Laser bonding of coated glass to foil

By using a multi-layer anti-reflective coating with an extended wavelength range in the laser bonding of glass and metal foil, the problem of unsuccessful bonding when the laser inclination angle is incident is solved, and successful bonding and airtight sealing of glass and metal foil are achieved.

CN118893306APending Publication Date: 2024-11-05CORNING INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410547188.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2024-05-06
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

When the laser enters the anti-reflective (AR) coating at an inclination angle, the spectral response of the AR coating may shift, resulting in unsuccessful laser bonding of the glass and metal foil.

Method used

An anti-reflective coating with an extended wavelength range is used to ensure that the inclined wavelength range includes the wavelength of the laser beam, thereby achieving successful bonding of glass and metal foil at an inclined angle. The coating consists of alternating a plurality of low and high refractive index layers with a refractive index difference of greater than 0.01 and maintains an average reflectance of less than or equal to about 5% in the inclined wavelength range.

Benefits of technology

It effectively solves the problem of unsuccessful bonding when the laser enters the AR coating at an inclination angle, ensures the airtight sealing bonding of glass and metal foil, and improves the display properties and sealing of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893306A_ABST
    Figure CN118893306A_ABST
Patent Text Reader

Abstract

A method of laser bonding a glass to a metal foil includes applying an anti-reflective coating to a first surface of a glass substrate; contacting the second surface of the glass substrate with the metal foil to create a first contact position between the second surface of the glass substrate and the metal foil; disposing a metal foil optically downstream of the first glass substrate; and performing a first welding step to join the first surface of the glass substrate to the metal foil by directing the laser beam at an inclination angle with respect to the first surface of the glass substrate, in which: the anti-reflective coating has an inclination wavelength range corresponding to the inclination angle at which the laser beam is aligned with the first surface of the glass substrate; the anti-reflective coating has an average reflectance of less than or equal to about 5% throughout the tilted wavelength range, and the tilted wavelength range includes a wavelength of the laser beam.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims the benefit of priority under 35 U.S.C. §120 to U.S. Provisional Application Serial No. 63 / 464,272, filed on May 5, 2023, the contents of which are based and are incorporated herein by reference in their entirety. Technical Field

[0002] The present description relates generally to glass bonding to foil and, more particularly, to laser bonding of coated glass to foil at an oblique angle. Background Art

[0003] Hermetically bonded glass and metal foil packages are becoming increasingly popular for electronic devices and other equipment that can benefit from a hermetic environment for continued operation. In consumer electronics applications, an anti-reflective (AR) coating can be applied to the glass to improve display properties. However, when laser light enters the AR coating at an oblique angle (i.e., non-normal incidence angle), the spectral response (or performance) of the AR coating may shift, resulting in unsuccessful bonding.

[0004] Accordingly, an alternative method is needed to produce laser-bonded AR-coated glass and foil packages. Summary of the invention

[0005] According to a first aspect A1, a method for laser bonding glass to a metal foil may include: applying an anti-reflective coating to a first surface of a first glass substrate, the first glass substrate having a second surface opposite to the first surface; contacting the second surface of the first glass substrate with the first surface of the first foil to create a first contact location between at least a portion of the second surface of the first glass substrate and the first surface of the first foil; arranging the first surface of the first foil optically downstream of the first glass substrate; and performing a welding step by directing a laser beam having a first wavelength at an inclined angle relative to the first surface of the first glass substrate and at least a portion of the first contact location to bond the second surface of the first glass substrate to the first foil, wherein: the anti-reflective coating has an inclined wavelength range corresponding to the inclined angle, at which the anti-reflective coating has an average reflectivity of less than or equal to about 5% over the entire inclined wavelength range, and the inclined wavelength range includes the wavelength of the laser beam.

[0006] A second aspect A2 comprises the method according to the first aspect A1, wherein the antireflective coating has an average reflectivity of less than or equal to about 4% over the entire tilted wavelength range.

[0007] A third aspect A3 comprises the method according to the first aspect A1, wherein the antireflective coating has an average reflectivity of less than or equal to about 3% over the entire tilted wavelength range.

[0008] The fourth aspect A4 includes the method according to the first aspect A1 to the third aspect A3, wherein the tilted wavelength range may be greater than or equal to 375 nm and less than or equal to 700 nm.

[0009] A fifth aspect A5 includes a method according to any one of the first to fourth aspects A1-A4, wherein the antireflective coating may include a plurality of layers, wherein the plurality of layers may include a first low refractive index layer and a second high refractive index layer.

[0010] The sixth aspect A6 includes the method according to the fifth aspect A5, wherein the refractive index difference between the first low refractive index layer and the second high refractive index layer may be greater than or equal to 0.01.

[0011] The seventh aspect A7 includes the method according to the fifth aspect A5 or the sixth aspect A6, wherein the first low refractive index layer may have a refractive index greater than or equal to 1.3 and less than or equal to 1.7.

[0012] An eighth aspect A8 includes the method according to any one of the fifth to seventh aspects A5-A7, wherein the second high refractive index layer may have a refractive index greater than 1.7.

[0013] A ninth aspect A9 includes a method according to any one of the fifth to eighth aspects A5-A8, wherein the first low refractive index layer may include SiO2, Al2O3, GeO2, SiO, AlO x N y 、SiO x N y 、Si u Al v O x N y , MgO, MgAl2O4, MgF2, BaF2, CaF2, DyF3, YbF3, YF3 and CeF3 or a combination thereof.

[0014] A tenth aspect A10 includes the method according to any one of the fifth to ninth aspects A5-A9, wherein the second high refractive index layer may include Si u AlvOxNy, Ta2O5, Nb2O5, AlN, Si3N4, AlO x N y 、SiO x N y , HfO2, TiO2, ZrO2, Y2O3, Al2O3, MoO3, diamond-like carbon, or a combination thereof.

[0015] An eleventh aspect A11 includes the method according to any one of the fifth to tenth aspects A5-A10, wherein the antireflective coating may include a plurality of periods such that first low refractive index layers and second high refractive index layers alternate.

[0016] A twelfth aspect A12 includes the method according to the eleventh aspect A11, wherein the antireflective coating may include greater than or equal to 2 and less than or equal to 20 periods.

[0017] The thirteenth aspect A13 includes the method according to any one of the first to twelfth aspects A1-A12, wherein the tilt angle incident on the first surface of the first glass substrate may be greater than 0° and less than or equal to 60°.

[0018] A fourteenth aspect A14 includes the method according to any one of the first to thirteenth aspects A1-A13, wherein the laser beam may include a pulsed laser.

[0019] The fifteenth aspect A15 includes the method according to the fourteenth aspect A14, wherein the pulse laser can be a nanosecond pulse laser, a picosecond pulse laser, or a femtosecond pulse laser.

[0020] The sixteenth aspect A16 includes a method according to the fourteenth aspect A14 or the fifteenth aspect A15, wherein the pulsed laser may include: a pulse energy greater than or equal to 2.8 μJ and less than or equal to 1000 μJ; a wavelength greater than or equal to 300 nm and less than or equal to 1100 nm; a repetition rate greater than or equal to 5 kHz and less than or equal to 1 MHz; and a spot size greater than or equal to 5 μm and less than or equal to 50 μm.

[0021] The seventeenth aspect A17 includes the method according to any one of the first to sixteenth aspects A1-A16, wherein the first foil may include aluminum, aluminum alloy, stainless steel, nickel, nickel alloy, silver, silver alloy, titanium, titanium alloy, tungsten, tungsten alloy, gold, gold alloy, copper, copper alloy, bronze, iron, or a combination thereof.

[0022] An eighteenth aspect A18 includes the method according to any one of the first to seventeenth aspects A1-A17, wherein the first foil may include a thickness greater than or equal to 5 μm and less than or equal to 75 μm.

[0023] The nineteenth aspect A19 includes the method according to any one of the first to eighteenth aspects A1-A18, wherein the first glass substrate may include a refractive index greater than or equal to 1.5 and less than or equal to 2.4.

[0024] The twentieth aspect A20 includes a method according to any one of the first to nineteenth aspects A1-A19, wherein the first glass substrate may include glass or glass ceramics, and the glass or glass ceramics include borate glass, borosilicate glass, phosphate-based glass, silicon carbide glass, soda-lime silicate glass, aluminosilicate glass, alkali aluminosilicate glass, borosilicate glass, alkali borosilicate glass, aluminoborosilicate glass, alkali aluminoborosilicate glass, alkali aluminosilicate glass or niobium tungsten lanthanum boron glass.

[0025] According to aspect A21, a welding product may include: a first glass substrate, the first glass substrate including a first surface and a second surface opposite to the first surface; an anti-reflection coating, the anti-reflection coating is arranged on the first surface of the first glass substrate, and the anti-reflection coating has a wavelength range; a first foil, the first foil is arranged on the second surface of the glass substrate; and a first interface weld, the first interface weld is between the first surface of the metal foil and the second surface of the glass substrate.

[0026] The twenty-second aspect A22 includes the welded article according to the twenty-first aspect A21, wherein the welded article can be a hermetically sealed package.

[0027] The twenty-third aspect A23 includes the welded article according to the twenty-first aspect A21 or the twenty-second aspect A22, wherein the wavelength range may be greater than or equal to 400 nm and less than or equal to 850 nm.

[0028] Aspect Twenty-four A24 includes a welded product according to any one of Aspects Twenty-one to Twenty-third A21-A23, wherein: the anti-reflective coating may have an inclined wavelength range corresponding to light incident at an inclined angle relative to the first surface of the first glass substrate, and the inclined wavelength range is greater than or equal to 375nm and less than or equal to 700nm.

[0029] The twenty-fifth aspect A25 includes the welded article according to any one of the twenty-first to twenty-fourth aspects A21-A24, wherein the antireflective coating may include a plurality of layers, wherein the plurality of layers includes a first low refractive index layer and a second high refractive index layer.

[0030] The twenty-sixth aspect A26 includes the welded article according to the twenty-fifth aspect A25, wherein the refractive index difference between the first low refractive index layer and the second high refractive index layer may be greater than or equal to 0.01.

[0031] The twenty-seventh aspect A27 includes the welded article according to the twenty-fifth aspect A25 or the twenty-sixth aspect A26, wherein the first low refractive index layer may have a refractive index greater than or equal to 1.3 and less than or equal to 1.7.

