Preparation method of chain extension nucleation modified poly (butylene succinate)
By reacting polybutylene succinate with peroxide and nucleating agent in an extruder, the chain extension and nucleation modification of PBS is achieved, and the complex and costly PBS chain extension in the prior art is solved. and poor performance problems, high performance, low cost modified materials are obtained.
Patent Information
- Application Number
- CN202410907418.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-19
AI Technical Summary
The existing PBS chain extension technology is complex, costly and ineffective, and cannot effectively improve the performance of polyester materials and may introduce ingredients that are harmful to the human body and the environment.
The chain-extended nucleation modification is carried out in the extruder using a reaction system including polybutylene succinate, peroxide and nucleating agent. By adjusting the proportion and type of peroxide and nucleating agent, the poly The molecular weight and crystallization temperature of butylene succinate reduce the melting index and improve the mechanical properties.
The chain extended nucleation modified PBS produced has high crystallization temperature, low melting index and excellent mechanical properties, which are simple to operate, low production costs, and do not introduce harmful components.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of PBS resins, and in particular relates to a method for preparing chain-extended nucleation-modified polybutylene succinate. Background Art
[0002] White pollution is increasingly harming the natural environment, causing irreversible damage to humans, animals and plants. Degradable materials can not only reduce the harm of white pollution, but also are an effective carrier for realizing resource recycling and utilization. Biodegradable plastics are one of them. It refers to a type of plastic that is degraded by microorganisms such as bacteria, mold (fungus) and algae in nature, and finally converted into carbon dioxide (CO2) and water (H2O) and other environmentally friendly substances.
[0003] The polyester material butylene succinate (PBS) is a biodegradable thermoplastic polymer, which has attracted much attention due to its excellent biodegradability, melt processability and chemical resistance, and can be widely used in the food and packaging industries. At present, it is difficult to obtain high molecular weight PBS by polymerization method; and in the process, due to the presence of thermal degradation and hydrolysis, the molecular weight of PBS will be reduced, the number of terminal carboxyl groups will increase, and the performance of the polymer will be reduced. One solution to the above problems is to extend the chain of polyester to significantly improve its molecular weight, viscosity and performance. People have invested considerable manpower, funds and time costs in research on this, but the PBS chain extension technology developed so far inevitably has various shortcomings, such as too complicated process, high cost, poor chain extension effect, and inability to effectively improve the performance of polyester materials. It is even possible to introduce additional components that are not conducive to human health or environmental protection into the polyester material after chain extension. The above problems have not been solved for a long time. Therefore, it is still very necessary to design a PBS chain extension modification method with simpler process and excellent product performance. Summary of the invention
[0004] To solve the above problems, the present invention provides a method for preparing chain-extended nucleated modified polybutylene succinate, which has a simple process and the prepared modified PBS product has a high crystallization temperature and a low melting index and excellent mechanical properties.
[0005] To achieve the above object, the technical scheme of the present invention is as follows: a method for preparing chain-extended nucleation-modified polybutylene succinate, comprising mixing a reaction system comprising polybutylene succinate, a peroxide and a nucleating agent uniformly, and then putting the mixture into an extruder for chain-extended nucleation modification to obtain chain-extended nucleation-modified PBS; wherein the weight parts of each component are: 100 parts of polybutylene succinate, 0.01 to 0.2 parts of peroxide, and 0.01 to 0.5 parts of nucleating agent.
[0006] The present invention is further configured such that the weight portion of the peroxide is 0.05 to 0.15 parts; the weight portion of the nucleating agent is 0.05 to 0.2 parts.
[0007] The present invention is further configured such that the peroxide is selected from one or more of diisopropylbenzene peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, (2,5-dimethyl-2,5-di-tert-butyl)peroxyhexane, (2,5-methyl-2,5-di-tert-butyl)peroxyhexyne, benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl formyl peroxide, and di-tert-butyl cumene peroxide.
[0008] The present invention is further configured such that the nucleating agent is a metal carboxylate nucleating agent.
