Mecoluminescent phosphors with adjustable emission color and intensity, preparation methods and applications

By adjusting the crystal phase composition and microstructure of manganese-doped gallium oxide materials, a mechanoluminescent phosphor with tunable luminescence color and intensity was prepared, solving the problem of difficult control of mechanoluminescence color and intensity in the prior art. It realizes effective force-induced luminescence under different mechanical deformations and can be applied in multiple fields.

CN118895122BActive Publication Date: 2026-11-17FUYANG NORMAL UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410806203.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2026-11-17
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing technologies make it difficult to effectively control the color and intensity of mechanoluminescence in the same type of matrix material, especially in the ultraviolet to near-infrared band.

Method used

By employing strategies such as element substitution, optimizing process conditions, and altering the sintering atmosphere, the crystal phase composition and microstructure of manganese-doped gallium oxide materials were adjusted, resulting in the preparation of metronic phosphors with tunable luminescence color and intensity, bearing the chemical formula a(Na2-yLiy)O-bGa2O3:xmol%Mn2+. These phosphors were then combined with organic polymers to prepare metronic materials of different shapes and hardness.

Benefits of technology

It achieves effective control of the emission spectrum and mechanoluminescence color and intensity of manganese-doped gallium oxide materials, and is suitable for force-induced luminescence under different mechanical deformations. It can be applied to the detection of micro-defects, structural health diagnosis, stress distribution visualization, novel light sources and flexible stress sensor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895122B_ABST
    Figure CN118895122B_ABST
Patent Text Reader

Abstract

This invention discloses a type of mechanoluminescent phosphor with tunable emission color and intensity, its preparation method, and its applications. The preparation method and steps of the phosphor are as follows: S1: Sodium source, lithium source, gallium source, and manganese source are ground and mixed in anhydrous ethanol according to stoichiometric ratio; S2: The mixed material is pre-calcined; S3: The pre-calcined material is sintered at high temperature under air or a special protective gas. After cooling, grinding, and sieving, the sintered material yields the mechanoluminescent phosphor with tunable emission color and intensity. This invention also includes mixing the high-temperature sintered phosphor with organic polymers such as PDMS, PVDF, and PSPI to prepare organic composite structures with obvious mechanoluminescence phenomena, such as cylinders, rods, and thin films. This invention uses strategies such as element substitution, changing process conditions, and sintering atmosphere to adjust the crystal phase composition and microstructure of the material, thereby achieving effective control of the photoluminescence and mechanoluminescence color and intensity of manganese-doped gallium oxides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of luminescent materials technology, and in particular to mechanoluminescent phosphors with adjustable luminescence color and intensity, their preparation methods, and applications. Background Technology

[0002] Due to their broad application prospects in areas such as micro-defect detection, structural health diagnosis, stress distribution visualization, novel light sources and display technologies, and flexible stress sensors, inorganic mechanoluminescent materials have attracted widespread attention from scholars both domestically and internationally in recent years. Research in this field focuses on two main aspects: first, the development of new material systems and the exploration of the physical origins of mechanoluminescence in these systems; second, the synthesis of mechanoluminescent composite materials or structures with varying mechanical properties by combining high-temperature solid-state sintered ceramic powders with organic polymers (epoxy resins, polydimethylsiloxane (PDMS), polyvinylidene fluoride (PVDF), PVDF-TrFE copolymer, photosensitive polyimide (PSPI), etc.), thus accumulating experimental data for the development of mechanoluminescent devices for different applications. Currently, through the optimization and improvement of rare-earth or transition metal activators and different matrices, researchers can achieve mechanoluminescence emission from the ultraviolet to near-infrared bands. However, due to the complexity of the energy levels of rare earth and transition metal ions and the huge differences in the energy bands, defect states, and phonon energies of various matrix materials, the luminescence intensity of different material systems varies greatly. It is difficult to effectively control the luminescence color by mixing different phosphors. In particular, there are very few cases of controlling the mechanoluminescence color and intensity in the same type of matrix material. Summary of the Invention

[0003] Based on the technical problems existing in the background technology, this invention proposes a mechanoluminescent phosphor with adjustable emission color and intensity, its preparation method and application. By using strategies such as element substitution, optimization and improvement of process conditions, and changes in sintering atmosphere, the crystal phase composition and microstructure of the material are adjusted, and the emission spectrum and mechanoluminescent color and intensity of manganese-doped gallium oxide materials are effectively controlled.