[0032] The twenty-eighth aspect A28 includes the welded article according to any one of the twenty-fifth to twenty-seventh aspects A25-A27, wherein the second high refractive index layer may have a refractive index greater than 1.7.

[0033] The twenty-ninth aspect A29 includes the welded article according to any one of the twenty-fifth to twenty-eighth aspects A25-A28, wherein the first low refractive index layer may include SiO2, Al2O3, GeO2, SiO, AlO x N y 、SiOx N y 、Si u Al v O x N y , MgO, MgAl2O4, MgF2, BaF2, CaF2, DyF3, YbF3, YF3 and CeF3 or a combination thereof.

[0034] The 30th aspect A30 includes the welded article according to any one of the 25th to 29th aspects A25-A29, wherein the second high refractive index layer may include Si u AlvOxNy, Ta2O5, Nb2O5, AlN, Si3N4, AlO x N y 、SiO x N y , HfO2, TiO2, ZrO2, Y2O3, Al2O3, MoO3, diamond-like carbon, or a combination thereof.

[0035] A thirty-first aspect A31 includes the welded article according to any one of aspects A25-A30 to A25-A30, wherein the antireflective coating may include a plurality of periods such that first low refractive index layers and second high refractive index layers alternate.

[0036] The thirty-second aspect A32 includes the soldered article according to any one of aspects A25-A31 to A25-A31, wherein the antireflective coating may include 2 to 20 periods.

[0037] The thirty-third aspect A33 includes a welded article according to any one of aspects A21-A32 to A33, wherein the first foil may include aluminum, aluminum alloy, stainless steel, nickel, nickel alloy, silver, silver alloy, titanium, titanium alloy, tungsten, tungsten alloy, gold, gold alloy, copper, copper alloy, bronze, iron, or a combination thereof.

[0038] The thirty-fourth aspect A34 includes the welded article according to any one of the twenty-first to thirty-third aspects A21-A33, wherein the first foil may include a thickness greater than or equal to 5 μm and less than or equal to 75 μm.

[0039] The thirty-fifth aspect A35 includes the welded article according to any one of the twenty-first to thirty-fourth aspects A21-A34, wherein the first glass substrate may include a refractive index greater than or equal to 1.5 and less than or equal to 2.4.

[0040] Aspect thirty-six A36 includes a welding product according to any one of Aspects twenty-one to thirty-fifth A21-A35, wherein the first glass substrate may include glass or glass ceramics, and the glass or glass ceramics include borate glass, borosilicate glass, phosphate-based glass, silicon carbide glass, soda-lime silicate glass, aluminosilicate glass, alkali aluminosilicate glass, borosilicate glass, alkali borosilicate glass, aluminoborosilicate glass, alkali aluminoborosilicate glass, alkali aluminoborosilicate glass or niobium tungsten lanthanum boron glass.

[0041] Additional features and advantages of the laser joining method described herein will be set forth in the following detailed description, and will become apparent in part to those skilled in the art from the description, or may be recognized by practicing the embodiments described herein (including the following detailed description, claims, and drawings).

[0042] It should be understood that both the above general description and the following detailed description describe various embodiments, and that they are intended to provide an overview or framework for understanding the nature and character of the claimed subject matter. The accompanying drawings are included to provide a further understanding of the various embodiments, and are incorporated into and constitute a part of this specification. The accompanying drawings illustrate various embodiments described herein, and together with the description, serve to explain the principles and operation of the claimed subject matter. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 is a flow chart of a method of laser bonding glass to metal foil according to one or more embodiments shown and described herein;

[0044] Figure 2 schematically depicts steps of a method according to one or more embodiments shown and described herein;

[0045] Figure 3 schematically depicts a side view of an antireflective coating according to one or more embodiments shown and described herein;

[0046] Figure 4 schematically depicts a side view of another antireflective coating according to one or more embodiments shown and described herein;

[0047] Figure 5 schematically depicts a side view of another antireflective coating according to one or more embodiments shown and described herein;

[0048] Figure 6 schematically depicts a side view of another antireflective coating according to one or more embodiments shown and described herein;

[0049] Figure 7schematically depicts another step of a method according to one or more embodiments shown and described herein;

[0050] Figure 8 schematically depicts another step of a method according to one or more embodiments shown and described herein;

[0051] Fig. 9 schematically depicts another step of a method according to one or more embodiments shown and described herein;

[0052] Fig.10 schematically depicts another step of a method according to one or more embodiments shown and described herein;

[0053] Fig.11 schematically depicts another step of a method according to one or more embodiments shown and described herein;

[0054] Fig.12 is a flow chart of a method of producing a hermetically sealed package having a foil bonded to a coated glass at an oblique angle according to one or more embodiments shown and described herein;

[0055] Fig.13 schematically depicts steps of a method according to one or more embodiments shown and described herein;

[0056] Fig.14 schematically depicts another step of a method according to one or more embodiments shown and described herein;

[0057] Fig.15 schematically depicts another step of a method according to one or more embodiments shown and described herein;

[0058] Fig.16 schematically depicts another step of a method according to one or more embodiments shown and described herein;

[0059] Fig.17 is a graph of reflectivity versus wavelength (y-axis: reflectivity (%); x-axis: wavelength (nm)) depicting the reflectivity of light with average polarization incident on an AR coating at several angles according to one or more embodiments shown and described herein;

[0060] Fig.18 is a graph of reflectivity versus wavelength (y-axis: reflectivity (%); x-axis: wavelength (nm)) depicting the reflectivity of light with average polarization incident at several angles onto an AR coating modified to have an extended low reflectivity wavelength range according to one or more embodiments shown and described herein;

[0061] Fig.19 is a graph of reflectivity versus incident angle (y-axis: reflectivity (%); x-axis: incident angle (degrees)) depicting the angular dependence of reflectivity of unpolarized light incident on an AR coating according to one or more embodiments shown and described herein;

[0062] Fig. 20 is a graph of reflectivity versus angle of incidence (y-axis: reflectivity (%); x-axis: angle of incidence (degrees)) depicting the angular dependence of reflectivity of p-polarized light incident on an AR coating according to one or more embodiments shown and described herein;

[0063] Fig.21 is a graph of reflectivity versus incident angle (y-axis: reflectivity (%); x-axis: incident angle (degrees)) depicting the angular dependence of reflectivity of unpolarized light incident on an AR coating according to one or more embodiments shown and described herein;

[0064] Fig. 22 is a graph of reflectivity versus angle of incidence (y-axis: reflectivity (%); x-axis: angle of incidence (degrees)) depicting the angular dependence of reflectivity of p-polarized light incident on an AR coating according to one or more embodiments shown and described herein. DETAILED DESCRIPTION

[0065] Reference will now be made in detail to various embodiments of a method of laser bonding glass to foil that accommodates the spectral response of an anti-reflective (AR) coating when the laser enters the AR coating at an oblique angle relative to the glass. Specifically, the method of laser bonding glass to foil disclosed herein includes applying an AR coating to a glass substrate, and bonding the foil to the glass substrate using a laser beam that travels through the glass substrate at an oblique angle relative to the glass substrate. The AR coating has an oblique wavelength range corresponding to the oblique angle, and the oblique wavelength range includes the wavelength of the laser beam, so that bonding can be achieved. According to an embodiment, a method of laser bonding glass to a metal foil may include: applying an anti-reflective coating to a first surface of a first glass substrate, the first glass substrate having a second surface opposite the first surface, the anti-reflective coating having a wavelength range; contacting the second surface of the first glass substrate with the first surface of the first foil to create a first contact location between at least a portion of the second surface of the first glass substrate and the first surface of the first foil; disposing the first surface of the first foil optically downstream of the first glass substrate; and performing a welding step by directing a laser beam having a first wavelength at an inclined angle relative to the first surface of the first glass substrate and at least a portion of the first contact location to bond the first surface of the first glass substrate to the first foil, wherein: the anti-reflective coating has an inclined wavelength range corresponding to the inclined angle, and the inclined wavelength range includes the wavelength of the laser beam. Various embodiments of laser bonding glass to metal foil and articles formed therefrom will be described herein with particular reference to the accompanying drawings.

[0066] Ranges may be expressed herein as from "about" one particular value, and / or to "about" another particular value. When such a range is expressed, another embodiment includes from a particular value and / or to another particular value. Similarly, when a value is expressed as an approximation by using the antecedent "about," it will be understood that the particular value forms another embodiment. It will be further understood that the endpoints of each range are significant relative to the other endpoint and are independent of the other endpoint.

[0067] Directional terms (eg, up, down, right, left, front, back, top, bottom) as used herein are made solely with reference to the drawings as drawn and are not intended to imply an absolute orientation.

[0068] Unless otherwise expressly stated, any method described herein is not to be construed as requiring that its steps be performed in a particular order, nor requiring any particular orientation of an apparatus. Thus, in the absence of a method claim actually reciting an order of steps to be followed, or any apparatus claim actually reciting an order or orientation of individual components, or otherwise specifically stating in the claim or description that the steps are to be limited to a particular order, or reciting a particular order or orientation of components of an apparatus, no order or orientation is intended to be inferred in any respect. This applies to any possible non-explicit basis for interpretation, including: matters of logic with respect to the arrangement of steps, flow of operations, order of components, or orientation of components; ordinary meaning derived from grammatical organization or punctuation; and the number or type of embodiments described in the specification.

[0069] As used herein, the singular forms "a", "an", and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a component" includes aspects having two or more such components unless the context clearly dictates otherwise.

[0070] As used herein with respect to an antireflective coating, "wavelength range" refers to the wavelengths at which the coating has a low reflectivity when directed at a normal angle relative to the glass substrate to which the coating is applied.

[0071] As used herein with respect to an antireflective coating, an "oblique wavelength range" refers to the wavelengths at which the coating has low reflectivity when directed at an oblique angle of incidence relative to the glass substrate to which the coating is applied. Depending on the specific degree of the oblique angle, the oblique wavelength range will differ, and thus each oblique wavelength range is associated with a specific oblique angle of incidence.

[0072] The "low reflectivity" described herein refers to a reflectivity of less than or equal to about 7%, or about 6%, or about 5%, or about 4%, or about 3%, or about 2%, or about 1%, or about 0.5%. The "high reflectivity" described herein refers to a reflectivity greater than 7%.

