A new type of acid scavenger and its application in polymer system

By using a new acid absorber with intercalated composite layered structure in polyolefin materials, combined with phosphate ion insertion and nitrogen doping technology, the precipitation, adsorption capacity and cost of existing acid absorbers are solved, and the polymerization is significantly improved The stability and processing properties of the material materials replace the high-priced DHT-4A hydrotalcite.

CN116081679BActive Publication Date: 2024-11-26XINER (SHANDONG) NEW MATERIAL TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310148232.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-11-26
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

The acid absorbents in existing polyolefin materials have problems such as precipitation residues, insufficient adsorption capacity, high cost and low stability, which affect the long-term performance of polymer materials and the safety of processing processes.

Method used

A new type of acid absorbent with an intercalated composite layer structure is used to optimize the structure and components of the acid absorbent, and improve its adsorption amount to acid ions and Dispersibility and compound with azine-based substance and phosphite-based substance in the polymer system to enhance the stability and aging resistance of the material.

Benefits of technology

It significantly improves the acid absorption and aging resistance of polymer materials, reduces costs, replaces the high-priced Japan Union DHT-4A hydrotalcite, and enhances the stability and processing performance of the polymer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004089836320000121
    Figure BDA0004089836320000121
Patent Text Reader

Abstract

The present application provides a novel acid absorbent, the structural formula of which is: 2+ x M 3+ y (OH) m (X n‑ ) z ; wherein the M 2+ M is a divalent metal ion. 3+ is a trivalent metal ion, wherein X n‑ The invention discloses an anion having an ‑n valence, wherein x:y is (0.1‑2.5):(0.3‑4), m=2(x+1), n ​​is an integer of 1‑5, and z=(3y‑2) / n. The acid absorber has low cost, good acid absorption performance, and excellent stability to polymer materials, and can effectively replace DHT‑4A of Kyowa of Japan, and is applied to the processing of polymer materials such as PP products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of acid absorbers, C08K9 / 00, and in particular to a novel acid absorber and application thereof in a polymer system. Background Art

[0002] Ziegler-Natta catalysts that are easy to remain are often used in the synthesis of polyolefin materials, which results in a certain amount of titanium chloride in the polyolefin materials, causing discoloration or reduction of mechanical structure of polyolefin products during long-term use; in addition, acidic chloride ions are corrosive and easily cause equipment damage during polyolefin processing. Metal stearates and hydrotalcites are common acid absorbers; however, metal stearates have a precipitation effect, are easy to remain on processing equipment, and have low acid absorption capacity; Japan Kyowa hydrotalcite DHT-4A has a low water content and a refractive index similar to that of polyolefins, and is widely used in the field of polymer processing, but the price of DHT-4A is very high, which significantly increases the production and processing costs of polyolefin products.

[0003] Chinese patent CN104558775A discloses a hydrotalcite acid absorber for polyolefins, which is doped with calcium ions to make magnesium aluminum hydrotalcite have a large number of adsorbable active sites, thereby improving the adsorption of acid ions. However, the hydrotalcite in the technology has low high temperature stability, insufficient adsorption of acid ions, and the stabilization effect on polyolefin materials needs to be strengthened. Therefore, it is necessary to develop an acid absorber with low cost, good acid absorption effect, and can significantly improve the stability and aging resistance of polyolefin materials for actual industrial production application. Summary of the invention

[0004] In order to solve the above technical problems, the present invention first provides a new acid absorber, whose structural formula is expressed as: 2 + x M 3+ y (OH) m (X n- ) z ; wherein the M 2+ M is a divalent metal ion. 3+ is a positive trivalent metal ion, said X n- It is an anion with a valence of -n, wherein x:y is (0.1-2.5):(0.3-4), m=2(x+1), n ​​is an integer of 1-5, and z=(3y-2) / n.

[0005] Furthermore, the acid absorbent of the present application has an intercalated composite layered structure; 2+ and M 3+ The hydroxides constitute the composite layered structure of the acid absorber.