[0004] The mechanoluminescent phosphor proposed in this invention has adjustable emission color and intensity. The general chemical formula of the phosphor is: a(Na) 2-y Li y O-bGa2O3: x mol% Mn 2+ Where 0.2≤a / b≤5, 0< x ≤20, 0≤ y <2.

[0005] The present invention proposes a method for preparing mechanoluminescent phosphors with adjustable emission color and intensity, the method steps of which are as follows: S1: Sodium source, lithium source, gallium source and manganese source are ground and mixed in anhydrous ethanol according to stoichiometric ratio; S2: Pre-fire the mixed material; S3: The pre-fired material is sintered at high temperature under the action of air or protective gas. After cooling, grinding and sieving, the sintered material yields metronome phosphor with adjustable luminescent color and intensity.

[0006] Preferably, the sodium source is one or more of Na2CO3, NaCl, NaNO3, Na2SO4, Na2C2O4, and sodium acetate; the lithium source is one or more of Li2CO3, LiCl, LiNO3, Li2SO4, Li2C2O4, and lithium acetate; the gallium source is one or more of Ga2O3, Ga(OH)3, and GaCl3; and the manganese source is one or more of MnCO3, MnO, MnO2, MnCl2, MnSO4, (CH3COO)2Mn, and MnC2O4.

[0007] Preferably, the pre-firing temperature in S2 is 400-1000 ℃, and the time is 0.5-20 h.

[0008] Preferably, the high-temperature sintering conditions in S3 are as follows: heating to 500-1400 ℃ at a rate of 1-15 ℃ / min and holding at that temperature for 2-16 h, and finally cooling to 500 ℃ at a rate of 1-15 ℃ / min.

[0009] Preferably, the special protective gas in S3 includes an inert gas and / or a reducing gas; the inert gas is nitrogen or argon, and the reducing gas is hydrogen.

[0010] The application of the metronic phosphor with adjustable luminescence color and intensity proposed in this invention is carried out by the following steps: the metronic phosphor with adjustable luminescence color and intensity is composited with PDMS, PVDF, PVDF-TrFE or PSPI, and a metronic phosphor / polymer composite film is prepared by spin casting, casting or hot pressing.

[0011] The application of the metronic phosphor with adjustable luminescence color and intensity proposed in this invention is carried out by the following steps: the metronic phosphor with adjustable luminescence color and intensity is compounded with epoxy resin, polydimethylsiloxane, polyvinylidene fluoride, copolymer of polyvinylidene fluoride and trifluoroethylene or photosensitive polyimide and curing agent, and metronic phosphor / polymer cylinder and fine rod-shaped metronic phosphor materials are prepared by cold solidification method.

[0012] Beneficial technical effects of the present invention: This invention employs strategies such as element substitution, optimized process conditions, and altered sintering atmosphere to adjust the crystal phase composition and microstructure of materials, achieving effective control over the emission spectrum and mechanoluminescence color and intensity of manganese-doped gallium oxide materials. Furthermore, this invention combines mechanoluminescent phosphors prepared by a high-temperature solid-state reaction method with organic polymer matrices such as epoxy resin, polydimethylsiloxane, polyvinylidene fluoride, copolymers of polyvinylidene fluoride and trifluoroethylene, or photosensitive polyimide. A series of mechanoluminescent cylindrical, rod-shaped, or composite thin film materials or structures composed of phosphors and organic polymers are prepared using methods such as melt hot pressing, dissolution spinning, or casting. These materials or structures possess different mechanical properties, allowing them to be excited by force under various mechanical deformations (such as compression, friction, tension, bending, and torsion), thereby achieving effective force-induced luminescence. Attached Figure Description