[0073] As used herein, a "hermetic bond" or "hermetic seal" refers to a package that includes a hermetic seal in accordance with MIL-STD-750E, Test Method 1071.9.

[0074] Hermetically bonded glass and metal foil packages are becoming increasingly popular for electronic devices and other devices that can benefit from a hermetic environment for continued operation. In consumer electronic applications, anti-reflective (AR) coatings can be applied to glass to improve display properties. Optical AR coatings are designed to substantially transmit light within a specific wavelength range (e.g., 400-700nm). However, increasing the transmittance at a specific wavelength increases the reflectivity at other wavelengths, so the optical AR coating will instead substantially reflect light outside the wavelength range. In addition, by extending the wavelength range, the maximum transmittance of the AR coating may also be reduced accordingly.

[0075] Laser bonding can be used to bond glass to foil to create a hermetically bonded package. Laser bonding using a laser beam in the visible spectrum (e.g., a wavelength of 400-700 nm) will generally not be affected when the laser is directed at a normal angle of incidence onto the AR coating. However, to form some hermetically bonded packages, it may be desirable to bond at an oblique angle. When the laser enters the AR coating at an oblique angle (i.e., a non-normal angle of incidence), the wavelength range of the AR coating may shift (e.g., toward shorter wavelengths) such that the wavelength of the laser beam is outside the oblique wavelength range of the AR coating, which may result in an unsuccessful bond.

[0076] Disclosed herein is a method of laser bonding glass to foil that alleviates the above-mentioned problems, making it possible to successfully bond a glass substrate having an AR coating to a metal foil by directing a laser at an oblique incident angle. Specifically, the method of laser bonding glass to foil disclosed herein includes applying an AR coating to a glass substrate, and bonding the foil to the glass substrate using a laser beam that travels through the glass substrate at an oblique angle relative to the glass substrate. The AR coating is designed to have an extended or relatively wide wavelength range, so that the oblique wavelength range of the AR coating corresponding to the oblique angle includes the wavelength of the laser beam, so that bonding can be achieved.

[0077] Reference now Figure 1 and Figure 2 The method of laser bonding glass to foil 100 begins at block 102 where an anti-reflective ("AR") coating 220 having an AR surface 221 is applied to a first surface 212 of a first glass substrate 210. The first glass substrate 210 further includes a second surface 214 opposite the first surface 212.

[0078] In an embodiment, the first glass substrate 210 may include a refractive index greater than or equal to 1.5 and less than or equal to 2.4. In an embodiment, the first glass substrate 210 may include a refractive index greater than or equal to 1.5, greater than or equal to 1.6, greater than or equal to 1.7, greater than or equal to 1.8, or even greater than or equal to 1.9. In an embodiment, the first glass substrate 210 may include a refractive index less than or equal to 2.4, less than or equal to 2.3, or even less than or equal to 2.2. In an embodiment, the first glass substrate 210 may include greater than or equal to 1.5 and less than or equal to 2.4, greater than or equal to 1.5 and less than or equal to 2.3, greater than or equal to 1.5 and less than or equal to 2.2, greater than or equal to 1.6 and less than or equal to 2.4, greater than or equal to 1.6 and less than or equal to 2.3, greater than or equal to 1.6 and less than or equal to 2.2, greater than or equal to 1.7 and less than or equal to 2.4, greater than or equal to 1.7 and less than or equal to 2.3, greater than or equal to 1.7 and less than or equal to 2.2, greater than or equal to 1.8 and less than or equal to 2.4, greater than or equal to 1.8 and less than or equal to 2.3, greater than or equal to 1.8 and less than or equal to 2.2, greater than or equal to 1.9 and less than or equal to 2.4, greater than or equal to 1.9 and less than or equal to 2.3, or even greater than or equal to 1.9 and less than or equal to 2.2, or any and all sub-ranges formed by any of these endpoints.

[0079] In an embodiment, the first glass substrate 210 may include glass or glass ceramics. As non-limiting examples, the first glass substrate 210 may include borate glass, borosilicate glass, phosphate-based glass, carborundum glass, soda-lime silicate glass, aluminosilicate glass, alkali aluminosilicate glass, borosilicate glass, alkali borosilicate glass, aluminoborosilicate glass, alkali aluminoborosilicate glass, alkali aluminosilicate glass, or niobium tungsten lanthanum boron glass. In an embodiment where a relatively high refractive index glass (e.g., a refractive index greater than or equal to 1.5 and less than or equal to 2.4) is desired, the first glass substrate 210 may include borate glass or borosilicate glass, such as the glass described in U.S. Provisional Application Serial No. 63 / 228,704, which is incorporated herein by reference in its entirety. In an embodiment, the first glass substrate 210 may be chemically strengthened, chemically tempered, and / or thermally tempered. Non-limiting examples of suitable commercially available glass substrates include Corning's EAGLE 、Lotus TM , and Glass, including chemically strengthened, chemically tempered and / or thermally tempered versions thereof. In embodiments, glass and glass ceramics that have been chemically strengthened by ion exchange may be suitable for use as substrates. In other embodiments, the first glass substrate 210 may be a strengthened glass to glass laminate.

[0080] In an embodiment, the first glass substrate 210 may be formed of a material that is substantially transparent to a selected wavelength of the laser beam. The term "substantially transparent" means that the wavelength of the laser beam is transmitted through the material without being substantially absorbed or scattered. For example, in an embodiment, a material that is substantially transparent to the wavelength of the laser beam may be a material that exhibits a transmittance greater than or equal to 90% at the wavelength. In an embodiment, the first glass substrate 210 may be substantially transparent to a wavelength of light greater than or equal to 300nm and less than or equal to 1100nm or even greater than or equal to 330nm and less than or equal to 750nm.

[0081] In an embodiment, the first glass substrate 210 may include a thickness greater than or equal to 0.1 mm, greater than or equal to 1 mm, greater than or equal to 10 mm, or even greater than or equal to 20 mm. In an embodiment, the first glass substrate 210 may include a thickness less than or equal to 100 mm, less than or equal to 75 mm, or even less than or equal to 50 mm. In an embodiment, the first glass substrate 210 may include a thickness of greater than or equal to 0.1 mm and less than or equal to 100 mm, greater than or equal to 0.1 mm and less than or equal to 75 mm, greater than or equal to 0.1 mm and less than or equal to 50 mm, greater than or equal to 1 mm and less than or equal to 100 mm, greater than or equal to 1 mm and less than or equal to 75 mm, greater than or equal to 1 mm and less than or equal to 50 mm, greater than or equal to 10 mm and less than or equal to 100 mm, greater than or equal to 10 mm and less than or equal to 75 mm, greater than or equal to 10 mm and less than or equal to 50 mm, greater than or equal to 20 mm and less than or equal to 100 mm, greater than or equal to 20 mm and less than or equal to 75 mm, or even greater than or equal to 20 mm and less than or equal to 50 mm, or any and all sub-ranges formed by any of these endpoints.

[0082] The AR coating 220 is applied to the first surface 212 of the first glass substrate 210 to provide anti-reflective qualities to the first glass substrate 210. These qualities include having a wavelength range in which the AR coating 220 has a low reflectivity for light incident at a normal angle relative to the first surface 212. Outside of this wavelength range, the AR coating 220 instead has a high reflectivity for light incident at a normal angle relative to the first surface 212. The wavelength range of the AR coating 220 may be a function of the composition of the AR coating, and in certain embodiments, the AR coating 220 may include one or more layers of one or more materials, and the materials of the AR coating 220 and their order within the layers may determine in whole or in part the wavelength range of the AR coating 220.

[0083] In some embodiments, the AR coating 220 may have a wavelength range in the visible spectrum (e.g., wavelengths of 400-700 nm). In other embodiments, the AR coating 220 may have an alternative wavelength range. However, as will be described in further detail below, when light enters the AR coating at an oblique angle (i.e., at a non-normal angle of incidence relative to the surface of the AR coating), the spectral response of the AR coating (i.e., the oblique wavelength range) is shifted toward shorter wavelengths (i.e., "blue-shifted"). This may lead to undesirable results, as will be described in further detail below.

[0084] In an embodiment, the AR coating 220 may have a wavelength range greater than or equal to 400 nm. In an embodiment, the AR coating 220 may have a wavelength range less than or equal to 1000 nm, less than or equal to 950 nm, less than or equal to 900 nm, less than or equal to 850 nm, or even less than or equal to 650 nm. In an embodiment, the AR coating 220 may have a wavelength range greater than or equal to 400 nm and less than or equal to 1000 nm, greater than or equal to 400 nm and less than or equal to 950 nm, greater than or equal to 400 nm and less than or equal to 900 nm, greater than or equal to 400 nm and less than or equal to 850 nm, or even greater than or equal to 400 nm and less than or equal to 650 nm, or any and all sub-ranges formed by any of these endpoints.

[0085] In an embodiment, block 102 may further include applying an AR coating to the second surface 214 of the first glass substrate 210. In an embodiment, the AR coating applied to the second surface of the first glass substrate 210 may be an AR coating 220. In an embodiment, the AR coating applied to the second surface of the first glass substrate 210 may be an AR coating different from the AR coating 220.

[0086] Reference now Figure 3 In an embodiment, the AR coating 220 may include a plurality of layers, including at least one layer of at least one material. The term "layer" may include a single layer or may include one or more sub-layers. Such sub-layers may be in direct contact with each other. The sub-layers may be formed of the same material or of two or more different materials. In one or more alternative embodiments, an intermediate layer of different materials may be provided between such sub-layers. In one or more embodiments, the layer may include one or more continuous and uninterrupted layers and / or one or more discontinuous and discontinuous layers (i.e., layers having different materials formed adjacent to each other). The layers or sub-layers may be formed by any method known in the art, including discrete deposition or continuous deposition processes. In one or more embodiments, the layers may be formed using only a continuous deposition process or alternatively only a discrete deposition process.

[0087] The AR coating 220 may have a thickness of about 1 μm or greater while still providing an article exhibiting the optical properties described herein. In some examples, the AR coating 220 may have a thickness in a range from about 1 μm to about 20 μm (e.g., from about 1 μm to about 10 μm, or from about 1 μm to about 5 μm).