[0009] The present invention is further configured that the nucleating agent is selected from one or more of potassium phthalate, potassium hexahydrophthalate, potassium adipate, potassium succinate, potassium nadic acid, sodium phthalate, sodium hexahydrophthalate, sodium adipate, sodium succinate, sodium nadic acid, zinc phthalate, zinc hexahydrophthalate, zinc nadic acid, calcium phthalate, calcium hexahydrophthalate, calcium nadic acid, aluminum phthalate, aluminum hexahydrophthalate, and aluminum nadic acid.
[0010] The present invention is further configured that the polybutylene succinate used is dried polybutylene succinate; further, the drying conditions of the raw material polybutylene succinate are 40-65° C. and dried for 1-24 hours.
[0011] The present invention is further configured as follows: the extruder is a twin-screw extruder, the temperature of the melting section and the natural exhaust section of the twin-screw extruder is 100-240°C, the main screw speed of the extruder is 100-300r / min, and the feeding screw speed is 10-30r / min.
[0012] The present invention is further configured such that the molecular weight of the obtained chain-extended nucleated polybutylene succinate is increased by 30 to 75% compared with the raw material polybutylene succinate.
[0013] The present invention also provides a chain-extended nucleation-modified polybutylene succinate prepared by the above-mentioned preparation method.
[0014] The present invention is further configured that the number average molecular weight of the chain extension nucleation modified polybutylene succinate is 1.3×10 5 ~2.0×10 5 g / mol, the melt index is 1.0-9.0g / 10min, and the crystallization temperature is 85-100℃.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) The chain extension nucleation modified polybutylene succinate product produced by the present invention has both high crystallization temperature and low melt index. Its melt index is reduced to 1.0-9.0 g / 10 min, and the crystallization temperature of the material is increased to 85-100° C.
[0017] (2) The chain extension nucleation modified polybutylene succinate product prepared by the present invention also has more excellent product properties, such as bending strength, tensile strength and notched impact strength;
[0018] (3) The preparation method and formula composition of the present invention are simpler, the production cost is low, the processing is convenient, and the raw materials are easy to store, which has great implementation value and economic benefits. DETAILED DESCRIPTION
[0019] The present invention is described in detail and completely with specific embodiments below. It should be understood that the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.
[0020] The present invention provides a method for preparing a chain-extended nucleated polybutylene succinate, which comprises mixing a reaction system including a raw material polybutylene succinate, a peroxide and a nucleating agent uniformly, and then putting the mixture into an extruder for chain-extended nucleating modification to obtain a chain-extended nucleated PBS; wherein the weight parts of each component are: 100 parts of the raw material polybutylene succinate, 0.01 to 0.2 parts of the peroxide, and 0.01 to 0.5 parts of the nucleating agent. Preferably, the weight part of the peroxide is 0.05 to 0.15 parts; the weight part of the nucleating agent is 0.05 to 0.2 parts.
[0021] In one example of the present application, the peroxide is selected from one or more of diisopropylbenzene peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, (2,5-dimethyl-2,5-di-tert-butyl)peroxyhexane, (2,5-methyl-2,5-di-tert-butyl)peroxyhexyne, benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl formyl peroxide, and di-tert-butyl cumene peroxide.
[0022] In one example of the present application, the nucleating agent is selected from one or more of potassium phthalate, potassium hexahydrophthalate, potassium adipate, potassium succinate, potassium naphthalate, sodium phthalate, sodium hexahydrophthalate, sodium adipate, sodium succinate, sodium naphthalate, zinc phthalate, zinc hexahydrophthalate, zinc naphthalate, calcium phthalate, calcium hexahydrophthalate, calcium naphthalate, aluminum phthalate, aluminum hexahydrophthalate, and aluminum naphthalate.
[0023] In the present application, the extruder is a twin-screw extruder, the temperature of the melting section and the natural exhaust section of the twin-screw extruder is 100-240°C, the main screw speed of the extruder is 100-300r / min, and the feeding screw speed is 10-30r / min.
[0024] Furthermore, the twin-screw extruder is divided into eight sections, the temperature range of the first feeding zone is 100-120°C, the temperature range of the second zone is 110-160°C, the temperature range of the third zone is 110-220°C, the temperature range of the fourth zone is 120-220°C, the temperature range of the fifth zone is 120-220°C, the temperature range of the sixth zone is 120-220°C, the temperature range of the seventh zone is 120-220°C, the temperature range of the eighth zone is 110-170°C, and the head temperature is 110-160°C.