[0013] Figure 1 (a) Photoluminescence excitation spectrum and (b) Photoluminescence emission spectrum of samples with different doping contents proposed in this invention; Figure 2 The photoluminescence emission spectra of sintered samples under different atmospheres proposed in this invention are shown in (a) NaGa 4.995 O8:0.005Mn 2+ (b) NaGa 4.99 O8:0.01Mn 2+ (c) NaGa 4.985 O8:0.015Mn 2+ ; Figure 3 This invention presents LiGa sintering samples under different atmospheres. 4.99 O8:0.01Mn 2+ The photoluminescence emission spectrum; Figure 4 The present invention provides a sample of NaGa sintered under an H2 / Ar atmosphere. 2.985 O5:0.015Mn 2+ The photoluminescence emission spectrum; Figure 5 The LiGa sample sintered under H2 / N2 atmosphere proposed in this invention 2.99 O5:0.01Mn 2+ The photoluminescence emission spectrum; Figure 6 This invention presents a LiGa sample sintered under an H2 / Ar atmosphere. 2.99 O5:0.01Mn 2+ The photoluminescence emission spectrum; Figure 7 The sintered samples (Na) proposed in this invention under different atmospheres 0.5 Li0.5 )Ga 2.99 O5:0.01Mn 2+ The photoluminescence emission spectra of (a) H2 / Ar, (b) H2 / N2, and (c) N2; Figure 8 The present invention provides a sample of Na2Ga sintered under an H2 / Ar atmosphere. 3.985 O7:0.015Mn 2+ The photoluminescence emission spectrum; Figure 9 This invention relates to the sintering of (Na,Li)Ga samples under H2 / Ar atmosphere. 3.99 O7:0.01Mn 2+ The photoluminescence emission spectrum; Figure 10 This invention presents sintered NaGa samples with different manganese doping concentrations. 1-x O2: x Mn 2+ ( x= Photoluminescence emission spectra of 0.005, 0.01, and 0.015; Figure 11 The sintered samples (Na) proposed in this invention under different atmospheres 0.5 Li 0.5 )Ga 0.99 O2:0.01Mn 2+ The photoluminescence emission spectrum; Figure 12 The sintering of the sample (Na) under H2 / Ar atmosphere proposed in this invention 0.5 Li 0.5 )Ga 0.985 O2: 0.015Mn 2+ The photoluminescence emission spectrum; Figure 13 This invention presents a LiGa sample sintered under an H2 / Ar atmosphere. 0.985 O2: 0.015Mn 2+ The photoluminescence emission spectrum; Figure 14 The present invention provides sintered samples of Na4Ga under different atmospheres. 1.99 O5:0.01Mn 2+ The photoluminescence emission spectra of (a) H2 / Ar and (b) H2 / N2; Figure 15 The Li4Ga samples sintered under different atmospheres proposed in this invention 1.99 O5:0.01Mn 2+ The photoluminescence emission spectra of (a) H2 / Ar and (b) H2 / N2; Figure 16 The present invention provides sintered samples of Na2Li2Ga under different atmospheres. 1.99 O5:0.01Mn 2+ The photoluminescence emission spectra of (a) H2 / Ar and (b) H2 / N2; Figure 17 The present invention relates to the sintering of Na5Ga samples in air atmosphere. 0.99 O4:0.01Mn 2+ The photoluminescence emission spectrum; Figure 18 The Li5Ga samples sintered under different atmospheres proposed in this invention 0.99 O4:0.01Mn 2+ The photoluminescence emission spectra of (a) H2 / Ar and (b) H2 / N2; Figure 19 The Na2Li3Ga sintered sample under H2 / Ar atmosphere proposed in this invention 0.99 O4:0.01Mn 2+ The photoluminescence emission spectrum; Figure 20 The present invention proposes sintering NaGa samples under an H2 / Ar atmosphere. 4.985 O8:0.015Mn 2+ Photoluminescence emission spectrum (PL spectra) and stress emission spectrum (ML spectra) of thin film samples prepared with PVDF. Figure 21 The present invention proposes sintering samples (Na) under N2 atmosphere. 0.5 Li 0.5 )Ga 2.99 O5: 0.01Mn 2+ Photoluminescence emission spectrum (PL spectra) and stress emission spectrum (ML spectra) of the sample prepared with PVDF-TrFE. Figure 22 The (Na) proposed in this invention 0.5 Li 0.5 )Ga 2.99 O5:0.01Mn 2+ Curve showing the change in the intensity of the sample luminescence over time under linearly varying pressure; Figure 23 This is a mechanoluminescence visible-near-infrared CCD camera image (sensing range 400-1700nm) of a typical cylindrical sample proposed in this invention under external pressure. Detailed Implementation

[0014] The present invention will be further explained below with reference to specific embodiments.

[0015] Example 1 Based on the chemical formula NaGa 5-x / 100 O8: x mol%Mn 2+ (in x The raw materials Na₂CO₃, Ga₂O₃, and MnCO₃ (with molar ratios of 0.25, 0.5, 0.75, 1.0, 1.5, and 2.0) were first weighed in the corresponding molar ratios and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. The mixed raw materials were then transferred to an alumina crucible and pre-calcined at 950 °C for 100 min in a muffle furnace. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 120 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 1100 °C for 8 h using an Ar / H₂ mixed gas (5% hydrogen by volume) as the reducing atmosphere. Finally, the sintered agglomerate was ground in a mortar and passed through a 500-mesh sieve to produce manganese-doped mechanoluminescent phosphor.