[0006] Furthermore, the M 2+ Including Ni 2+ 、Zn 2+ Mg 2+ , Ca 2+ , Cu 2+ , Mn 2+ , Fe 2+ At least one of .

[0007] Preferably, the M 2+ Including Zn 2+ and Mg 2+ .

[0008] Furthermore, the M 2+ Medium Zn 2+ and Mg 2+ The molar ratio is (0.2-2.2):(0.3-1.5).

[0009] Furthermore, the M 3+ Including Al 3+ , Fe 3+ Cr 3+ 、Co 3+ , Ga 3+ 、In 3+ At least one of .

[0010] Preferably, the M 3+ Including Al 3+ ; The x:y is (0.5-2):(0.3-3).

[0011] Furthermore, the M 2+ and M 3+ The sources include, but are not limited to, at least one of its halides, nitrates, carbonates, bicarbonates, sulfates, hypochlorites, perchlorates, thiosulfates, hydroxides, and oxides.

[0012] Furthermore, the X n- Any one of -1, -2, -3, -4, -5 anions, including but not limited to (NO3) - 、(ClO4) - 、(IO3) - 、(H2PO4) - 、(HCO3) - 、(CO3) 2- 、(SO3) 2- 、(S2O3) 2- 、(SiO3) 2- 、(SO4) 2- 、(WO4) 2-、(CrO4) 2- 、(HPO4) 2- 、(PO4) 3- At least one of .

[0013] Preferably, the X n- (CO3) 2- 、(NO3) - 、(SiO3) 2- 、(PO4) 3- At least one of .

[0014] In a preferred embodiment, the X n- (PO4) 3- or (CO3) 2- . The present invention uses a layered metal hydroxide as a skeleton, inserts anions between the layers to increase the activity of the layered structure and its dispersibility in the organic system. It is found in the study that when a composite layered structure of aluminum hydroxide, zinc hydroxide and magnesium hydroxide is used and phosphate ions are inserted between the layers, the acid absorber has a greater adsorption capacity for chloride ions and a more obvious improvement effect on polymer materials. It is speculated that this may be because the insertion of phosphate between the layers will form crystal phases of magnesium phosphate, zinc phosphate and aluminum phosphate. Due to the differences in atomic or ionic radius and electron distribution, the atomic arrangement states of these crystal phases and the original interlayer hydroxides are different, and the crystal fields are also different, resulting in a large number of defect sites in the structure, which increases the adsorption capacity of chloride ions; however, it is necessary to control the relative content of ions to ensure that the defect sites are increased without destroying the original crystal structure.

[0015] Preferably, the acid scavenger is further doped with heteroatoms, wherein the heteroatoms are selected from at least one of N, P, B, Bi, and rare earth metal atoms.

[0016] Furthermore, the rare earth metal atom is selected from at least one of Pr, Nb, Er, Ce and Yb.

[0017] Preferably, the heteroatom is N.

[0018] Furthermore, the preparation method of the acid scavenger comprises the following steps:

[0019] S1. Preparation of M by coprecipitation 2+ x M 3+ y (OH) m (X n- ) z :Soluble M 2+ and M 3+ The salt is prepared into a mixed salt solution, and then X n-The mixed salt and alkali regulator are used to prepare a mixed alkali solution, the mixed salt solution and the mixed alkali solution are mixed, and after aging for 20-36 hours, the mixed salt solution is washed and dried to obtain a powder;

[0020] S2, heteroatom-doped M 2+ x M 3+ y (OH) m (X n- ) z : Mix the powder in S1 and the dopant source and calcine at 600-850°C.

[0021] Furthermore, in step S1, M 2+ Salt and M 3+ The molar ratio of the salt is (0.1-2.5):(0.3-4).

[0022] Preferably, the M 2+ Salt and M 3+ The molar ratio of the salt is (0.5-2):(0.3-3).

[0023] In a preferred embodiment, when the M 2+ Including Zn 2+ and Mg 2+ When the Zn 2+ Salt, Mg 2+ Salt and M 3+ The molar ratio of the salt is (0.2-2.2):(0.3-1.5):(0.4-1.8).

[0024] Furthermore, in the step S, the aging temperature is 60-130°C, preferably 70-90°C.

