Low-melt-index, high-modulus and high-impact polypropylene resin as well as preparation method and application thereof
Through the combination of batch process and specific additives, the problem of inflexible switching grades in polypropylene resin production is solved, and the problem of high rigidity and high toughness is difficult to meet high rigidity and high toughness is prepared. Low melting finger, high modulus, and high impact polypropylene resin is suitable for Polypropylene wound sewage pipes meet high performance standards.
Patent Information
- Application Number
- CN202410819100.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-24
AI Technical Summary
In the prior art, when producing polypropylene resins with low melt fingers, high modulus and high impact resistance, the switching grade is inflexible and difficult to meet the requirements of high rigidity and high toughness at the same time.
By adopting batch process, polypropylene powder is obtained by adding external electron donor, main catalyst, co-catalyst and refined propylene to the polymerization kettle, and polypropylene powder is obtained and the main antioxidant, auxiliary antioxidant, and stearin is employed. Calcium acid, β-crystal nucleating agent and copolymerized polypropylene resin containing ethylene phase were mixed, and extruded and granulated by a twin screw extruder to prepare low-melt finger, high modulus, and high impact polypropylene resin.
The flexibility of grade switching and the reduction of transition materials are achieved, and polypropylene resin with high rigidity and high toughness is obtained. The bending modulus can reach more than 1600MPa, the impact strength of room temperature can reach more than 110kJ/m2, and the impact strength of low temperature (- 20℃) can reach more than 5kJ/m2, meeting the A-level indicators of GB T 35451.2-2018 standards.
Smart Images

Figure BDA0004908607720000071 
Figure BDA0004908607720000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material synthesis, and in particular to a low melt index, high modulus, high impact polypropylene resin and a preparation method and application thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Polypropylene with low melt index, high modulus and high impact resistance is the main raw material for winding drainage pipes. Compared with traditional polyethylene double-wall corrugated pipes, fiberglass pipes, cement pipes, etc. for drainage, this kind of pipe has significant advantages in chemical resistance and anti-aging performance, and is very suitable for municipal, construction, farmland and highway rain and sewage discharge projects. When dealing with extraordinary rainfall or large-scale drainage, large-diameter high-modulus polypropylene winding pipes have obvious advantages. Compared with traditional PE and PVC pipes, polypropylene winding drainage pipes have the following advantages: high modulus leads to high ring stiffness and better ability to resist external loads; low density, light weight, and material saving; good shaping, small pipe shrinkage, and higher flow rate; high tensile strength, better resistance to bending deformation and stretching, and resistance to geological settlement.
[0004] At present, the production of polypropylene with low melt index, high modulus and high impact resistance is based on the ring tube process. However, this process is continuous production, the switching of grades is not flexible, and a lot of transition materials are produced. At the same time, the polypropylene material prepared by this method is difficult to meet the requirements of good rigidity and toughness at the same time. Therefore, how to provide a polypropylene resin with low melt index, high modulus and high impact resistance based on an intermittent process, so that it is suitable for the production of winding pipes, is an urgent problem to be solved. Summary of the invention
[0005] In view of this, the present invention provides a low melt index, high modulus, high impact polypropylene resin and a preparation method and application thereof, which solves the problem that when producing polypropylene resin by the ring tube process, switching grades is inflexible and the produced polypropylene resin is difficult to simultaneously meet high rigidity and high toughness.
[0006] In a first aspect, the present invention provides a method for preparing a low melt index, high modulus, high impact polypropylene resin, comprising the following steps:
[0007] Adding an external electron donor, a main catalyst, a co-catalyst and purified propylene into a polymerization kettle, introducing hydrogen to carry out polymerization reaction, and obtaining polypropylene powder;
[0008] The polypropylene powder is mixed with a primary antioxidant, an auxiliary antioxidant, calcium stearate, a β-crystal nucleating agent and a copolymerized polypropylene resin containing an ethylene phase, and the mixture is extruded and granulated by a twin-screw extruder to obtain the product.