[0016] Example 2 Based on the chemical formula NaGa 5-x / 100 O8: x mol%Mn 2+ (in x (The molar ratios are 0.75, 1.0, and 1.5). First, weigh the raw materials Na2CO3, Ga2O3, and MnCO3 in the corresponding molar ratios, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Then, transfer the mixed raw materials to an alumina crucible and pre-calcine them in a muffle furnace at 900 °C for 100 min. After cooling, grind the pre-calcineed material again in an agate mortar with anhydrous ethanol for 120 min. Subsequently, load the ground powder into an alumina crucible and sinter it in a tube furnace at 1150 °C for 8 h using a N2 / H2 mixed gas (hydrogen volume ratio 5%) as the reducing atmosphere. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare manganese-doped mechanoluminescent phosphor.

[0017] Example 3 Based on the chemical formula LiGa 5-x / 100 O8: x mol%Mn 2+ (in x=0.75, 1.0, and 1.5), firstly, weigh the raw materials Li2CO3, Ga2O3, and MnCO3 in the corresponding molar ratios, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Then, transfer the mixed raw materials to an alumina crucible and pre-calcine them in a muffle furnace at 800 °C for 100 min. After the pre-calcination and cooling, grind the pre-calcined material again in an agate mortar with anhydrous ethanol for 120 min. Subsequently, load the ground powder into an alumina crucible and sinter it in a tube furnace at 1250 °C for 8 h using an Ar / H2 mixed gas (hydrogen volume ratio 5%) as the reducing atmosphere. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare manganese-doped mechanoluminescent phosphor.

[0018] Example 4 Based on the chemical formula LiGa 5-x / 100 O8: x mol%Mn 2+ (in x =0.75, 1.0, and 1.5), firstly, weigh the raw materials Li2CO3, Ga2O3, and MnCO3 in the corresponding molar ratios, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Then, transfer the mixed raw materials to an alumina crucible and pre-calcine them in a muffle furnace at 800 °C for 100 min. After the pre-calcination and cooling, grind the pre-calcined material again in an agate mortar with anhydrous ethanol for 120 min. Subsequently, load the ground powder into an alumina crucible and sinter it in a tube furnace at 1250 °C for 8 h using a N2 / H2 mixed gas (hydrogen volume ratio of 5%) as the reducing atmosphere. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare manganese-doped mechanoluminescent phosphor.

[0019] Example 5 Based on the chemical formula LiGa 5-x / 100 O8: x mol%Mn 2+ (in x =0.75, 1.0, and 1.5), firstly, weigh the raw materials Li2CO3, Ga2O3, and MnCO3 in the corresponding molar ratios, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Next, transfer the mixed raw materials to an alumina crucible and pre-calcine at 800 ℃ for 100 min in a muffle furnace. After cooling, grind the pre-calcineed material again in an agate mortar with anhydrous ethanol for 120 min. Subsequently, load the ground powder into an alumina crucible and sinter it in a tube furnace at 1250 ℃ for 8 h using N2 as a protective atmosphere. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare manganese-doped mechanoluminescent phosphor.

[0020] Example 6 Based on the chemical formula NaGa 2.99 O5:0.01Mn 2+ First, weigh the raw materials Na2CO3, Ga2O3, and MnCO3 in the appropriate molar ratio, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Then, transfer the mixed raw materials to an alumina crucible and pre-calcine at 850 °C for 100 min in a muffle furnace. After cooling, grind the pre-calcineed material again in an agate mortar with anhydrous ethanol for 120 min. Subsequently, load the ground powder into an alumina crucible, use an Ar / H2 mixed gas (5% hydrogen by volume) as the reducing atmosphere, and sinter at 1200 °C for 6 h in a tube furnace. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare manganese-doped mechanoluminescent phosphor.

[0021] Example 7 Based on the chemical formula LiGa 2.99 O5:0.01Mn 2+ First, the raw materials Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio were weighed and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. Next, the mixed raw materials were transferred to an alumina crucible and pre-calcined in a muffle furnace at 850 °C for 100 min. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 120 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 1200 °C for 6 h using an Ar / H₂ mixed gas (5% hydrogen by volume) as the reducing atmosphere. Finally, the sintered agglomerate was ground in a mortar and passed through a 500-mesh sieve to produce manganese-doped mechanoluminescent phosphor.