[0025] In one embodiment, the dopant source is a nitrogen source, including but not limited to at least one of urea, melamine, hydrazine hydrate, imidazole compounds, and pyridine compounds.

[0026] Preferably, the nitrogen source is urea or melamine. The present application found that when the acid absorber is treated with nitrogen, the adsorption capacity of the acid absorber will be further improved. This is because the doping of nitrogen ions in the crystal structure of the acid absorber can increase defect sites, increase the porosity and effective specific surface area of ​​the acid absorber, and nitrogen has a certain alkalinity and can show good deacidification performance.

[0027] Furthermore, in step S2, the mass ratio of the powder to the nitrogen source is (4-6):1.

[0028] Furthermore, in step S2, the calcination temperature is 700-850° C., and the calcination time is 6-10 hours.

[0029] Furthermore, the present application also provides a use of the acid scavenger in a polymer system.

[0030] Furthermore, the polymer includes but is not limited to any one or a combination of PE, PP, EVA, POE, MMA, poly-4-methyl-1-pentene, SBS, SIS, and SEBS, and is preferably any one or a combination of polyolefins such as PE, PP, EVA, and poly-4-methyl-1-pentene.

[0031] Furthermore, the acid absorber is added when the polymer is processed into a product, and the method of use is: the acid absorber, the polymer and the auxiliary agent are mixed and melt-extruded.

[0032] Furthermore, in the mixture of the acid scavenger, the polymer and the auxiliary agent, the concentration of the acid scavenger is 200-500 ppm, and the concentration of the auxiliary agent is 500-900 ppm.

[0033] Furthermore, the auxiliary agent is at least one of oxazine substances, phosphite substances, and hindered phenol substances.

[0034] Preferably, the auxiliary agent includes an oxazine substance and a phosphite substance, and the mass ratio of the two is (3-7): (2-4), and more preferably (3-5): (2-3).

[0035] Furthermore, the azine substance is selected from at least one of tris(3,3-di-tert-butyl-4-hydroxybenzyl) isocyanurate, 3,7-di(1-methyl-1-phenylethyl)-phenothiazine, and 3,7-(1,1,3,3-tetramethyl-butyl)-phenothiazine, preferably tris(3,3-di-tert-butyl-4-hydroxybenzyl) isocyanurate.

[0036] Furthermore, the phosphite substance is at least one selected from bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, tri(tridecyl)phosphite, 4,4'-isopropyl diphenyl C12-C15-ol phosphite, and poly(dipropylene glycol)phenyl phosphite, preferably bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite.

[0037] Furthermore, the hindered phenol anti-substance is selected from at least one of N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)octanediamine, and N,N'-bis-(4-(3,5-di-tert-butyl-4-hydroxyphenyl)butyryl)hexanediamine, preferably N,N'-bis-(4-(3,5-di-tert-butyl-4-hydroxyphenyl)butyryl)hexanediamine.

[0038] In a preferred embodiment, when the acid absorber of the present application is used, tris(3,3-di-tert-butyl-4-hydroxybenzyl) isocyanurate and bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite are added at the same time, and the mass ratio of the two is set to 4:3, the polymer material exhibits excellent processability, structural stability and aging resistance. The applicant speculates that tris(3,3-di-tert-butyl-4-hydroxybenzyl) isocyanurate and bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite contain a large number of polar groups or conjugated groups such as hydroxyl groups, C=O, benzene rings, etc., which can produce electron conjugation with the anionic phosphate between the acid absorber layers, and generate intermolecular forces with the N atoms or nitrogen source molecular chains therein, thereby reducing the interface effect between the inorganic powdered acid absorber and the organic material, increasing the compatibility between the organic material and the acid absorber, further optimizing the mass ratio of the two, balancing the forces within the system, and enhancing the processability, stability and aging resistance of the polymer material.

[0039] Furthermore, in step (2), the melt extrusion temperature is 240-290°C.

[0040] Furthermore, the average particle diameter of the acid scavenger is less than 10 μm, preferably less than 8 μm.