[0009] Preferably, the external electron donor is selected from dicyclopentyldimethoxysilane.
[0010] Preferably, the main catalyst is TiC1 4 / MgC1 2 The catalyst has a mass fraction of Ti in the main catalyst of 2 to 4 wt %; and the addition amount of the main catalyst is 12 to 60 g per ton of propylene.
[0011] Preferably, the co-catalyst is triethylaluminum; the molar ratio of Al in the triethylaluminum to Ti in the main catalyst is (200-240):1.
[0012] Preferably, the amount of the external electron donor added is 15 to 55 mL per ton of propylene.
[0013] Preferably, the polymerization reaction pressure is 3-3.8 MPa, the polymerization reaction temperature is 65-82° C., and the polymerization reaction time is 2-3 h.
[0014] Preferably, the concentration of the hydrogen is 200-300 ppm.
[0015] Preferably, the mass ratio of the polypropylene powder, the primary antioxidant, the auxiliary antioxidant, calcium stearate, the β-crystal nucleating agent and the copolymerized polypropylene resin containing the ethylene phase is 100:(0.1-0.3):(0.05-0.2):(0.02-0.1):(0.02-0.15):(3-10).
[0016] Preferably, the main antioxidant is antioxidant 1010, and the auxiliary antioxidant is antioxidant 168.
[0017] Preferably, in the copolymerized polypropylene resin containing an ethylene phase, the ethylene phase content is 1 to 5 wt%.
[0018] In a second aspect, the present invention provides a low melt index, high modulus, high impact polypropylene resin prepared by the above preparation method.
[0019] In a third aspect, the present invention provides the use of the low melt index, high modulus, high impact polypropylene resin in the preparation of polypropylene wound sewage pipes.
[0020] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0021] (1) The present invention adopts an intermittent bulk process to prepare a low melt index, high modulus, high impact polypropylene resin, which can be easily switched between grades with less transition material;
[0022] (2) In the production process of polypropylene resin, the present invention prepares a polypropylene resin with low melt index, high modulus and high impact resistance by adding appropriate additives, which has both high rigidity and high toughness, a flexural modulus of more than 1600 MPa, and a room temperature impact strength of 110 kJ / m 2 Above, low temperature impact strength (-20℃) can reach 5kJ / m 2 Above, and the melt index is below 0.3g / 10min, which is suitable as a special material for polypropylene wrapped sewage pipes, and meets the A-level index of melt mass flow rate in GB T 35451.2-2018 standard. DETAILED DESCRIPTION
[0023] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0024] The present invention provides a method for preparing a low melt index, high modulus, and high impact polypropylene resin, comprising the following steps:
[0025] Adding an external electron donor, a main catalyst, a co-catalyst and purified propylene into a polymerization kettle, introducing hydrogen to carry out polymerization reaction, and obtaining polypropylene powder;
[0026] The polypropylene powder is mixed with a primary antioxidant, an auxiliary antioxidant, calcium stearate, a β-crystal nucleating agent and a copolymerized polypropylene resin containing an ethylene phase, and the mixture is extruded and granulated by a twin-screw extruder to obtain the product.
[0027] The present invention does not impose any special restrictions on the refining process of propylene, and the refining method commonly used in the art can be used. The present invention preferably passes the raw material propylene through a solid alkali tower, a hydrolysis tower, a desulfurization tower, a drying tower, a sample removal tower, a molecular sieve drying tower, and a desulfurization phosphorus arsenic tower once to purify the polypropylene raw material to obtain the propylene raw material for polymerization reaction. The present invention does not impose any special restrictions on the specific process conditions of the solid alkali tower, the hydrolysis tower, the desulfurization tower, the drying tower, the deoxygenation tower, the molecular sieve drying tower, and the desulfurization phosphorus arsenic tower, and the refining parameters commonly used by those skilled in the art can be used.