[0022] Example 8 Based on the chemical formula LiGa 2.99 O5:0.01Mn 2+ First, the raw materials Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio were weighed and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. Next, the mixed raw materials were transferred to an alumina crucible and pre-calcined in a muffle furnace at 850 °C for 100 min. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 120 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 1200 °C for 6 h using a N₂ / H₂ mixture (5% hydrogen by volume) as the reducing atmosphere. Finally, the sintered agglomerate was ground in a mortar and passed through a 500-mesh sieve to produce manganese-doped mechanoluminescent phosphor.

[0023] Example 9 According to the chemical formula (Na) 0.5Li 0.5 )Ga 2.99 O5:0.01Mn 2+ First, weigh the raw materials Na₂CO₃, Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Next, transfer the mixed raw materials to a corundum crucible and pre-calcine at 700 °C for 100 min in a muffle furnace. After cooling, grind the pre-calcine material again in an agate mortar with anhydrous ethanol for 100 min. Then, load the ground powder into a corundum crucible, use an Ar / H₂ mixture (5% hydrogen by volume) as the reducing atmosphere, and sinter at 1150 °C for 6 h in a tube furnace. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare (Na₂CO₃) powder. 0.5 Li 0.5 )Ga 2.99 O5:0.01Mn 2+ Mechanoluminescent phosphor.

[0024] Example 10 According to the chemical formula (Na) 0.5 Li 0.5 )Ga 2.99 O5:0.01Mn 2+ First, weigh the raw materials Na₂CO₃, Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Next, transfer the mixed raw materials to a corundum crucible and pre-calcine at 700 °C for 100 min in a muffle furnace. After cooling, grind the pre-calcine material again in an agate mortar with anhydrous ethanol for 100 min. Then, load the ground powder into a corundum crucible, use a N₂ / H₂ mixture (5% hydrogen by volume) as the reducing atmosphere, and sinter at 1150 °C for 6 h in a tube furnace. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare (Na₂CO₃) powder. 0.5 Li 0.5 )Ga 2.99 O5:0.01Mn 2+ Mechanoluminescent phosphor.

[0025] Example 11 According to the chemical formula (Na) 0.5 Li 0.5 )Ga 2.99 O5:0.01Mn 2+First, weigh the raw materials Na₂CO₃, Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Next, transfer the mixed raw materials to a corundum crucible and pre-calcine at 700 °C for 100 min in a muffle furnace. After cooling, grind the pre-calcine material again in an agate mortar with anhydrous ethanol for 100 min. Then, place the ground powder into a corundum crucible, sinter it in a tube furnace at 1150 °C for 6 h under a N₂ protective atmosphere, and finally grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare (Na₂CO₃) powder. 0.5 Li 0.5 )Ga 2.99 O5:0.01Mn 2+ Mechanoluminescent phosphor.

[0026] Example 12 According to the chemical formula Na₂Ga 3.985 O7:0.015Mn 2+ First, the raw materials Na2CO3, Ga2O3, and MnCO3 in the appropriate molar ratio were weighed and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. Next, the mixed raw materials were transferred to an alumina crucible and pre-calcined in a muffle furnace at 600 °C for 100 min. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 80 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 1100 °C for 6 h using an Ar / H2 mixed gas (5% hydrogen by volume) as the reducing atmosphere. Finally, the sintered agglomerate was ground in a mortar and passed through a 500-mesh sieve to produce manganese-doped mechanoluminescent phosphor.

[0027] Example 13 Based on the chemical formula NaGa 0.995 O2: 0.005Mn 2+ First, the raw materials Na2CO3, Ga2O3, and MnCO3 in the appropriate molar ratio were weighed and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. Next, the mixed raw materials were transferred to an alumina crucible and pre-calcined in a muffle furnace at 800 °C for 100 min. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 100 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 1250 °C for 4 h using an Ar / H2 mixed gas (5% hydrogen by volume) as the reducing atmosphere. Finally, the sintered agglomerate was ground in a mortar and passed through a 500-mesh sieve to produce manganese-doped mechanoluminescent phosphor.