[0088] As used herein, the term "disposed" includes coating, depositing and / or forming a material on a surface using any method known in the art. The disposed material may constitute a layer as defined herein. The phrase "disposed on..." includes the case where the material is formed on a surface so that the material is in direct contact with the surface, and also includes the case where the material is formed on a surface with one or more intermediate materials between the disposed material and the surface. (Multiple) intermediate material(s) may constitute a layer as defined herein.

[0089] like Figure 3 As shown, the AR coating 220 may include a plurality of layers. In one or more embodiments, the AR coating 220 may include a period 222, which includes two or more layers. In one or more embodiments, the two or more layers may be characterized by having different refractive indices from each other. In one embodiment, the period 222 includes a first layer 220A and a second layer 220B. In some embodiments, the first layer 220A may be a high refractive index layer, and the second layer 220B may be a low refractive index layer. In other embodiments, the first layer 220A may be a low refractive index layer, and the second layer 220B may be a high refractive index layer. The AR coating 220 may include a plurality of periods, such that the first layer 220A and the second layer 220B alternate. In an embodiment, the AR coating 220 may include greater than or equal to 2 and less than or equal to 20 periods. In an embodiment, the refractive index difference between the low refractive index layer and the high refractive index layer (e.g., layers 220A and 220B, respectively) may be greater than or equal to 0.01. In an embodiment, the low refractive index layer may have a refractive index greater than or equal to 1.3 and less than or equal to 1.7. In an embodiment, the high refractive index layer may have a refractive index greater than 1.7. In an embodiment, the low refractive index layer may include SiO2, Al2O3, GeO2, SiO, AlO x N y 、SiO x N y 、Si u Al v O x N y , MgO, MgAl2O4, MgF2, BaF2, CaF2, DyF3, YbF3, YF3 and CeF3 or a combination thereof. In an embodiment, the high refractive index layer may include Si u AlvOxNy, Ta2O5, Nb2O5, AlN, Si3N4, AlO x Ny 、SiO x N y , HfO2, TiO2, ZrO2, Y2O3, Al2O3, MoO3, diamond-like carbon, or a combination thereof.

[0090] Reference now Figure 4 In some embodiments, the period 222 may include one or more third layers 220C. The third layer(s) 220C may have a low refractive index, a high refractive index, or a medium refractive index. In some embodiments, the third layer(s) 220C may have the same refractive index as the first layer 220A or as the second layer 220B. In other embodiments, the third layer(s) 220C may have a medium refractive index between the refractive indexes of the first layer 220A and the second layer 220B. Alternatively, the third layer(s) 220C may have a refractive index greater than the refractive indexes of the two layers 220A, 220B. The third layer 220C may be disposed in the AR coating 220 in the following exemplary configurations: 第三层 / H / L / H / L;H 第三层 / L / H / L / H; L / H / L / H / L 第三层 ;H / L / H / L / H 第三层 ; L 第三层 / H / L / H / L / H 第三层 ;H 第三层 / L / H / L / H / L 第三层 ; L 第三层 / L / H / L / H;H 第三层 / H / L / H / L; H / L / H / L / L 第三层 ; L / H / L / H / H 第三层 ; L 第三层 / L / H / L / H / H 第三层 ;H 第三层 / H / L / H / L / L 第三层 ; L / M / H / L / M / H; H / M / L / H / M / L; M / L / H / L / M; and other combinations. In these configurations, "L" without any subscript refers to the first low refractive index layer, and "H" without any subscript refers to the second high refractive index layer. 第三层 ” refers to the third layer with a low refractive index, “H 第三层 " refers to the third layer with a high refractive index, and "M" refers to the third layer with a medium refractive index, both of which are relative to the first low refractive index layer and the second high refractive index layer.

[0091] As used herein, the terms "low refractive index", "high refractive index", and "medium refractive index" refer to relative values ​​of refractive index when compared to other refractive indices (e.g., low refractive index <medium refractive index <high ​​refractive index). In some embodiments, the term "medium refractive index" includes a range of 1.5 to 1.8 when used with (multiple) third layers 220C. Accordingly, in embodiments of layers having a medium refractive index, the term "low refractive index" may include a range of values ​​less than the lower limit of the medium refractive index range of the embodiment (i.e., less than 1.5). Similarly, in similar embodiments of layers having a medium refractive index, the term "high refractive index" may include a range of values ​​greater than the upper limit of the medium refractive index range of the embodiment (i.e., greater than 1.8). In some embodiments, the ranges of low refractive index, high refractive index, and medium refractive index may overlap; however, in most embodiments, the layers of the AR coating 220 have a general relationship with respect to refractive index: low refractive index <medium refractive index <high ​​refractive index.

[0092] The third layer(s) 220C may be provided as a layer separate from the period 222, and in some alternative embodiments having multiple periods, the third layer(s) 220C may be disposed between different periods in the multiple periods. The third layer(s) 220C may also be provided as a layer separate from the period 222 and disposed above the remaining layers 220A, 220B, such as Figure 5 The third layer(s) 220C may also be provided as a layer separated from the period 222 and disposed between the remaining layers 220A, 220B and the first glass substrate 210, as shown. Figure 6 shown.

[0093] Exemplary materials suitable for AR coating 220 include: SiO2, Al2O3, GeO2, SiO, AlO x N y 、AlN、SiN x 、SiO x N y 、Si u Al v O x N y , Ta2O5, Nb2O5, TiO2, ZrO2, TiN, MgO, MgF2, BaF2, CaF2, SnO2, HfO2, Y2O3, MoO3, D yF3, YbF3, YF3, CeF3, polymers, fluorinated polymers, plasma polymerized polymers, siloxane polymers, silsesquioxanes, polyimides, fluorinated polyimides, polyetherimides, polyethersulfones, polyphenylsulfones, polycarbonates, polyethylene terephthalate, polyethylene naphthalate, acrylic polymers, polyurethane polymers, polymethyl methacrylate, and other materials known in the art. Examples of some suitable materials for the low refractive index layer include SiO2, Al2O3, GeO2, SiO, AlO x N y 、SiO x N y 、Si u Al v O x N y , MgO, MgAl2O4, MgF2, BaF2, CaF2, DyF3, YbF3, YF3, and CeF3. The nitrogen content of the material used for the low refractive index layer can be minimized (for example, in materials such as Al2O3 and MgAl2O4). Some examples of materials suitable for the high refractive index layer include Si u AlP x N y , Ta2O5, Nb2O5, AlN, Si3N4, AlO x N y 、SiO x N y , HfO2, TiO2, ZrO2, Y2O3, Al2O3, MoO3 and diamond-like carbon. The oxygen content of the material of the high refractive index layer can be minimized, especially in SiN x or AlN x Materials. AlO x N y The material can be considered as oxygen-doped AlN x , i.e. they may have AlN x Crystal structure (such as wurtzite) and need not have AlON crystal structure (such as wurtzite) and need not have AlON crystal structure. Exemplary preferred AlO x N y The high refractive index material may include about 0 atomic % to about 20 atomic % oxygen, or about 5 atomic % to about 15 atomic % oxygen, and 30 atomic % to about 50 atomic % nitrogen. u Al v O x N yThe high refractive index material may include about 10 atomic % to about 30 atomic % or about 15 atomic % to about 25 atomic % silicon, about 20 atomic % to about 40 atomic % or about 25 atomic % to about 35 atomic % aluminum, about 0 atomic % to about 20 atomic % or about 1 atomic % to about 20 atomic % oxygen, and about 30 atomic % to about 50 atomic % nitrogen. The above materials may be hydrogenated to up to about 30% by weight. When a material with a medium refractive index is desired, some embodiments may utilize MN and / or SiO x N y .

[0094] In one or more embodiments, at least one of the (multiple) layers of the AR coating 220 may include a specific optical thickness range. As used herein, the term "optical thickness" is determined by (n×d), where "n" refers to the refractive index of the sublayer and "d" refers to the physical thickness of the layer. In one or more embodiments, at least one of the (multiple) layers of the AR coating 220 may include an optical thickness in the range of about 2 nm to about 200 nm, about 10 nm to about 100 nm, about 15 nm to about 100 nm, about 15 to about 500 nm, or about 15 to about 5000 nm. In some embodiments, all layers of the AR coating 220 may each have an optical thickness in the range of about 2 nm to about 200 nm, about 10 nm to about 100 nm, about 15 nm to about 100 nm, about 15 to about 500 nm, or about 15 to about 5000 nm. In some cases, at least one layer of the AR coating 220 has an optical thickness of about 50 nm or more. In some cases, each low refractive index layer has an optical thickness in the range of about 2 nm to about 200 nm, about 10 nm to about 100 nm, about 15 nm to about 100 nm, about 15 nm to about 500 nm, or about 15 to about 5000 nm. In other cases, each high refractive index layer has an optical thickness in the range of about 2 nm to about 200 nm, about 10 nm to about 100 nm, about 15 nm to about 100 nm, about 15 nm to about 100 nm, about 15 to about 500 nm, or about 15 to about 5000 nm. In yet other cases, each of the third layers has an optical thickness in the range of about 2 nm to about 200 nm, about 10 nm to about 100 nm, about 15 nm to about 100 nm, about 15 nm to about 500 nm, or about 15 to about 5000 nm.

[0095] In some embodiments, the thickness of one or more of the layers of the AR coating 220 may be minimized. In one or more embodiments, the thickness of the high refractive index layer(s) and / or the medium refractive index layer(s) are minimized such that they are less than about 500 nm. In one or more embodiments, the combined thickness of the high refractive index layer(s), the medium refractive index layer(s), and / or the combination of the high refractive index layer(s) and the medium refractive index layer(s) is less than about 500 nm.

[0096] In some embodiments, the amount of low refractive index material in the AR coating 220 can be minimized. Expressed as a fraction of the physical thickness of the AR coating 220, the low refractive index material can include less than about 60%, less than about 50%, less than about 40%, less than about 30%, less than about 20%, less than about 10%, or less than about 5% of the physical thickness of the AR coating 220. Alternatively or additionally, the amount of low refractive index material can be quantified as the sum of the physical thicknesses of all layers of low refractive index material disposed above the thickest high refractive index layer in the AR coating 220 (i.e., on the side opposite to the first glass substrate 210, the user side or the air side). The amount of low refractive index material disposed on the thickest high refractive index layer (i.e., on the side opposite the glass substrate, the user side or the air side) may have a thickness of less than or equal to about 150 nm, less than or equal to about 120 nm, less than or equal to about 110 nm, 100 nm, 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, 25 nm, 20 nm, 15 nm, or less than or equal to about 12 nm.