[0025] The molecular weight of the chain-extended nucleated polybutylene succinate prepared by the above method is increased by 30-75% compared with the raw material polybutylene succinate.
[0026] The present invention also provides a chain-extended nucleated modified polybutylene succinate prepared by the above-mentioned preparation method, wherein the number average molecular weight of the chain-extended nucleated modified polybutylene succinate is 1.3×10 5 ~2.0×10 5 g / mol, the melt index is 1.0-9.0g / 10min, and the crystallization temperature is 85-100℃.
[0027] The twin-screw extruder used in the embodiments of the present invention is a HT-30 twin-screw extruder purchased from Nanjing Rubber Machinery Factory Co., Ltd.
[0028] The present invention is further described below with reference to examples, but the present invention is not limited to these examples.
[0029] Example 1
[0030] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0031] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 h are uniformly mixed with 0.12 parts of benzoyl peroxide (BPO) and 0.2 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 120° C., 130° C., 145° C., 160° C., 160° C., 160° C., 150° C., respectively, the die head temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0032] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0033] Example 2
[0034] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0035] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours were uniformly mixed with 0.1 parts of BPO and 0.2 parts of HHPA-Zn, and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 120° C., 130° C., 145° C., 160° C., 160° C., 160° C., 150° C., respectively, the die head temperature was 140° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0036] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0037] Example 3
[0038] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0039] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours were uniformly mixed with 0.14 parts of BPO and 0.2 parts of HHPA-Zn, and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 120° C., 130° C., 145° C., 160° C., 160° C., 160° C., 150° C., respectively, the die head temperature was 140° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0040] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0041] Example 4
[0042] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0043] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours were uniformly mixed with 0.12 parts of BPO and 0.2 parts of HHPA-Zn, and then added into an extruder blending device for melt granulation to prepare a chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 115° C., 120° C., 125° C., 130° C., 130° C., 125° C., the die head temperature was 125° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0044] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0045] Example 5
[0046] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0047] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours were uniformly mixed with 0.12 parts of BPO and 0.2 parts of HHPA-Zn, and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 120° C., 130° C., 135° C., 140° C., 140° C., 135° C., the die head temperature was 130° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0048] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0049] Example 6
[0050] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0051] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours were uniformly mixed with 0.12 parts of BPO and 0.2 parts of HHPA-Zn, and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 120° C., 130° C., 140° C., 150° C., 150° C., 140° C., respectively, the die temperature was 130° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0052] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0053] Example 7
[0054] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0055] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours were uniformly mixed with 0.12 parts of BPO and 0.2 parts of HHPA-Zn, and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 125° C., 140° C., 155° C., 170° C., 170° C., 155° C., the die head temperature was 140° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0056] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0057] Example 8
[0058] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0059] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 h and 0.12 parts of benzoyl peroxide (BPO) were mixed uniformly, and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 120° C., 130° C., 145° C., 160° C., 160° C., 160° C., 150° C., respectively, the die head temperature was 140° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0060] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0061] Example 9
[0062] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0063] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 h and 0.2 parts of hexahydrophthalic acid zinc (HHPA-Zn) were mixed uniformly, and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 120° C., 130° C., 145° C., 160° C., 160° C., 160° C., 150° C., respectively, the die head temperature was 140° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0064] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0065] Example 10
[0066] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0067] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 h are uniformly mixed with 0.12 parts of benzoyl peroxide (BPO) and 0.05 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 120° C., 130° C., 145° C., 160° C., 160° C., 160° C., 150° C., respectively, the die head temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0068] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0069] Embodiment 11
[0070] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0071] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 h are uniformly mixed with 0.12 parts of benzoyl peroxide (BPO) and 0.1 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 120° C., 130° C., 145° C., 160° C., 160° C., 160° C., 150° C., respectively, the die head temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0072] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0073] Example 12
[0074] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0075] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 h are uniformly mixed with 0.12 parts of benzoyl peroxide (BPO) and 0.15 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 120° C., 130° C., 145° C., 160° C., 160° C., 160° C., 150° C., respectively, the die head temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0076] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0077] Comparative Example 1
[0078] 100 parts of the same polybutylene succinate raw material as in Examples 1 to 12 were dried at 60° C. for 12 hours, and subsequent performance tests were performed.