[0028] Example 14 Based on the chemical formula NaGa0.99 O2:0.01Mn 2+ First, the raw materials Na2CO3, Ga2O3, and MnCO3 in the appropriate molar ratio were weighed and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. Next, the mixed raw materials were transferred to an alumina crucible and pre-calcined in a muffle furnace at 800 °C for 100 min. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 100 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 1250 °C for 4 h using an Ar / H2 mixed gas (5% hydrogen by volume) as the reducing atmosphere. Finally, the sintered agglomerate was ground in a mortar and passed through a 500-mesh sieve to produce manganese-doped mechanoluminescent phosphor.

[0029] Example 15 Based on the chemical formula NaGa 0.985 O2: 0.015Mn 2+ First, the raw materials Na₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio were weighed and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. Next, the mixed raw materials were transferred to an alumina crucible and pre-calcined at 800 °C for 100 min in a muffle furnace. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 100 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 1250 °C for 4 h using an Ar / H₂ mixed gas (5% hydrogen by volume) as the reducing atmosphere. Finally, the sintered agglomerate was ground in a mortar and passed through a 500-mesh sieve to produce manganese-doped NaGaO₂ mechanoluminescent phosphor.

[0030] Example 16 According to the chemical formula (Na) 0.5 Li 0.5 )Ga 0.99 O2:0.01Mn 2+ First, weigh the raw materials Na₂CO₃, Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Next, transfer the mixed raw materials to a corundum crucible and pre-calcine at 750 °C for 100 min in a muffle furnace. After cooling, grind the pre-calcine material again in an agate mortar with anhydrous ethanol for 100 min. Then, load the ground powder into a corundum crucible and sinter it in a tube furnace at 1200 °C for 4 h using an Ar / H₂ or N₂ / H₂ mixture (5% hydrogen by volume) as the reducing atmosphere, or using N₂ as the protective gas. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare (Na₂CO₃) powder. 0.5 Li 0.5)Ga 0.99 O2:0.01Mn 2+ Mechanoluminescent phosphor.

[0031] Example 17 According to the chemical formula (Na) 0.5 Li 0.5 )Ga 0.985 O2: 0.015Mn 2+ First, weigh the raw materials Na₂CO₃, Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Next, transfer the mixed raw materials to a corundum crucible and pre-calcine at 750 °C for 100 min in a muffle furnace. After cooling, grind the pre-calcine material again in an agate mortar with anhydrous ethanol for 100 min. Then, load the ground powder into a corundum crucible and sinter it in a tube furnace at 1200 °C for 4 h using an Ar / H₂ mixture (5% hydrogen by volume) as the reducing atmosphere. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare (Na₂CO₃) powder. 0.5 Li 0.5 )Ga 0.985 O2: 0.015Mn 2+ Mechanoluminescent phosphor.

[0032] Example 18 Based on the chemical formula Na₄Ga 1.99 O5:0.01Mn 2+ First, the raw materials Na2CO3, Ga2O3, and MnCO3 in the appropriate molar ratio were weighed and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. Next, the mixed raw materials were transferred to an alumina crucible and pre-calcined at 500 °C for 100 min in a muffle furnace. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 100 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 1000 °C for 6 h using Ar / H2 and N2 / H2 mixed gases (5% hydrogen by volume) as reducing atmospheres. Finally, the sintered agglomerates were ground in a mortar and passed through a 500-mesh sieve to produce manganese-doped Na4Ga2O5 mechanoluminescent phosphor.

[0033] Example 19 According to the chemical formula Li4Ga 1.99 O5:0.01Mn 2+First, the raw materials Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio were weighed and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. Next, the mixed raw materials were transferred to an alumina crucible and pre-calcined at 500 °C for 100 min in a muffle furnace. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 100 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 1000 °C for 6 h using Ar / H₂ and N₂ / H₂ mixed gases (5% hydrogen by volume) as reducing atmospheres. Finally, the sintered agglomerates were ground in a mortar and passed through a 500-mesh sieve to produce manganese-doped Li₄Ga₂O₅ mechanoluminescent phosphor.

[0034] Example 20 Based on the chemical formula (Na2Li2)Ga 1.99 O5:0.01Mn 2+ First, weigh the raw materials Na₂CO₃, Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Next, transfer the mixed raw materials to a corundum crucible and pre-calcine at 450 °C for 100 min in a muffle furnace. After cooling, grind the pre-calcine material again in an agate mortar with anhydrous ethanol for 100 min. Then, load the ground powder into a corundum crucible and sinter it in a tube furnace at 800 °C for 4 h using Ar / H₂ and N₂ / H₂ mixed gases (5% hydrogen by volume) as reducing atmospheres. Finally, grind the sintered agglomerate in a mortar, pass it through a 500-mesh sieve, and prepare (Na₂Li₂)Ga₂O₃. 1.99 O5:0.01Mn 2+ Mechanoluminescent phosphor.