[0028] In the present invention, the external electron donor is selected from dicyclopentyldimethoxysilane. In the present invention, the main catalyst is selected from TiC1 4 / MgC1 2The catalyst has a mass fraction of Ti of 2 to 4 wt% in the main catalyst; and the addition amount of the main catalyst is 12 to 60 g per ton of propylene. The selection of a suitable external electron donor and main catalyst can improve the isotacticity and bending strength of the polypropylene resin.
[0029] In the present invention, the cocatalyst is triethylaluminum; the molar ratio of Al in the triethylaluminum to Ti in the main catalyst is (200-240): 1. The main function of the cocatalyst is to remove trace impurities in propylene and improve the reaction activity.
[0030] In the present invention, the added amount of the external electron donor is 15 to 55 mL per ton of propylene.
[0031] In the present invention, the polymerization reaction pressure is 3-3.8 MPa, the polymerization reaction temperature is 65-82° C., and the polymerization reaction time is 2-3 h.
[0032] In the present invention, the concentration of hydrogen in each ton of propylene is 200-300 ppm. The melting index of the polypropylene resin is regulated by controlling the amount of hydrogen added.
[0033] In the present invention, the mass ratio of the polypropylene powder, the primary antioxidant, the auxiliary antioxidant, calcium stearate, the β-crystal nucleating agent and the copolymerized polypropylene resin containing the ethylene phase is 100: (0.1-0.3): (0.05-0.2): (0.02-0.1): (0.02-0.15): (3-10). The addition of calcium stearate can play a certain reinforcing role, improve the processing properties of polypropylene, and improve the impact resistance and thermal stability of polypropylene.
[0034] The present invention finds that the β-crystal nucleating agent and the copolymerized polypropylene resin containing an ethylene phase can have a significant effect on the toughness of the polypropylene resin. The appropriate addition of the β-crystal nucleating agent and the copolymerized polypropylene resin containing an ethylene phase can improve the low-temperature toughness and room-temperature toughness of the polypropylene resin. However, excessive addition of the β-crystal nucleating agent and the copolymerized polypropylene resin containing an ethylene phase will lead to a significant reduction in rigidity.
[0035] In the present invention, the primary antioxidant is antioxidant 1010, and the auxiliary antioxidant is antioxidant 168. The primary antioxidant and the auxiliary antioxidant can play a synergistic role in preventing the oxidative decomposition of polypropylene.
[0036] In the present invention, the content of ethylene phase in the copolymerized polypropylene resin containing ethylene phase is 1-5wt%. The introduction of ethylene phase can improve the low-temperature impact performance of the final polypropylene resin.
[0037] The present invention also provides a low melt index, high modulus, high impact polypropylene resin prepared by the above preparation method. The low melt index, high modulus, high impact polypropylene resin obtained by the present invention has both rigidity and toughness, a bending modulus of more than 1600MPa, and a room temperature impact strength of 110kJ / m 2 Above, low temperature impact strength (-20℃) can reach 5kJ / m 2 Above, and the melt index is below 0.3g / 10min, which is suitable as a special material for polypropylene wrapped sewage pipes, and meets the A-level index of melt mass flow rate in GB T 35451.2-2018 standard.
[0038] The present invention also provides the use of the low melt index, high modulus and high impact polypropylene resin in the preparation of polypropylene wound sewage pipes.
[0039] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0040] Example 1
[0041] This embodiment provides a method for preparing a low melt index, high modulus, and high impact polypropylene resin.
[0042] The raw material propylene enters the refining unit of the device. The raw material propylene first enters the solid alkali tower to remove trace acidic substances, inorganic sulfur and most of the trace water, and then passes through the hydrolysis tower and desulfurization tower to remove organic sulfur. After that, it enters the alumina drying tower to remove trace water, and enters the deoxygenation tower to remove trace oxygen. Water will be generated in this process. Then it enters the molecular sieve drying tower to remove trace impurities and trace water, and finally enters the desulfurization and dephosphorization tower. After the water, oxygen, sulfur and other test results are qualified, it can be used for polymerization. The propylene is pumped into the polymerization unit.