[0079] The modified polybutylene succinate prepared in the above Examples 1 to 12 and the polybutylene succinate in Comparative Example 1 were subjected to performance tests. The test results are shown in Table 1:
[0080] Table 1 Test results of chain extension nucleation modified polybutylene succinate properties
[0081]
[0082]
[0083] Embodiment 13
[0084] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0085] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours are uniformly mixed with 0.09 parts of di-tert-butyl diisopropylbenzene peroxide (BIPB) and 0.2 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 140° C., 200° C., 200° C., 200° C., 200° C., 155° C., respectively, the die temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0086] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0087] Embodiment 14
[0088] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0089] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours are uniformly mixed with 0.1 parts of di-tert-butyl diisopropylbenzene peroxide (BIPB) and 0.2 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 140° C., 200° C., 200° C., 200° C., 200° C., 155° C., respectively, the die temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0090] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0091] Embodiment 15
[0092] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0093] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours are uniformly mixed with 0.11 parts of di-tert-butyl diisopropylbenzene peroxide (BIPB) and 0.2 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 140° C., 200° C., 200° C., 200° C., 200° C., 155° C., respectively, the die temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0094] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0095] Example 16
[0096] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0097] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours are uniformly mixed with 0.09 parts of di-tert-butyl diisopropylbenzene peroxide (BIPB) and 0.2 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 140° C., 170° C., 190° C., 190° C., 170° C., and 155° C., respectively, the die head temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0098] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0099] Embodiment 17
[0100] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0101] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours are uniformly mixed with 0.09 parts of di-tert-butyl diisopropylbenzene peroxide (BIPB) and 0.2 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 140° C., 170° C., 180° C., 180° C., 180° C., 170° C., and 155° C., respectively, the die head temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0102] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0103] Embodiment 18
[0104] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0105] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours are uniformly mixed with 0.09 parts of di-tert-butyl diisopropylbenzene peroxide (BIPB) and 0.2 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to prepare chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 140° C., 170° C., 170° C., 170° C., 170° C., 170° C., 155° C., respectively, the die head temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0106] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0107] Embodiment 19
[0108] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0109] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours and 0.10 parts of di-tert-butyl diisopropylbenzene peroxide (BIPB) were mixed uniformly, and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 140° C., 200° C., 200° C., 200° C., 200° C., 155° C., respectively, the die head temperature was 140° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0110] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0111] Embodiment 20
[0112] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0113] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours and 0.20 parts of hexahydrophthalic acid zinc (HHPA-Zn) were mixed uniformly, and then added into an extruder blending device for melt granulation to prepare chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder were 110° C., 140° C., 200° C., 200° C., 200° C., 200° C., 155° C., respectively, the die temperature was 140° C., the main engine speed was 100 r / min, and the feed speed was 10 r / min.
[0114] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0115] Embodiment 21
[0116] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0117] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours are uniformly mixed with 0.10 parts of di-tert-butyl diisopropylbenzene peroxide (BIPB) and 0.15 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 140° C., 200° C., 200° C., 200° C., 200° C., 155° C., respectively, the head temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0118] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0119] Embodiment 22
[0120] This embodiment provides a method for preparing chain-extended nucleation-modified polybutylene succinate, which specifically comprises the following steps:
[0121] (1) 100 parts of polybutylene succinate dried at 60° C. for 12 hours are uniformly mixed with 0.10 parts of di-tert-butyl diisopropylbenzene peroxide (BIPB) and 0.05 parts of hexahydrophthalate zinc (HHPA-Zn), and then added into an extruder blending device for melt granulation to obtain chain-extended nucleated PBS; wherein the temperature ranges of the twin-screw extruder are 110° C., 140° C., 200° C., 200° C., 200° C., 200° C., 155° C., respectively, the die temperature is 140° C., the main engine speed is 100 r / min, and the feed speed is 10 r / min.