[0097] In one or more embodiments, the combined physical thickness of the high refractive index layer(s) may be characterized. For example, in some embodiments, the combined thickness of the high refractive index layer(s) may be about 100 nm or more, about 150 nm or more, about 200 nm or more, about 500 nm or more. The combined thickness is a calculated combination of the thicknesses of the individual high refractive index layers(s) in the AR coating 220, even when there are(s) intermediate low refractive index layers or(s) other layers. In some embodiments, the combined physical thickness of the high refractive index layer(s) may be greater than 30% of the total physical thickness of the AR coating 220. For example, the combined physical thickness of the high refractive index layer(s) may be about 40% or more, about 50% or more, about 60% or more, about 70% or more, about 75% or more, or even about 80% or more of the total physical thickness of the anti-reflective layer. Additionally or alternatively, the amount of high refractive index material included in the AR coating 220 may be characterized as a percentage of the physical thickness of the topmost 500 nm of the article or AR coating 220 (i.e., the user side or the side of the AR coating 220 opposite the first glass substrate 210). The combined physical thickness of the (multiple) high refractive index layers (or the thickness of the high refractive index material) expressed as a percentage of the topmost 500 nm of the article or AR coating 220 may be about 50% or greater, about 60% or greater, about 70% or greater, about 80% or greater, or even about 90% or greater. In one or more embodiments, the high refractive index layer may include a material with a refractive index greater than about 1.85, and the low refractive index layer may include a material with a refractive index less than about 1.75. In some embodiments, the high refractive index layer may include a nitride or oxynitride material. In some cases, the combined thickness of all low-refractive index layers in AR coating 220 can be about 200 nm or less (eg, about 150 nm or less, about 100 nm or less, about 75 nm or less, or about 50 nm or less).

[0098] In some embodiments, the AR coating 220 exhibits an average light reflectance of about 9% or less, about 8% or less, about 7% or less, about 6% or less, about 5% or less, about 4% or less, about 3% or less, or about 2% or less over a range of optical wavelengths when measured only at the AR surface 221 of the AR coating 220 (e.g., when any reflection is removed from the uncoated back side of the article (e.g., the second surface 214), such as by using an index matching oil on the back side coupled to the absorber, or other known methods). The average reflectance, which may be a photopic average, may be in the range of about 0.4% to about 9%, about 0.4% to about 8%, about 0.4% to about 7%, about 0.4% to about 6%, or about 0.4% to about 5%, and all ranges therebetween. In some cases, the AR coating 220 may exhibit such average light reflectivity in other wavelength ranges, such as about 450 nm to about 650 nm, about 420 nm to about 680 nm, about 420 nm to about 700 nm, about 420 nm to about 740 nm, about 420 nm to about 850 nm, or about 420 nm to about 950 nm. In some embodiments, the AR surface 221 exhibits an average light transmittance of about 90% or greater, about 92% or greater, about 94% or greater, about 96% or greater, or about 98% or greater in optical wavelength transmittance when measured at an incident illumination angle of about 0 degrees to about 10 degrees (however, such measurements may be provided at an incident illumination angle of 45 degrees or 60 degrees).

[0099] In some embodiments, there may be one or more additional coatings disposed on the AR coating 220 and / or between the various layers of the AR coating 220. In one or more embodiments, the additional coatings may include a scratch resistant coating, an easy to clean coating, and / or an abrasion resistant coating. Examples of scratch resistant and abrasion resistant coatings are described in U.S. Pat. No. 9,335,444, filed May 7, 2015, entitled “DURABLE AND SCRATCH-RESISTANT ANTI-REFLECTIVE ARTICLES,” which is incorporated herein by reference in its entirety. Examples of suitable easy-to-clean coatings are described in U.S. patent application Ser. No. 13 / 690,904, filed on Nov. 30, 2012, entitled “PROCESS FOR MAKING OF GLASS ARTICLES WITH OPTICAL AND EASY-TO-CLEAN COATINGS” (U.S. Publication No. 2014 / 0113083A1), which is incorporated herein by reference in its entirety.

[0100] refer to Figures 3 to 6, the AR coating 220 may include Figures 3 to 6 Any combination of any or all of the depicted layer, layer order, and / or layer pattern embodiments.

[0101] Reference again Figure 1 And as Figure 7 As shown, at block 104, the second surface 214 of the first glass substrate 200 is contacted with the first surface 232 of the foil 230 to create a first contact location 234 between at least a portion of the second surface 214 of the first glass substrate 200 and the first surface 232 of the first foil 230. In embodiments, the first foil 230 may be in contact with only a portion of the second surface 214. In other embodiments, the first foil 230 may be in contact with the entire second surface 214.

[0102] In an embodiment, before applying the AR coating 220, or in other embodiments, before bonding the first glass substrate 210 to the first foil 230, the first glass substrate 210 may be subjected to surface preparation. For example, in an embodiment, the first glass substrate 210 may be polished until its surface exhibits a relatively low surface roughness value, which may enhance bonding. In an embodiment, one or both of the first surface 212 and the second surface 214 of the first glass substrate 210 may be polished until one or both of the first surface 212 and the second surface 214 exhibit an average surface roughness (Ra) of less than or equal to 1 μm, less than or equal to 0.5 μm, or even less than or equal to 0.25 μm. The smooth surface may allow one or both of the first surface 212 and the second surface 214 to be placed in close contact with a foil (e.g., the first foil 230). In addition, the first glass ceramic substrate 210 may be cleaned with water and / or a solvent to remove any debris present on the surface and / or to remove any material (oil, grease, etc.) that may reduce the transparency of the substrate to the desired laser wavelength. Removing any debris may allow the first glass substrate 210 to be placed in close contact with the metal foil to better facilitate laser bonding of the first foil 230 to the glass. Removing any debris may also or alternatively allow the AR coating 220 to be applied to the first glass substrate 210 to better facilitate laser bonding of the first foil 230 to the first glass substrate 210, to better provide anti-reflective qualities, or to better facilitate uniform distribution of the AR coating 220 on the first glass substrate 210.

[0103] In an embodiment, the first foil 230 may have a thickness of less than or equal to 75 μm. In an embodiment, the first foil 230 may have a thickness of greater than or equal to 5 μm and less than or equal to 75 μm. In an embodiment, the first foil 230 may have a thickness of greater than or equal to 5 μm, greater than or equal to 10 μm, or even greater than or equal to 20 μm. In an embodiment, the first foil 230 may have a thickness of less than or equal to 75 μm, less than or equal to 50 μm, less than or equal to 40 μm, or even less than or equal to 30 μm. In an embodiment, the first foil 230 may have a thickness of greater than or equal to 5 μm and less than or equal to 75 μm, greater than or equal to 5 μm and less than or equal to 50 μm, greater than or equal to 5 μm and less than or equal to 40 μm, greater than or equal to 5 μm and less than or equal to 30 μm, greater than or equal to 10 μm and less than or equal to 75 μm, greater than or equal to 10 μm and less than or equal to 50 μm, greater than or equal to 10 μm and less than or equal to 40 μm, greater than or equal to 10 μm and less than or equal to 30 μm, greater than or equal to 20 μm and less than or equal to 75 μm, greater than or equal to 20 μm and less than or equal to 50 μm, greater than or equal to 20 μm and less than or equal to 40 μm, or even greater than or equal to 20 μm and less than or equal to 30 μm, or any and all subranges formed by any of these endpoints.

[0104] In an embodiment, the first foil 230 may include aluminum, aluminum alloy, stainless steel, nickel, nickel alloy, silver, silver alloy, titanium, titanium alloy, tungsten, tungsten alloy, gold, gold alloy, copper, copper alloy, bronze, iron, or a combination thereof. In an embodiment, the first foil 230 may include a combination of a metal and another non-metallic material.

[0105] In embodiments, the first foil 230 may be formed of a material having a melting point that allows successful bonding to a glass substrate.In embodiments, the first foil 230 may include a melting point less than or equal to 1600°C, less than or equal to 1500°C, and less than or equal to 1400°C.

[0106] In an embodiment, the first foil 230 may be formed of a material that is chemically compatible with (ie, easily bonded to) a glass substrate. For example, a glass substrate including aluminum may be more easily bonded to an aluminum metal foil.

[0107] In an embodiment, the first foil 230 may be formed of a material that is substantially opaque to a selected wavelength of the laser beam. The term "substantially opaque" means that when the laser beam contacts the material, the wavelength of the laser beam is substantially absorbed. For example, in an embodiment, the material that is substantially opaque to the wavelength of the laser beam may be a material that exhibits an absorptivity greater than or equal to 35% at the wavelength.

[0108] In an embodiment, the first foil 230 may have a similar average surface roughness (Ra) as the first glass substrate 210 to similarly allow the first glass substrate 210 to be placed in close contact with the first foil 230 .

[0109] Reference again Figure 1 And as Figure 8 As shown, at block 106 , a first foil 230 is disposed optically downstream of the first glass substrate 210 relative to the laser 240 .

[0110] It should be noted that this specification and claims refer to arranging various components "optically downstream" of various other components. Arranging a first component "optically downstream" of a second component encompasses placing the first component relative to the second component and a laser (or other radiation generating device) such that a laser beam or other radiation beam of the laser or other radiation generating device will follow an optical path that passes through both the first component and the second component such that the second component precedes the first component in the optical path. For example, in Figure 8 , the first foil 230 is arranged optically downstream of the first glass substrate 210 so that a potential laser beam of the laser 240 (if activated) will pass through the AR coating 220 , then through the first glass substrate 210 , and then impinge on a first contact location 234 on the first surface 232 of the first foil 230 .

[0111] Reference again Figure 1 And as Figure 9-10 As shown, the method 100 continues at box 108 by performing a welding step by directing a laser beam 242 of a laser 240 to be incident on the first surface 212 of the first glass substrate 210 at an oblique angle 244 on at least a portion of the first contact location 234 to bond the first glass substrate 210 to the foil 230 and form a first bonding location 236 .