[0035] Example 21 Based on the chemical formula Li5Ga 0.99 O4:0.01Mn 2+ First, the raw materials Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio were weighed and placed in a mortar. Anhydrous ethanol was added, and the mixture was wet-milled twice until fully mixed. Next, the mixed raw materials were transferred to an alumina crucible and pre-calcined at 400 °C for 100 min in a muffle furnace. After cooling, the pre-calcined material was ground again in an agate mortar with anhydrous ethanol for 100 min. Subsequently, the ground powder was placed in an alumina crucible and sintered in a tube furnace at 550 °C for 6 h using Ar / H₂ and N₂ / H₂ mixed gases (5% hydrogen by volume) as reducing atmospheres. Finally, the sintered agglomerates were ground in a mortar, passed through a 500-mesh sieve, and manganese-doped mechanoluminescent phosphor was prepared.

[0036] Example 22 Based on the chemical formula (Na2Li3)Ga 0.99 O4:0.01Mn 2+ First, weigh the raw materials Na₂CO₃, Li₂CO₃, Ga₂O₃, and MnCO₃ in the appropriate molar ratio, place them in a mortar, add anhydrous ethanol, and wet-mill twice until fully mixed. Next, transfer the mixed raw materials to a corundum crucible and pre-calcine at 400 °C for 100 min in a muffle furnace. After cooling, grind the pre-calcine material again in an agate mortar with anhydrous ethanol for 100 min. Then, load the ground powder into a corundum crucible and sinter it in a tube furnace at 550 °C for 6 h using Ar / H₂ and N₂ / H₂ mixed gases (5% hydrogen by volume) as reducing atmospheres. Finally, grind the sintered agglomerates in a mortar, pass them through a 500-mesh sieve, and prepare (Na₂Li₃)Ga₂O₃. 0.99 O4:0.01Mn 2+ Mechanoluminescent phosphor.

[0037] Example 23 First, epoxy resin (C 11 H 12 O3) n The liquid and curing agent are mixed in a mass ratio of 10:1, and then sintered and passed through a 250-mesh sieve, metronic luminescent powder is added. a (Na 2-y Li y )O- b Ga2O3: x mol%Mn 2+ (Where 0.2≤a / b≤5, 0<x≤20, 0≤y<2), the composite slurry was prepared by stirring thoroughly with a magnetic stirrer for 0.5 hours. The slurry was then transferred to a solidification mold with a diameter of 25 cm and a depth of approximately 2 cm. It was left to stand at room temperature for 24 hours, then solidified at 60 ℃ for 6 hours. After cooling to room temperature, it was demolded to produce a cylindrical mechanoluminescent sample.

[0038] Example 24 First, epoxy resin (C 11 H 12 O3) n The liquid and curing agent are mixed in a mass ratio of 10:1, and then sintered and passed through a 250-mesh sieve, metronic luminescent powder is added. a (Na 2-y Li y )O- b Ga2O3: x mol%Mn 2+ Where 0.2≤a / b≤5, 0< x ≤20, 0≤y <2) The composite slurry was thoroughly stirred with a magnetic stirrer for 0.5 hours, transferred to a solidification mold with a diameter of 25 cm and a depth of about 2 cm, and left to stand at room temperature for 24 hours. Then it was solidified at 60 ℃ for 6 hours and cooled to room temperature before demolding. A thin rod-shaped mechanoluminescent sample was prepared.

[0039] Example 25 Mechanoluminescent powder a (Na 2-y Li y )O- b Ga2O3: x mol%Mn 2+ 0.2≤a / b≤5, 0< x ≤20, 0≤ y <2. A dispersion was prepared by ultrasonic dispersion in N,N-dimethylacetamide (DMAc). PVDF, PVDF-TrFE, or biphenyl-type PI precursor polyamic acid (PAA) was added and magnetically stirred for 30 min to prepare a composite slurry. Mechanoluminescent powder / polymer composite film structures were then prepared using a casting method, with a polymer to mechanoluminescent powder mass ratio of 10:3. The film was heated at 65℃ for 6 hours, followed by heat treatment at 140℃ using a gradient heating method for 4 hours. The resulting composite film thickness ranged from 5 to 200 μm depending on the template specifications.

