction at a constant temperature of 500° C. for 12 h in a mixed gas with a hydrogen-nitrogen flow rate of 1:3.
[0018] The beneficial effect of the present invention is that the catalyst precursor prepared by the present invention is used for the liquid phase hydrogenation of octenal to produce octanol after reduction activation, and has the characteristics of high catalytic hydrogenation activity and high selectivity for product octanol. Description of the drawings:
[0019] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0020] Figure 1 This is the H2-TPR diagram of the catalyst in Example 1. Specific implementation method:
[0021] Comparative Example 1
[0022] Ni(NO3)2·6H2O and Cu(NO3)2·3H2O were prepared into solution a in a molar ratio of 3:1, and equal volumes were impregnated on γ-Al2O3 (Ni, Cu, Al molar ratio was 3:1:6). After standing for 24 h, it was dried in an oven at 120°C and then calcined in a muffle furnace at 500°C to obtain catalyst precursor X.
[0023] Example 1
[0024] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly in a molar ratio of 3:1:6 to prepare solution a, and then a mixed solution b with a molar ratio of Na2CO3 and NaOH of 7:1 was prepared. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a 65°C constant temperature water bath using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 6 hours, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor A.
[0025] Example 2
[0026] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly in a molar ratio of 4:0:6 to prepare solution a, and then a mixed solution b with a molar ratio of Na2CO3 and NaOH of 7:1 was prepared. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a 65°C constant temperature water bath using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 6 hours, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor B.
[0027] Example 3
[0028] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly in a molar ratio of 2:2:6 to prepare solution a, and then a mixed solution b was prepared in a molar ratio of 7:1 between Na2CO3 and NaOH. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a 65°C constant temperature water bath using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 6 hours, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor C.
[0029] Example 4
[0030] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly at a molar ratio of 0:4:6 to prepare solution a, and then a mixed solution b with a molar ratio of Na2CO3 and NaOH of 7:1 was prepared. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a 65°C constant temperature water bath using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 6 hours, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor D.
[0031] Example 5
[0032] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly in a molar ratio of 3:1:6 to prepare solution a, and then a mixed solution b was prepared in a molar ratio of 5:1 between Na2CO3 and NaOH. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a 65°C constant temperature water bath using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 6 hours, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor E.
[0033] Example 6
[0034] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly in a molar ratio of 3:1:6 to prepare solution a, and then a mixed solution b with a molar ratio of Na2CO3 and NaOH of 9:1 was prepared. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a 65°C constant temperature water bath using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 6 hours, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor F.
[0035] Example 7
[0036] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly in a molar ratio of 3:1:6 to prepare solution a, and then a mixed solution b with a molar ratio of Na2CO3 and NaOH of 7:1 was prepared. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a 60°C constant temperature water bath using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 6 hours, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor G.
[0037] Example 8
[0038] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly in a molar ratio of 3:1:6 to prepare solution a, and then a mixed solution b with a molar ratio of Na2CO3 and NaOH of 7:1 was prepared. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a constant temperature water bath at 80°C using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 6 hours, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor H.
[0039] Example 9
[0040] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly in a molar ratio of 3:1:6 to prepare solution a, and then a mixed solution b with a molar ratio of Na2CO3 and NaOH of 7:1 was prepared. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a 65°C constant temperature water bath using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 2h, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor I.
[0041] Example 10
[0042] First, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Al(NO3)3·9H2O were mixed uniformly in a molar ratio of 3:1:6 to prepare solution a, and then a mixed solution b with a molar ratio of Na2CO3 and NaOH of 7:1 was prepared. The prepared solution a and solution b were placed in a dropping funnel respectively, and the two solutions were added drop by drop into a three-necked flask placed in a 65°C constant temperature water bath using a dropping funnel, and the pH of the mixed solution was kept stirred to 9-10. After aging for 12 hours, the precipitate was filtered and washed until the upper washing liquid was neutral, dried in an oven at 120°C, and then calcined at 500°C in a muffle furnace to obtain catalyst precursor J.
[0043] The catalyst precursors prepared in Comparative Example 1 and Examples 1-10 were activated by reduction and then used for the liquid phase hydrogenation of octenal to produce octanol at mild conditions of 120° C. to 130° C. The reaction performance is shown in Table 1.
[0044] Table 1 Octenal liquid phase hydrogenation performance of catalysts
[0045] catalyst Octenal conversion rate (%) Octanol selectivity (%) A 99.9 99.7 B 90.6 98.0 C 96.7 98.8 D 81.2 89.9 E 95.4 99.0 F 94.3 99.2 G 98.2 99.6 H 97.9 99.5 I 96.8 99.0 J 99.4 99.6 X 87.3 97.6
[0046] As shown in Table 1, the catalyst prepared by the present invention has the characteristics of high catalytic hydrogenation activity and high selectivity for the product octanol.
[0047] It can be understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.
Claims
1. A method for preparing an octenal liquid phase hydrogenation catalyst, characterized in that: The steps of this method are as follows: Step 1: Mix Ni(NO3)2·6H2O, Cu(NO3)2·3H2O and Al(NO3)3·9H2O according to the amount of substances to prepare solution a; Step 2: Mix Na2CO3 and NaOH according to the amount of substance to prepare solution b; Step 3: Place the prepared solution a and solution b in a dropping funnel respectively, and use the dropping funnel to drop the two solutions into a three-necked flask placed in a constant temperature water bath at 60°C to 80°C, and react under constant stirring; Step 4: After aging for 2 h to 12 h, the precipitate is filtered and washed with distilled water, and then dried and calcined to obtain a catalyst precursor.
2. The method for preparing the octenal liquid phase hydrogenation catalyst according to claim 1, wherein: The molar ratio of Ni(NO3)2·6H2O, Cu(NO3)2·3H2O and Al(NO3)3·9H2O in step 1 is x:y:6, wherein x+y+6=10.
3. The preparation method of the octenal liquid phase hydrogenation catalyst according to claim 1, characterized in that: The molar ratio of Na2CO3 to NaOH in step 2 is 5:1 to 9:
1.
4. The method for preparing the octenal liquid phase hydrogenation catalyst according to claim 1, wherein: After the solution a in step 3 reacts with the solution b, the pH value of the solution is controlled to be 9-10.
5. The method for preparing the octenal liquid phase hydrogenation catalyst according to claim 1, wherein: In the step 4, the precipitate after the reaction of solution a and solution b is filtered and washed until the upper washing liquid is neutral.
6. The method for preparing the octenal liquid phase hydrogenation catalyst according to claim 1, wherein: In the step 4, the precipitate is filtered and washed with distilled water, dried in an oven at 120° C., and calcined in a muffle furnace at 500° C.
7. The method for preparing the octenal liquid phase hydrogenation catalyst according to claim 1, characterized in that: The reduction activation conditions of the prepared catalyst precursor are: reduction at a constant temperature of 500° C. for 12 hours in a mixed gas with a hydrogen-nitrogen flow rate of 1:3.
Citation Information
Patent Citations
Preparation method of octylene aldehyde gas phase hydrogenation catalyst for octanol production
CN102407122A
Catalyst for hydrogenating octenal gas phase to prepare octanol and preparation method of catalyst
CN104549304A
Preparation method, product and application of Cu-Ni / Al2O3 catalyst
CN106179351A
High-efficiency catalyst for preparing butanedioic anhydride through maleic anhydride hydrogenation and preparation method of high-efficiency catalyst
CN111841551A
NiCu alloy hydrogenation catalyst as well as preparation method and application thereof
CN112569944A