[0043] The co-catalyst triethylaluminum was pressed into the co-catalyst metering tank by nitrogen.
[0044] Under the protection of nitrogen, the external electron donor dicyclopentyldimethoxysilane is flushed into the polymerization kettle.
[0045] Open the catalyst hopper and, under the protection of nitrogen, add the main catalyst TiC1 4 / MgC1 2 (Ti content is 3wt%, catalyst model is S-copo) is poured into the catalyst feeding port, and the main catalyst is flushed into the polymerization kettle with propylene.
[0046] Open the hydrogen valve on the polymerization kettle and add hydrogen into the polymerization kettle.
[0047] Continue to add propylene, and when the propylene reaches the set value, close the propylene feed valve.
[0048] Start the heating system and slowly heat up the temperature, then enter the constant temperature stage, react at the constant temperature for 2.5 hours, open the propylene recovery valve, recover the unreacted propylene monomer, and the recovered propylene is condensed and then enters the propylene recovery tank as recycled material for standby use as raw material.
[0049] The flash kettle is replaced with nitrogen, and the polypropylene powder in the polymerization kettle is pressed into the flash kettle. The nitrogen is replaced several times until the volume content of propylene in the tail gas is less than 0.8%, and the polypropylene powder enters the granulator.
[0050] The extrusion granulation processing conditions of the twin-screw extruder are adjusted, and 2kg of antioxidant 1010, 1kg of antioxidant 168, 0.5kg of calcium stearate, 0.3kg of β-crystal nucleating agent NA-328, and 50kg of ethylene-containing copolymer polypropylene resin EP200R (ethylene phase content is 3wt%) are added to each ton of polypropylene powder, and the final product, polypropylene wrapped sewage pipe special material, is obtained through extrusion granulation.
[0051] The polymerization reaction conditions in this embodiment are shown in Table 1, and the extrusion granulation processing conditions of the twin-screw extruder are shown in Table 2.
[0052] Table 1 Example 1 Polymerization conditions
[0053]
[0054] Example 2
[0055] The difference between this embodiment and embodiment 1 is that the addition amount of the copolymerized polypropylene resin EP200R (ethylene phase content is 3 wt%) containing ethylene phase in this embodiment is 80 kg (per ton of polypropylene powder).
[0056] Example 3
[0057] The difference between this embodiment and embodiment 1 is that the addition amount of the beta crystal nucleating agent NA-328 in this embodiment is 0.5 kg (per ton of polypropylene powder).
[0058] Comparative Example 1
[0059] The difference between this comparative example and Example 1 is that the β-crystal nucleating agent NA-328 and the copolymerized polypropylene resin EP200R containing an ethylene phase are not added in this comparative example.
[0060] Comparative Example 2
[0061] The difference between this comparative example and Example 1 is that the copolymerized polypropylene resin EP200R containing an ethylene phase is not added in this comparative example.
[0062] Comparative Example 3
[0063] The difference between this comparative example and Example 1 is that the addition amount of the copolymerized polypropylene resin EP200R (ethylene phase content is 3 wt%) containing ethylene phase in this comparative example is 150 kg (per ton of polypropylene powder).
[0064] Comparative Example 4
[0065] The difference between this comparative example and Example 1 is that the addition amount of the β-crystal nucleating agent NA-328 in this comparative example is 2 kg.
[0066] Comparative Example 5
[0067] The difference between this comparative example and Example 1 is that the external electron donor in this comparative example is cyclohexylmethyldimethoxysilane.
[0068] Test example
[0069] The properties of the polypropylene resins of Examples 1 to 3 and Comparative Examples 1 to 5 were measured, and the test results are shown in Table 2.