[0041] Beneficial Effects

[0042] 1. The present application first provides an acid absorber, which optimizes the intercalation structure of the acid absorber to increase the adsorption capacity of acidic ions such as chloride ions by making a large number of defect sites in different crystal phases of the structure;

[0043] 2. By doping the acid absorber with elements, the defect sites are further increased. When nitrogen source doping is used, the dispersion of the acid absorber in the organic polymer system can be improved, thereby making the stability, aging resistance and yellowing resistance of the polymer material more excellent;

[0044] 3. When using the acid absorber, compounding the azine and phosphite substances simultaneously, optimizing the components and relative contents of the two, can further improve the acid absorption and aging resistance of the polymer material, and reduce the melt index of the polymer system through appropriate intermolecular interaction, thereby improving its processing performance;

[0045] 4. The acid absorber of the present application has low cost, good acid absorption performance, and excellent stability to polymer materials. It can effectively replace DHT-4A of Kyowa of Japan and be used in the processing of polymer materials such as PP products. DETAILED DESCRIPTION

[0046] Example

[0047] Example 1

[0048] A new type of acid absorbent, the structural formula of which is: Zn 0.5 Mg 0.7 Al 1.2 (OH) 4.4 (PO4 3- ) 0.533 , the acid absorber is doped with N, and its preparation method is as follows:

[0049] S1. Dissolve 0.5 mol of zinc chloride, 0.7 mol of magnesium chloride and 1.2 mol of sodium aluminate in 500 mL of water to prepare a mixed salt solution, then add 0.533 mol of sodium phosphate and 4.4 mol of sodium hydroxide to prepare 500 mL of a mixed alkali solution, mix the mixed salt solution and the mixed alkali solution by a double drop method, age at 80 ° C for 32 hours after dropping, wash and dry to obtain a powder;

[0050] S2. Grind the powder and mix it with urea in a mass ratio of 5:1, and calcine it at 790°C for 6-10h in a nitrogen atmosphere (heating rate of 5°C / min).

[0051] The method for using the acid absorber in the polymer material is as follows:

[0052] (1) grinding the acid absorber to an average particle diameter of 8 μm, and mixing the particle with PP material (Shanghai Petrochemical, T30S), 400 ppm of tris(3,3-di-tert-butyl-4-hydroxybenzyl) isocyanurate, and 300 ppm of bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, wherein the amount of the acid absorber is 300 ppm;

[0053] (2) The mixture is mixed uniformly by a high-speed mixer and then extruded by a twin-screw extruder at an extrusion temperature of 260°C.

[0054] Example 2

[0055] A new type of acid absorbent, the structural formula of which is: Zn 0.12 Mg 0.71 Al3(OH) 3.66 (PO4 3- ) 2.33 , the acid absorber is doped with N, and its preparation method is as follows:

[0056] S1. Dissolve 0.12 mol of zinc chloride, 0.71 mol of magnesium chloride and 3.0 mol of sodium aluminate in 500 mL of water to prepare a mixed salt solution, then add 2.33 mol of sodium phosphate and 3.66 mol of sodium hydroxide to prepare 500 mL of a mixed alkali solution, mix the mixed salt solution and the mixed alkali solution by a double drop method, age at 70 ° C for 36 hours after dropping, wash and dry to obtain a powder;

[0057] S2. Grind the powder and mix it with urea in a mass ratio of 4:1, and calcine it at 850°C for 6h in a nitrogen atmosphere (heating rate of 5°C / min).

[0058] The method for using the acid absorber in the polymer material is as follows:

[0059] (1) grinding the acid absorber to an average particle diameter of 5 μm, mixing the particle with PP material, 300 ppm of tris(3,3-di-tert-butyl-4-hydroxybenzyl) isocyanurate, and 200 ppm of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, wherein the amount of the acid absorber is 200 ppm;

[0060] (2) The mixture was mixed uniformly by a high-speed mixer and then extruded by a twin-screw extruder at an extrusion temperature of 290°C.