[0112] In an embodiment, laser beam 242 may be unpolarized light. In other embodiments, laser beam 242 may be p-polarized light. In other embodiments, laser beam 242 may be s-polarized light. In other embodiments, laser beam 242 may be average polarized light. In other embodiments, laser beam 242 may have another polarization.

[0113] As used herein, "unpolarized light" is light that includes waves of all possible polarizations. As used herein, "p-polarized light" is light that is polarized parallel to a plane of interest (e.g., the first surface 212 of the AR coating 220). As used herein, "s-polarized light" is light that is polarized at a normal angle relative to a plane of interest (e.g., the first surface 212 of the AR coating 220). As used herein, "average polarized light" is light that has an average polarization of s-polarized light and p-polarized light.

[0114] In an embodiment, the laser 240 includes a pulsed laser. In an embodiment, the pulsed laser may be a nanosecond pulsed laser, a picosecond pulsed laser, or a femtosecond pulsed laser.

[0115] In an embodiment, the pulsed laser may include a pulse energy greater than or equal to 2.8 μJ and less than or equal to 1000 μJ. In an embodiment, the pulsed laser may include a pulse energy greater than or equal to 2.8 μJ, greater than or equal to 10 μJ, greater than or equal to 25 μJ, or even greater than or equal to 50 μJ. In an embodiment, the pulsed laser may include a pulse energy less than or equal to 1000 μJ, less than or equal to 750 μJ, less than or equal to 500 μJ, or even less than or equal to 250 μJ. In an embodiment, the pulsed laser may include greater than or equal to 2.8 μJ and less than or equal to 1000 μJ, greater than or equal to 2.8 μJ and less than or equal to 750 μJ, greater than or equal to 2.8 μJ and less than or equal to 500 μJ, greater than or equal to 2.8 μJ and less than or equal to 250 μJ, greater than or equal to 10 μJ and less than or equal to 1000 μJ, greater than or equal to 10 μJ and less than or equal to 750 μJ, greater than or equal to 10 μJ and less than or equal to 500 μJ, greater than or equal to 10 μJ and less than or equal to 250 μJ, or greater than or equal to 25 μJ and less than or equal to 1000 μJ, greater than or equal to 25 μJ and less than or equal to 750 μJ, greater than or equal to 25 μJ and less than or equal to 500 μJ, greater than or equal to 25 μJ and less than or equal to 250 μJ, greater than or equal to 50 μJ and less than or equal to 1000 μJ, greater than or equal to 50 μJ and less than or equal to 750 μJ, greater than or equal to 50 μJ and less than or equal to 500 μJ, or even greater than or equal to 50 μJ and less than or equal to 250 μJ, or any and all sub-ranges formed by any of these endpoints.

[0116] In an embodiment, the pulsed laser may have a wavelength such that the first glass substrate 210 is substantially transparent to the wavelength of the laser beam and the first foil 230 is substantially opaque to the wavelength of the laser beam. For example, in an embodiment, the pulsed laser may have a wavelength greater than or equal to 300 nm and less than or equal to 1100 nm. In an embodiment, the pulsed laser may have a wavelength greater than or equal to 300 nm, greater than or equal to 325 nm, or even greater than or equal to 350 nm. In an embodiment, the pulsed laser may have a wavelength less than or equal to 1100 nm, less than or equal to 900 nm, or even less than or equal to 700 nm. In embodiments, the pulsed laser may have a wavelength greater than or equal to 300 nm and less than or equal to 1100 nm, greater than or equal to 300 nm and less than or equal to 900 nm, greater than or equal to 300 nm and less than or equal to 700 nm, greater than or equal to 325 nm and less than or equal to 1100 nm, greater than or equal to 325 nm and less than or equal to 900 nm, greater than or equal to 325 nm and less than or equal to 700 nm, greater than or equal to 350 nm and less than or equal to 1100 nm, greater than or equal to 350 nm and less than or equal to 900 nm, or even greater than or equal to 350 nm and less than or equal to 700 nm, or any and all sub-ranges formed by any of these endpoints.

[0117] In an embodiment, the pulsed laser may include a high repetition rate pulsed UV laser operating at approximately 355 nm, 532 nm, 750 nm, 1064 nm, or any other suitable wavelength, depending on the transmittance of the glass.

[0118] In an embodiment, the pulsed laser may have a repetition rate greater than or equal to 5 kHz and less than or equal to 1 MHz. In an embodiment, the pulsed laser may have a repetition rate greater than or equal to 5 kHz, greater than or equal to 50 kHz, greater than or equal to 100 kHz, or even greater than or equal to 250 kHz. In an embodiment, the pulsed laser may have a repetition rate less than or equal to 1 MHz, less than or equal to 750 kHz, or even less than or equal to 500 KHz. In embodiments, the pulsed laser may have a repetition rate greater than or equal to 5 kHz and less than or equal to 1 MHz, greater than or equal to 5 kHz and less than or equal to 750 kHz, greater than or equal to 5 kHz and less than or equal to 500 kHz, greater than or equal to 50 kHz and less than or equal to 1 MHz, greater than or equal to 50 kHz and less than or equal to 750 kHz, greater than or equal to 50 kHz and less than or equal to 500 kHz, greater than or equal to 100 kHz and less than or equal to 1 MHz, greater than or equal to 100 kHz and less than or equal to 750 kHz, greater than or equal to 100 kHz and less than or equal to 500 kHz, greater than or equal to 250 kHz and less than or equal to 1 MHz, greater than or equal to 250 kHz and less than or equal to 750 kHz, or even greater than or equal to 250 kHz and less than or equal to 500 kHz, or any and all sub-ranges formed by any of these endpoints.

[0119] As used herein, "spot size" (ie, ω0) refers to the number of intensity values ​​of the beam falling within the axial value of the beam intensity (e 2 ) -1 The beam spot radius at . In an embodiment, the pulsed laser may have a spot size greater than or equal to 5 μm and less than or equal to 50 μm. In an embodiment, the pulsed laser may have a spot size greater than or equal to 5 μm or even greater than or equal to 10 μm. In an embodiment, the pulsed laser may have a spot size less than or equal to 50 μm, less than or equal to 35 μm, or even less than or equal to 20 μm. In an embodiment, the pulsed laser may have a spot size greater than or equal to 5 μm and less than or equal to 50 μm, greater than or equal to 5 μm and less than or equal to 35 μm, greater than or equal to 5 μm and less than or equal to 20 μm, greater than or equal to 10 μm and less than or equal to 50 μm, greater than or equal to 10 μm and less than or equal to 35 μm, or even greater than or equal to 10 μm and less than or equal to 20 μm, or any and all sub-ranges formed by any of these endpoints.

[0120] In an embodiment, Fig. 9As shown in FIG. 1 , during a first welding step, the first foil 230 is disposed optically downstream of the first glass substrate 210 such that a laser beam 242 passes through the AR coating 220, then through the first glass substrate 210, and then is incident on a first contact location 234. The laser beam 242 may pass along the first contact location 234 to facilitate a line bond between the glass and the foil. For example, the laser beam 242 may pass along the first contact location 234 (e.g., into and / or out of the page and / or transverse to the page). Fig. 9 page plane in the glass) to facilitate line bonding between the glass and the foil.

[0121] exist Fig. 9 , the laser beam 242 is incident on the AR coating 220 and the first glass substrate 210 at an oblique angle 244. In different embodiments, the oblique angle 244 can be one of many different non-normal (i.e., non-perpendicular) angles, including, for example, any angle less than 90 degrees or any angle less than or equal to 60 degrees. In further embodiments, the oblique angle 244 can be less than or equal to 45 degrees or less than or equal to 30 degrees.

[0122] AR coatings (e.g., AR coating 220) may rely on destructive interference to produce anti-reflection qualities, including, for example, the wavelength range of the AR coating 220. Such destructive interference may depend on the path length of the incident light, and thus, if the angle of incidence of the incident light relative to the AR surface 221 is increased (i.e., the angle of incidence is a non-normal angle), the path length of the incident light within the AR coating 220 changes, and the performance (i.e., wavelength range) of the AR coating 220 may also similarly change. This may cause the wavelength range of the AR coating 220 to shift to lower wavelengths (e.g., blue shift), resulting in a tilted wavelength range (e.g., a wavelength range with lower upper and lower wavelength limits) corresponding to the non-normal angle of incidence. Due to this behavior, a wavelength of incident light that may be within the wavelength range of the AR coating 220 at a normal angle may still not be within the tilted wavelength range of the AR coating 220.

[0123] The laser beam 242 entering the AR coating 220 at the tilt angle 244 may thus cause the reflectivity of the laser beam 242 to be determined by the tilt wavelength range corresponding to the tilt angle 244 rather than the wavelength range of the AR coating 220 (the particular limits of the tilt wavelength range being at least partially a function of the angle of incidence). To accommodate this effect, the AR coating 220 has a broadened extended wavelength range (compared to, for example, certain conventional AR coatings having a wavelength range corresponding to the visible spectrum) such that the tilt wavelength range of the AR coating 220 corresponding to the tilt angle 244 includes the wavelength of the laser beam 242. Thus, the laser beam 242 may pass along the first contact location 234 to facilitate the wire bonding between the glass and the foil without causing interference or with reduced interference because the laser beam 242 enters the AR coating 220 at the tilt angle 244.

[0124] In some embodiments, the extended wavelength range includes the original wavelength range (e.g., a wavelength range including the visible spectrum) that the AR coating 220 alone requires to exhibit low reflectivity during the welding step (e.g., for the end use of the associated optical device). In such embodiments, the extended wavelength range is not derived solely from the optical device (e.g., Figure 2-Figure 5 ) (or a larger product incorporating such an optical device), is offset from the original wavelength range required, but is instead broadened relative to the original wavelength range (i.e., the extended wavelength range completely includes the original wavelength range) to provide a tilted wavelength range suitable for the first bonding step and the desired functionality in the larger product.