[0040] Example 26 Mechanoluminescent powder a (Na 2-y Li y )O- b Ga2O3: x mol%Mn 2+ 0.2≤a / b≤5, 0< x ≤20, 0≤ y <2, ultrasonically dispersed in thermosetting photosensitive polyimide (PSPI) and N,N-dimethylacetamide (DMAc), and magnetically stirred for 30 min to prepare a composite slurry. Then, a mechanoluminescent powder / PSPI composite film structure is prepared using a casting method, wherein the mass ratio of PSPI to mechanoluminescent powder is 10:3, and an appropriate amount of N,N-dimethylacetamide (DMAc) is added. The mixture is heated at 150 ℃ for 6 hours, followed by heat treatment at 140 ℃ using a gradient heating method, with a holding time of 4 hours. The resulting composite film has a thickness between 5-200 μm depending on the template specifications.

[0041] Table 1 shows the main performance parameters of fluorescence and mechanoluminescence of materials from samples with different compositions and sintered under different atmospheres.

[0042] Table 1. Main performance parameters of sample fluorescence and methemoluminescence By adjusting the molar ratio of alkali metal elements to gallium, and changing the sintering atmosphere, sintering temperature, and holding time, the emission color and intensity of mechanoluminescence in materials can be effectively controlled. Different polymer composites can yield mechanoluminescent samples of different shapes and hardnesses, allowing for convenient testing of mechanoluminescence as needed.

Claims

1. A phosphor, characterized by, The phosphor is selected from any one of the following: NaGa 2.99 O5:0.01Mn 2+ , LiGa 2.99 O5:0.01Mn 2+ , (Na 0.5 Li 0.5 )Ga 2.99 O5:0.01Mn 2+ , Na2Ga 3.985 O7:0.015Mn 2+ , Na4Ga 1.99 O5:0.01Mn 2+ , Li4Ga 1.99 O5:0.01Mn 2+ , (Na2Li2)Ga 1.99 O5:0.01Mn 2+ , Li5Ga 0.99 O4:0.01Mn 2+ and (Na2Li3)Ga 0.99 O4:0.01Mn 2+ .

2. A method of producing the phosphor according to claim 1, characterized by, Includes the following steps: S1: According to the stoichiometric ratio of the phosphor, place the sodium source, gallium source and manganese source, or the sodium source, lithium source, gallium source and manganese source, or the lithium source, gallium source and manganese source in a mortar, add anhydrous ethanol, and grind until fully mixed; S2: Transfer the mixture obtained in step S1 to a corundum crucible for pre-firing; after the pre-firing material cools, place the pre-firing material in an agate mortar, add anhydrous ethanol and grind again; S3: The grinding powder obtained in step S2 is placed into an alumina crucible and sintered at high temperature in a mixed atmosphere of inert gas and hydrogen. After sintering, the sintered agglomerate is crushed and sieved to obtain the phosphor.

3. The method for preparing phosphor according to claim 2, characterized in that, The sodium source is Na2CO3, the lithium source is Li2CO3, the gallium source is Ga2O3, and the manganese source is MnCO3.

4. The method for preparing phosphor according to claim 2, characterized in that: The preheating temperature in S2 is 400-1000℃, and the time is 0.5-20h.

5. The method for preparing phosphor according to claim 2, characterized in that: The conditions for high-temperature sintering in S3 are as follows: heat up to 500-1400℃ at a rate of 1-15℃ / min and hold for 2-16 hours, and finally cool down to 500℃ at a rate of 1-15℃ / min.

6. The method for preparing phosphor according to claim 2, characterized in that, The inert gas mentioned in S3 is nitrogen or argon.

7. The application of the phosphor as described in claim 1, characterized in that, The method steps are as follows: The phosphor is compounded with polydimethylsiloxane, polyvinylidene fluoride, a copolymer of polyvinylidene fluoride and trifluoroethylene or photosensitive polyimide, and a luminescent powder / polymer composite film is prepared by spin casting, casting or hot pressing.

8. The application of the phosphor as described in claim 1, characterized in that, The method steps are as follows: The phosphor is compounded with epoxy resin, polydimethylsiloxane, polyvinylidene fluoride, copolymer of polyvinylidene fluoride and trifluoroethylene or photosensitive polyimide and curing agent, and the luminescent powder / polymer cylindrical luminescent material is prepared by the cold solidification method.

Citation Information

Patent Citations

  • Luminous eraser and preparation method thereof

    CN115746470A