[0061] Example 3

[0062] A new type of acid absorbent, the structural formula of which is: Zn 1.93 Mg 0.1 Al 0.9 (OH) 6.06 (PO4 3- ) 0.23 , the acid absorber is doped with N, and its preparation method is as follows:

[0063] S1. Dissolve 1.93 mol of zinc chloride, 0.1 mol of magnesium chloride and 0.9 mol of sodium aluminate in 500 mL of water to prepare a mixed salt solution, then add 0.23 mol of sodium phosphate and 6.06 mol of sodium hydroxide to prepare 500 mL of a mixed alkali solution, mix the mixed salt solution and the mixed alkali solution by a double drop method, age at 90 ° C for 20 hours after dropping, wash and dry to obtain a powder;

[0064] S2. Grind the powder and mix it with urea in a mass ratio of 6:1, and calcine it at 700°C for 10 hours in a nitrogen atmosphere (heating rate of 5°C / min).

[0065] The method for using the acid absorber in the polymer material is as follows:

[0066] (1) grinding the acid absorber to an average particle diameter of 8 μm, mixing the particle with PP material, 560 ppm of tris(3,3-di-tert-butyl-4-hydroxybenzyl) isocyanurate, and 340 ppm of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, wherein the amount of the acid absorber is 500 ppm;

[0067] (2) The mixture is mixed uniformly by a high-speed mixer and then extruded by a twin-screw extruder at an extrusion temperature of 240°C.

[0068] Comparative Example 1

[0069] The same as Example 1, except that the structural formula of the acid scavenger is: Zn 0.18 Mg 1.82 Al 1.2 (OH)6(PO4 3- ) 0.533 , the acid absorber is doped with N, and its preparation method is as follows:

[0070] S1. Dissolve 0.18 mol of zinc chloride, 1.82 mol of magnesium chloride and 1.2 mol of sodium aluminate in 500 mL of water to prepare a mixed salt solution, then add 0.533 mol of sodium phosphate and 4.4 mol of sodium hydroxide to prepare 500 mL of a mixed alkali solution, mix the mixed salt solution and the mixed alkali solution by a double drop method, age at 80 ° C for 32 hours after dropping, wash and dry to obtain a powder;

[0071] S2. Grind the powder and mix it with urea in a mass ratio of 5:1, and calcine it at 790°C for 6-10h in a nitrogen atmosphere (heating rate of 5°C / min).

[0072] Comparative Example 2

[0073] The same as Example 1, except that the structural formula of the acid scavenger is: Zn 2.0 Al 1.2 (OH)6(PO4 3- ) 0.533 , the acid absorber is doped with N, and its preparation method is as follows:

[0074] S1. Dissolve 2.0 mol of zinc chloride and 1.2 mol of sodium aluminate in 500 mL of water to prepare a mixed salt solution, then add 0.533 mol of sodium phosphate and 4.4 mol of sodium hydroxide to prepare a 500 mL mixed alkali solution, mix the mixed salt solution and the mixed alkali solution by a double drop method, age at 80 ° C for 32 hours after dropping, wash, and dry to obtain a powder;

[0075] S2. Grind the powder and mix it with urea in a mass ratio of 5:1, and calcine it at 790°C for 6-10h in a nitrogen atmosphere (heating rate of 5°C / min).

[0076] Comparative Example 3

[0077] The method is basically the same as Example 1, except that: the acid scavenger is doped with N, and during its preparation, the mass ratio of the acid scavenger powder to urea is 2:1.

[0078] Comparative Example 4

[0079] The method is basically the same as Example 1, except that: in the method for using the acid scavenger in the polymer material, the amount of the acid scavenger is 300 ppm, the amount of tris(3,3-di-tert-butyl-4-hydroxybenzyl) isocyanurate is 600 ppm, and the amount of bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite is 100 ppm.

[0080] Comparative Example 5

[0081] The method is basically the same as Example 1, except that bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite is replaced by tris(tridecyl)phosphite.

[0082] Comparative Example 6

[0083] The acid absorber is Japan Kyowa DHT-4A.