[0070] Table 2 Determination of polypropylene resin properties of Examples 1 to 3 and Comparative Examples 1 to 5
[0071]
[0072] Note: The flexural modulus test standard is GB / T 9341-2008; the room temperature impact strength is measured at 23°C, and the low temperature impact strength is measured at -20°C. The test standard is GB / T 1043.1-2008; the melt index test standard is GB / T3682.1-2018.
[0073] As can be seen from Table 2, since no nucleating agent and copolymerized PP were added to Comparative Example 1, the room temperature and low temperature impacts were greatly reduced, and the flexural modulus and tensile strength were increased; compared with Comparative Example 1, a nucleating agent was added to Comparative Example 2, and the room temperature impact resistance was greatly improved, but the flexural modulus decreased; in Comparative Example 3, the amount of copolymerized polypropylene resin containing ethylene phase added was too much, resulting in a significant decrease in the flexural modulus and tensile strength, and the low-temperature impact performance and room temperature impact performance were also reduced; in Comparative Example 4, the amount of nucleating agent added was too much, which also caused a significant decrease in the flexural modulus and tensile strength, and a slight decrease in the low-temperature impact performance and room temperature impact performance; in Comparative Example 5, the external electron donor was replaced with cyclohexylmethyldimethoxysilane, and it can be seen that its rigidity and toughness related values were slightly reduced compared with Example 1.
[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a low melt index, high modulus, high impact polypropylene resin, characterized in that: The steps include: Adding an external electron donor, a main catalyst, a co-catalyst and purified propylene into a polymerization kettle, introducing hydrogen to carry out polymerization reaction, and obtaining polypropylene powder; The polypropylene powder is mixed with a primary antioxidant, an auxiliary antioxidant, calcium stearate, a β-crystal nucleating agent and a copolymerized polypropylene resin containing an ethylene phase, and the mixture is extruded and granulated by a twin-screw extruder to obtain the product.
2. The preparation method according to claim 1, characterized in that The external electron donor is selected from dicyclopentyldimethoxysilane; and the added amount of the external electron donor is 15 to 55 mL per ton of propylene.
3. The preparation method according to claim 1, characterized in that: The main catalyst is a TiC14 / MgC12 catalyst, the mass fraction of Ti in the main catalyst is 2-4wt%; the addition amount of the main catalyst is 12-60g per ton of propylene.
4. The preparation method according to claim 3, characterized in that: The co-catalyst is triethylaluminum; the molar ratio of Al in the triethylaluminum to Ti in the main catalyst is (200-240):
1.
5. The preparation method according to claim 1, characterized in that: The polymerization reaction pressure is 3-3.8 MPa, the polymerization reaction temperature is 65-82° C., and the polymerization reaction time is 2-3 hours.
6. The preparation method according to claim 1, characterized in that: The concentration of the hydrogen is 200-300 ppm.
7. The preparation method according to claim 1, characterized in that: The mass ratio of the polypropylene powder, the primary antioxidant, the auxiliary antioxidant, calcium stearate, the beta crystal nucleating agent and the copolymerized polypropylene resin containing the ethylene phase is 100: (0.1-0.3): (0.05-0.2): (0.02-0.1): (0.02-0.15): (3-10).
8. The preparation method according to claim 7, characterized in that: The main antioxidant is antioxidant 1010, and the auxiliary antioxidant is antioxidant 168; In the copolymerized polypropylene resin containing an ethylene phase, the content of the ethylene phase is 1 to 5 wt%.
9. The low melt index, high modulus, high impact polypropylene resin prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the low melt index, high modulus, high impact polypropylene resin as claimed in claim 9 in the preparation of polypropylene wound sewage pipes.
Citation Information
Patent Citations
High-melt index polypropylene composition and preparation method thereof
CN103571039A
High-transparency and high-impact polypropylene resin suitable for blow molding process
CN107880402A
Method for preparing low-odor polypropylene by intermittent liquid-phase bulk process
CN111454518A
High-impact transparent polypropylene resin and preparation method thereof
CN114058113A
Catalytic system for preparing ultra-pure isotactic polypropylene and application of catalytic system
CN117510687A