[0122] (2) The obtained modified polybutylene succinate was dried at 80° C. for 4 hours and then sealed and stored.
[0123] Comparative Example 2
[0124] 100 parts of polybutylene succinate, which is the same as the raw material in Examples 13 to 22, was dried at 60° C. for 12 hours and then a subsequent performance test was performed.
[0125] Table 2 Test results of chain extension nucleation modified polybutylene succinate properties
[0126]
[0127]
[0128] Combining the chain extension nucleation modified polybutylene succinate performance test results in Table 1 and Table 2, it can be seen that the modified PBS product prepared by the chain extension nucleation process provided by the present invention has both a low melt index and a high crystallization temperature, and the mechanical properties are improved; and the chain extension nucleation process is simple to operate and has great application value.
[0129] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing chain-extending nucleated modified polybutylene succinate, characterized in that: The reaction system including polybutylene succinate, peroxide and nucleating agent is mixed uniformly, and then put into an extruder for chain extension and nucleating modification to obtain chain extension and nucleating modified PBS; wherein the weight parts of each component are: 100 parts of polybutylene succinate, 0.01-0.2 parts of peroxide, and 0.01-0.5 parts of nucleating agent.
2. The method for preparing the chain-extending nucleating modified polybutylene succinate according to claim 1, characterized in that: The peroxide is selected from one or more of diisopropylbenzene peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, (2,5-dimethyl-2,5-di-tert-butyl)peroxyhexane, (2,5-methyl-2,5-di-tert-butyl)peroxyhexyne, benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl formyl peroxide, and di-tert-butyl cumene peroxide.
3. The method for preparing the chain-extending nucleating modified polybutylene succinate according to claim 1, characterized in that: The nucleating agent is a metal carboxylate nucleating agent.
4. The method for preparing the chain-extending nucleating modified polybutylene succinate according to claim 1, characterized in that: The nucleating agent is selected from one or more of potassium phthalate, potassium hexahydrophthalate, potassium adipate, potassium succinate, potassium nadate, sodium phthalate, sodium hexahydrophthalate, sodium adipate, sodium succinate, sodium nadate, zinc phthalate, zinc hexahydrophthalate, zinc nadate, calcium phthalate, calcium hexahydrophthalate, calcium nadate, aluminum phthalate, aluminum hexahydrophthalate, and aluminum nadate.
5. The method for preparing the chain-extending nucleation-modified polybutylene succinate according to claim 1, characterized in that: The weight proportions of the components are: 100 parts of polybutylene succinate, 0.05 to 0.15 parts of peroxide, and 0.05 to 0.2 parts of nucleating agent.
6. The method for preparing the chain-extending nucleation-modified polybutylene succinate according to claim 1, characterized in that: The extruder is a twin-screw extruder, the temperatures of the melting section and the natural exhaust section of the twin-screw extruder are 100-240° C., the main screw speed of the extruder is 100-300 r / min, and the feeding screw speed is 10-30 r / min.
7. The method for preparing the chain-extending nucleation-modified polybutylene succinate according to claim 1, characterized in that: The molecular weight of the obtained chain-extended nucleated polybutylene succinate is increased by 30-75% compared with the raw material polybutylene succinate.
8. A chain-extended nucleated modified polybutylene succinate prepared according to the preparation method according to any one of claims 1 to 7.
9. The chain-extended nucleation-modified polybutylene succinate according to claim 8, characterized in that: The obtained chain-extended nucleation-modified polybutylene succinate has a melting index of 1.0 to 9.0 g / 10 min and a crystallization temperature of 85 to 100° C.
Citation Information
Patent Citations
Preparation method of biodegradable poly butylene succinate (PBS) foam materials
CN101899200A
Biodegradable polybutylene succinate (PBS) foaming material and preparation method thereof
CN102627837A
Fully-biodegradable mulch film, and preparation method and application thereof
CN110283433A
Heat-resistant poly (butylene succinate) composition, nucleating agent and preparation method of heat-resistant poly (butylene succinate) composition