[0084] Performance testing method:

[0085] Melt index MI: is a value that indicates the fluidity of plastic materials during processing. It is formulated by the American Institute of Measurement and Testing based on the method used by DuPont to identify plastic properties. The larger the MI, the lower the viscosity of the plastic material and the smaller the molecular weight; the smaller the MI, the higher the viscosity and molecular weight of the plastic, and the better the structural stability.

[0086] Yellowness Index YI: It is used to characterize the yellowing degree of colorless, transparent, translucent or nearly white polymer materials. It is one of the important optical indicators in the resin plastics industry. The larger the yellowness index, the yellower the sample, and the smaller the yellowness index, the whiter the sample.

[0087] Impact strength: An indicator to measure the toughness of a material, usually defined as the energy absorbed per unit cross-sectional area when a specimen breaks or fractures under an impact load. It is a numerical value that represents the toughness of the material. The larger the value, the better the toughness of the material.

[0088] During the melt extrusion process of the embodiment, samples extruded 1 time, 3 times and 5 times were taken to test their melt index MI (230°C / 2.16kg, GB / T 3682.1-2018), yellowness index YI (GB / T 39822-2021) and impact strength (GB / T1843-2008).

[0089] Performance test results:

[0090] The test results are shown in Table 1.

[0091] Table 1

[0092]

Claims

1. A new type of acid absorber, It is characterized in that Its structural formula is: M 2+ x M 3+ y (OH) m (X n- ) z ; wherein the M 2+ M is a divalent metal ion. 3+ is a trivalent metal ion, wherein X n- is an anion with a valence of -n, wherein x:y is (0.1-2.5):(0.3-4), m=2(x+1), n ​​is an integer of 1-5, and z=(3y-2) / n; The M 2+ Including Zn 2+ and Mg 2+ ; The M 2+ Medium Zn 2+ and Mg 2+ The molar ratio is (0.2-2.2): (0.3-1.5); The M 3+ For Al 3+ ; The anion is PO 4 3- .

2. The acid scavenger according to claim 1, It is characterized in that The x:y is (0.5-2):(0.3-3).

3. The acid scavenger according to claim 1, It is characterized in that The acid absorber is further doped with heteroatoms, wherein the heteroatoms are selected from at least one of N, P, B, Bi, and rare earth metal atoms.

4. The acid scavenger according to claim 3, It is characterized in that The preparation method of the acid absorbing agent comprises the following steps: S1. Preparation of M by coprecipitation 2+ x M 3+ y (OH) m (X n- ) z :Soluble M 2+ and M 3+ The salt is prepared into a mixed salt solution, and then X n- The mixed salt and alkali regulator are used to prepare a mixed alkali solution, the mixed salt solution and the mixed alkali solution are mixed, and after aging for 20-36 hours, the mixed salt solution is washed and dried to obtain a powder; S2, heteroatom-doped M 2+ x M 3+ y (OH) m (X n- ) z : Mix the powder in S1 and the dopant source and calcine at 600-850°C; the mass ratio of the powder to the nitrogen source is (4-6):

1.

5. Use of the acid scavenger according to any one of claims 1 to 4 in a polymer system, It is characterized in that The acid absorber is added when the polymer is processed into a product, and the method of use is: the acid absorber, the polymer and the auxiliary agent are mixed and melt-extruded.

6. The use according to claim 5, It is characterized in that The concentration of the acid scavenger is 200-500 ppm, and the concentration of the auxiliary agent is 500-900 ppm.

7. The use according to claim 6, It is characterized in that The auxiliary agent includes azine-based substance and phosphite-based substance, and the mass ratio of the two is (3-7): (2-4).

Citation Information

Patent Citations

  • Hydrotalcite acid acceptor for polyolefin

    CN104558775A

  • Preparation method for hydrotalcite acid absorption agent used for polyolefin

    CN104841358A

  • Anti-ultraviolet flame retardant, preparation method thereof, anti-ultraviolet flame-retardant composition and product

    CN114753160A

  • Quaternary intercalation structure acid acceptor as well as preparation method and application thereof

    CN115260588A

  • Dispersion of hydrotalcite-like compound and flame-resistant coating using same

    WO2015152279A1