[0125] In an embodiment, the AR coating 220 has a broadened wavelength range such that the AR coating 220 has a tilted wavelength range corresponding to a tilt angle 244, at which the AR coating 220 has an average reflectivity of less than or equal to about 7% over the entire tilted wavelength range. More specifically, the AR coating 220 has an average reflectivity of less than or equal to about 6%, or about 5%, or about 4%, or about 3%, or about 2%, or about 1%, or about 0.5% over the entire tilted wavelength range. The tilted wavelength range may be greater than or equal to about 375 nm and less than or equal to about 800 nm, or greater than or equal to about 380 nm and less than or equal to about 790 nm, or greater than or equal to about 385 nm and less than or equal to about 785 nm, or greater than or equal to about 390 nm and less than or equal to about 780 nm, or greater than or equal to about 395 nm and less than or equal to about 775 nm, or greater than or equal to about 400 nm and less than or equal to about 770 nm. In an embodiment, the tilt angle 244 is 0°, or 30°, or 45°, or 60°, or any range covering these values ​​(e.g., 0° to 60°, 30° to 45°, 0° to 55°, 25° to 45°).

[0126] In an embodiment, the laser beam 242 may have a wavelength of, for example, 532 nm, and thus, in such embodiments, the extended wavelength range of the AR coating 220 has a tilted wavelength range corresponding to light incident at the tilt angle 224, including the 532 nm wavelength. In other embodiments, the laser beam 242 may have a wavelength of, for example, 750 nm, and thus, in such embodiments, the extended wavelength range of the AR coating 220 has a tilted wavelength range corresponding to light incident at the tilt angle 244, including the 750 nm wavelength. In other embodiments and as described above, the laser beam 242 may have another wavelength. In some specific embodiments, the extended wavelength range of the AR coating 220 has a tilted wavelength range corresponding to light incident at the tilt angle 244, which may be greater than or equal to 375 nm and less than or equal to 700 nm at a tilt angle of 30 degrees. In other embodiments, the AR coating 220 has a tilted wavelength range corresponding to light incident at the tilt angle 244, which may be greater than or equal to 360 nm and less than or equal to 675 nm at a tilt angle of 45 degrees. In other embodiments, the AR coating 220 has a tilted wavelength range corresponding to light incident at the tilt angle 244, which may be greater than or equal to 350 nm and less than or equal to 650 nm at a tilt angle of 60 degrees. In other embodiments, the AR coating 220 may have a tilted wavelength range corresponding to any wavelength range including the wavelength of the laser when bonding at a predetermined bonding angle.

[0127] In an embodiment, the AR coating 220 may have a wavelength range configured to have a tilted wavelength range that includes the wavelength of the laser beam 242 at an incident angle of 60 degrees. In other embodiments, the AR coating 220 may have a wavelength range configured to have a tilted wavelength range that includes the wavelength of the laser beam 242 at an incident angle of 45 degrees. In other embodiments, the AR coating 220 may have a wavelength range configured to have a tilted wavelength range that includes the wavelength of the laser beam 242 at an incident angle of 30 degrees. In other embodiments, the AR coating 220 may have a wavelength range configured to have a tilted wavelength range that includes the wavelength of the laser beam 242 at an incident angle of less than 90 degrees. In other embodiments, the AR coating 220 may have a wavelength range configured to have a tilted wavelength range that includes the wavelength of the laser beam 242 at an incident angle of less than or equal to 60 degrees. In other embodiments, the AR coating 220 may have a wavelength range configured to have a tilted wavelength range that includes the wavelength of the laser beam 242 at an incident angle of less than or equal to 45 degrees. In other embodiments, the AR coating 220 may have a wavelength range configured to have a tilted wavelength range that includes the wavelength of the laser beam 242 at an incident angle of less than or equal to 30 degrees.

[0128] Reference again Figure 1 And if Fig.10 As shown, at block 108 , the welding step continues by directing a laser beam 242 of a laser 240 over at least a portion of the contact location 234 at a second tilt angle 246 relative to the first surface 212 of the first glass substrate 210 to form a second bonded location 238 .

[0129] exist Fig.10 , the laser beam 242 is incident on the AR coating 220 and the first glass substrate 210 at a second tilt angle 246. Like the tilt angle 244, in different embodiments, the second tilt angle 246 can be one of many different non-normal (i.e., non-perpendicular or not equal to 90 degrees) angles, including, for example, any angle between 0 and 90 degrees or any angle less than or equal to 60 degrees. In some embodiments, the tilt angle 244 can be the same as the second tilt angle 246. In other embodiments, the tilt angle 244 can be different from the second tilt angle 246. As with the bonding of the first bonding location 236, the formation of the second bonding location 238 by bonding with the laser beam 242 at the second tilt angle 246 may similarly require the AR coating 220 to have an extended wavelength range having a tilted wavelength range corresponding to the second tilt angle 246, which includes the wavelength 242 of the laser beam.

[0130] As discussed above with reference to the tilt angle 244, similarly, the AR coating 220 has a tilt wavelength range corresponding to the tilt angle 246, at which the AR coating 220 has an average reflectivity of less than or equal to about 7% (or about 6%, or about 5%, or about 4%, or about 3%, or about 2%, or about 1%, or about 0.5%) over the entire tilt wavelength range. In an embodiment, the tilt angle 246 is 0°, or 30°, or 45°, or 60°, or any range covering these values ​​(e.g., 0° to 60°, 30° to 45°, 0° to 55°, 25° to 45°), similar to the tilt angle 244 discussed above. The tilted wavelength range may be greater than or equal to about 375 nm and less than or equal to about 800 nm, or greater than or equal to about 380 nm and less than or equal to about 790 nm, or greater than or equal to about 385 nm and less than or equal to about 785 nm, or greater than or equal to about 390 nm and less than or equal to about 780 nm, or greater than or equal to about 395 nm and less than or equal to about 775 nm, or greater than or equal to about 400 nm and less than or equal to about 770 nm.

[0131] Reference again Figure 1 And if Fig.11As shown, at block 110, a portion of the first foil 230 may be removed from a central region of the first glass substrate 210 to form a first hole 250 on the first glass substrate 210. The first hole 250 may be formed before, during, or after bonding the first glass substrate 210 to the first foil 230.

[0132] refer to Fig.12 And as Fig.13 As shown, after the method 100 is ended and the method 100 is repeated, the method 150 of producing a hermetically sealed package is started in which the foil is bonded to the coated glass at an oblique angle to produce a second glass substrate 310 bonded to a second foil 330, thereby forming a third bonding location 336 and a fourth bonding location 338 between the second glass substrate 310 and the second foil 330 to form a second hole 350 on the second glass substrate 310. In an embodiment, an AR coating 320 may be applied to the first surface 312 of the second glass substrate 310. In an embodiment, the AR coating 320 may be the same as the AR coating 220. In an embodiment, the AR coating 220 and the AR coating 320 are different (e.g., have different wavelength ranges). In an embodiment, the AR coating may not be applied to the first surface 312.

[0133] The method 150 starts at block 152 where the second surface 233 of the first foil 230 is positioned adjacent to the second surface 333 of the second foil 330. In an embodiment, during positioning the second surface 233 of the first foil 230 adjacent to the second surface 333 of the second foil 330, the first bonding location 236 may be aligned with the third bonding location 336.

[0134] Reference again Fig.12 And as Fig.14 As shown, the method 150 continues at block 154 by positioning the assembly 400 between the first glass substrate 210 and the second glass substrate 310. In an embodiment, the assembly 400 may include a polymer. In an embodiment, the assembly 400 may include a material or may be configured such that the resulting hermetically sealed package is configured for use in a television, a sensor, an optical device, an organic light emitting diode display, a 3D inkjet printer, a solid state light source, or a photovoltaic structure.

[0135] Reference again Fig.12 And as Fig.15 As shown, the method 150 continues at block 156 by sealing the first foil 230 and the second foil 330 to form the foil joint location 408 and produce the hermetically sealed package 500. In an embodiment, the sealing step may include sealing the first foil 230 and the second foil 330 using any conventional metal-to-metal welding process, such as laser welding (e.g., via the laser beam 242), seam welding, or resistance welding.

[0136] In an embodiment, during the sealing step, the foil engagement position 408 may be offset from the first engagement position 236 and the third engagement position 336. Fig.15 As shown, the first glass substrate 210 and the second glass substrate 310 of the hermetically sealed package 500 are spaced apart and not bonded to each other, so that the hermetically sealed package 500 has elasticity and flexibility.

[0137] Although pressure may be applied during the welding step of method 100, no pressure is applied after assembly 400 is positioned between first glass substrate 210 and second glass substrate 310, which mitigates deformation of assembly 400 between glass substrates 210, 310 and the resulting hermetically sealed package 500. Any thermal expansion of assembly 400 due to laser beam 242 during welding may be compensated by deformation of foils 230, 330.

[0138] refer to Fig.16 , an alternative embodiment of the hermetically sealed package 500 further includes an AR coating 225 applied to the second surface 214 of the first glass substrate 210 and an AR coating 325 applied to the second surface 314 of the second glass substrate 310. In an embodiment, the AR coatings 225, 325 melt when the foils 230, 330 are bonded to the glass substrates 210, 310, respectively, resulting in the foils 230, 330 being directly bonded to the glass substrates 210, 310, respectively.

[0139] In an embodiment, any or all of the AR coatings 220, 225, 320, 325 may include the same quality (e.g., wavelength range). In other embodiments, any or all of the AR coatings 220, 225, 320, 325 may include different qualities. In an embodiment, the hermetically sealed package 500 may include only one of the AR coatings 220, 225, 320, and 325. In an embodiment, the hermetically sealed package 500 includes only two of the AR coatings 220, 225, 320, and 325. In an embodiment, the hermetically sealed package 500 includes only three of the AR coatings 220, 225, 320, and 325. Example

[0140] In order to more readily understand the various embodiments, reference is made to the following examples, which are intended to illustrate various embodiments of the laser bonding methods described herein.

[0141] Reference now Fig.17, shows the reflectivity of average polarized light incident on an AR coating at several angles, the AR coating having a wavelength range corresponding to the visible spectrum of 400nm to 700nm ("Example AR Coating"). As illustrated, when the junction wavelength is outside the wavelength range of the AR coating, the reflectivity increases even at normal incidence. Increasing the incident angle of the light exacerbates this effect.

[0142] Reference now Fig.18 , shows the reflectivity of average polarized light incident on an AR coating at several angles, the AR coating having been modified to have an extended wavelength range of 400nm to 850nm ("modified AR coating"). As illustrated, extending the wavelength range to longer wavelengths reduces the reflectivity at longer wavelengths for light incident at normal and non-normal angles, while the larger the angle of incidence, the more the wavelength range shifts to a lower wavelength range.

[0143] Reference now Fig.19 , showing incident on an example AR coating ( Fig.19 and "E1" in subsequent figures) and modified AR coating ( Fig.19 , and "M1" in subsequent figures). As shown, there is no significant improvement or degradation between the two coatings under 532nm light, and in both cases, the reflectivity increases with increasing angle of incidence.

[0144] Reference now Fig. 20 , shows the angular dependence of the reflectivity of 532 nm wavelength p-polarized light (i.e., light polarized parallel to the plane of incidence) incident on an example AR coating and a modified AR coating. The p-polarization of the light results in a decrease in the effect on the reflectivity associated with an increase in the angle of incidence, as previously described in Fig.19 As shown in Figure 2, both coatings maintain a reflectivity below 2% at incident angles up to 60 degrees.

[0145] Reference now Fig.21 , shows the angular dependence of reflectivity for unpolarized light of 750 nm wavelength (i.e., outside the visible spectrum) incident on an example AR coating and a modified AR coating. As might be expected, the modified AR coating exhibits lower reflectivity at all measured incident angles due to its extended wavelength range.

[0146] Reference now Fig. 22 , shows the angular dependence of the reflectivity of 750 nm wavelength p-polarized light incident on the example AR coating and the modified AR coating. Fig.19 and 20Unlike the results comparing unpolarized and p-polarized 532 nm light in Figure 2, p-polarized 750 nm light does not show a significant decrease in reflectivity associated with an increase in the angle of incidence compared to unpolarized 750 nm light. The p-polarized 750 nm light shows results similar to Fig.21 The results for unpolarized 750nm light are shown in Figure 2, except that the reflectivity of light incident on the modified AR is reduced at incident angles between 10 and 50 degrees.

[0147] It is obvious to those skilled in the art that various modifications and changes can be made to the embodiments described herein without departing from the spirit and scope of the subject matter claimed. Therefore, it is intended that the specification covers various modifications and changes of the embodiments described herein, as long as these modifications and changes fall within the scope of the attached claims and their equivalents.

Claims

1. A method for laser bonding glass to metal foil, the method comprising: applying an antireflective coating to a first surface of a first glass substrate, the first glass substrate having a second surface opposite the first surface; bringing the second surface of the first glass substrate into contact with the first surface of the first foil to create a first contact location between at least a portion of the second surface of the first glass substrate and the first surface of the first foil; disposing the first surface of the first foil optically downstream of the first glass substrate; as well as a welding step to bond the second surface of the first glass substrate to the first foil by directing a laser beam having a first wavelength at an oblique angle relative to the first surface of the first glass substrate and over at least a portion of the first contact location, wherein: The anti-reflection coating has a tilted wavelength range corresponding to the tilt angle, and at the tilt angle, the anti-reflection coating has an average reflectivity of less than or equal to about 5% in the entire tilted wavelength range, and The tilted wavelength range includes the wavelength of the laser beam.

2. The method according to claim 1, characterized in that The antireflective coating has an average reflectivity of less than or equal to about 4% over the entire tilted wavelength range.

3. The method according to claim 1, characterized in that The antireflective coating has an average reflectivity of less than or equal to about 3% over the entire tilted wavelength range.

4. The method according to claim 1, characterized in that The tilted wavelength range is greater than or equal to 375 nm and less than or equal to 800 nm.

5. The method according to claim 1, characterized in that The antireflective coating includes a plurality of layers, wherein the plurality of layers includes a first low refractive index layer and a second high refractive index layer.

6. The method according to claim 5, characterized in that A refractive index difference between the first low refractive index layer and the second high refractive index layer is greater than or equal to 0.

01.

7. The method according to claim 5, characterized in that The first low-refractive index layer has a refractive index greater than or equal to 1.3 and less than or equal to 1.

7.

8. The method according to claim 5, characterized in that The second high refractive index layer has a refractive index greater than 1.

7.

9. The method according to claim 5, characterized in that The first low refractive index layer includes SiO2, Al2O3, GeO2, SiO, AlO x N y 、SiO x N y 、Si u Al v O x N y , MgO, MgAl2O4, MgF2, BaF2, CaF2, DyF3, YbF3, YF3 and CeF3 or a combination thereof.

10. The method according to claim 5, characterized in that The second high refractive index layer includes Si u AlvOxNy, Ta2O5, Nb2O5, AlN, Si3N4, AlO x N y 、SiO x N y , HfO2, TiO2, ZrO2, Y2O3, Al2O3, MoO3, diamond-like carbon, or a combination thereof.

11. The method according to claim 5, characterized in that The anti-reflection coating includes a plurality of periods such that the first low refractive index layers and the second high refractive index layers alternate.

12. The method according to claim 11, characterized in that The antireflection coating includes greater than or equal to 2 and less than or equal to 20 periods.

13. The method according to any one of claims 1 to 12, characterized in that The tilt angle incident on the first surface of the first glass substrate is greater than 0° and less than or equal to 60°.

14. The method according to any one of claims 1 to 12, characterized in that The laser beam includes a pulsed laser.

15. The method according to claim 14, characterized in that The pulse laser is a nanosecond pulse laser, a picosecond pulse laser or a femtosecond pulse laser.

16. The method according to claim 14, characterized in that The pulse laser comprises: Pulse energy greater than or equal to 2.8 μJ and less than or equal to 1000 μJ; A wavelength greater than or equal to 300 nm and less than or equal to 1100 nm; A repetition rate greater than or equal to 5 kHz and less than or equal to 1 MHz; and Spot size greater than or equal to 5 μm and less than or equal to 50 μm.

17. The method according to any one of claims 1 to 12, characterized in that The first foil includes aluminum, aluminum alloy, stainless steel, nickel, nickel alloy, silver, silver alloy, titanium, titanium alloy, tungsten, tungsten alloy, gold, gold alloy, copper, copper alloy, bronze, iron, or a combination thereof.

18. The method according to any one of claims 1 to 12, characterized in that The first foil comprises a thickness greater than or equal to 5 μm and less than or equal to 75 μm.

19. The method according to any one of claims 1 to 12, characterized in that The first glass substrate includes a refractive index greater than or equal to 1.5 and less than or equal to 2.

4.

20. The method according to any one of claims 1 to 12, characterized in that The first glass substrate includes glass or glass ceramic, and the glass or glass ceramic includes borate glass, borosilicate glass, phosphate-based glass, silicon carbide glass, soda-lime silicate glass, aluminosilicate glass, alkali aluminosilicate glass, borosilicate glass, alkali borosilicate glass, aluminoborosilicate glass, alkali aluminoborosilicate glass, alkali aluminoborosilicate glass or niobium tungsten lanthanum boron glass.

21. A welding product comprising: a first glass substrate, the first glass substrate comprising a first surface and a second surface opposite to the first surface; an anti-reflection coating disposed on the first surface of the first glass substrate, the anti-reflection coating having a tilted wavelength range, wherein the anti-reflection coating has an average reflectivity less than or equal to about 5% over the entire tilted wavelength range; a first foil disposed on the second surface of the glass substrate; and A first interface weld is disposed between the first surface of the metal foil and the second surface of the glass substrate.

22. The welded product according to claim 21, characterized in that The welded product is a hermetically sealed package.

23. The welded product according to claim 21, characterized in that The tilted wavelength range is greater than or equal to 375 nm and less than or equal to 800 nm.

24. The welded product according to claim 21, wherein: The antireflective coating has an average reflectivity of less than or equal to about 4% over the entire tilted wavelength range.

25. The welded product according to claim 21, wherein: The antireflective coating includes a plurality of layers, wherein the plurality of layers includes a first low refractive index layer and a second high refractive index layer.

26. The welded product according to claim 25, characterized in that A refractive index difference between the first low refractive index layer and the second high refractive index layer is greater than or equal to 0.

01.

27. The welded product according to claim 25, characterized in that The first low-refractive index layer has a refractive index greater than or equal to 1.3 and less than or equal to 1.

7.

28. The welded product according to claim 25, characterized in that The second high refractive index layer has a refractive index greater than 1.

7.

29. The welded product according to claim 25, characterized in that The first low refractive index layer includes SiO2, Al2O3, GeO2, SiO, AlO x N y 、SiO x N y 、Si u Al v O x N y , MgO, MgAl2O4, MgF2, BaF2, CaF2, DyF3, YbF3, YF3 and CeF3 or a combination thereof.

30. The welded product according to claim 25, wherein: The second high refractive index layer includes Si u AlvOxNy, Ta2O5, Nb2O5, AlN, Si3N4, AlO x N y 、SiO x N y , HfO2, TiO2, ZrO2, Y2O3, Al2O3, MoO3, diamond-like carbon, or a combination thereof.

31. The welded product according to claim 25, wherein: The anti-reflection coating includes a plurality of periods such that the first low refractive index layers and the second high refractive index layers alternate.

32. The welded product according to claim 25, wherein: The antireflection coating includes greater than or equal to 2 and less than or equal to 20 periods.

33. The welded product according to any one of claims 21 to 32, characterized in that The first foil includes aluminum, aluminum alloy, stainless steel, nickel, nickel alloy, silver, silver alloy, titanium, titanium alloy, tungsten, tungsten alloy, gold, gold alloy, copper, copper alloy, bronze, iron, or a combination thereof.

34. The welded product according to any one of claims 21 to 32, characterized in that The first foil comprises a thickness greater than or equal to 5 μm and less than or equal to 75 μm.

35. The welded product according to any one of claims 21 to 32, characterized in that The first glass substrate includes a refractive index greater than or equal to 1.5 and less than or equal to 2.

4.

36. The welded product according to any one of claims 21 to 32, characterized in that The first glass substrate includes glass or glass ceramic, and the glass or glass ceramic includes borate glass, borosilicate glass, phosphate-based glass, silicon carbide glass, soda-lime silicate glass, aluminosilicate glass, alkali aluminosilicate glass, borosilicate glass, alkali borosilicate glass, aluminoborosilicate glass, alkali aluminoborosilicate glass, alkali aluminoborosilicate glass or niobium tungsten lanthanum boron glass.

Citation Information

Patent Citations

  • Process for making of glass articles with optical and easy-to-clean coatings

    US20140113083A1

  • Durable and scratch-resistant anti-reflective articles

    US9335444B2