Application of hydrogenated graphdiyne material in field of H2S gas sensing
By using the mesoporous structure and high-active sp carbon hybridization characteristics of hydrogenated graphiteyne materials, the problems of high detection threshold and poor stability of existing H2S gas sensing detection materials are solved, and rapid response and high sensitivity detection of H2S gas are achieved , significantly improves detection performance.
Patent Information
- Application Number
- CN202410934591.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
The existing H2S gas sensing detection materials have problems such as high detection threshold, high operating temperature and poor stability, making it difficult to effectively detect H2S gas.
Hydrographyne material is used as a new two-dimensional structural carbon material. Through its mesoporous structure and highly active sp carbon hybrid structure, combined with electrostatic interaction, it is used for H2S gas sensing, and prepare hydrogenated graphyne slurry and coated on gas. The resensitode chip is used for H2S gas sensing testing after ultrasonic treatment and drying.
It realizes rapid response and high sensitivity detection to H2S gas, lowers the detection threshold, improves the stability of the material and operating temperature range, and significantly improves the sensing performance of H2S gas.
Smart Images

Figure CN118896984A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of gas-sensitive materials and environmental detection, and in particular relates to an application of hydrogenated graphene material in the field of H2S gas sensing. Background Art
[0002] H2S is widely derived from common industries such as petroleum, steelmaking and papermaking. In daily life, sewage discharge, garbage accumulation and other behaviors will also produce H2S due to the decomposition of organic matter. As a typical malodorous gas, the olfactory threshold of H2S is extremely low, and it will cause nausea and poisoning when it is higher than 30ppm. In industrial production, the presence of H2S can easily lead to the deactivation of catalysts and corrosion of production equipment, seriously affecting production safety. Therefore, it is necessary to provide a highly sensitive and stable H2S gas-sensitive detection material. Summary of the invention
[0003] In order to solve the above technical problems, the present invention proposes an application of hydrogenated graphene material in the field of H2S gas sensing.
[0004] To achieve the above objectives, the present invention provides an application of hydrogenated graphene material in the field of H2S gas sensing.
[0005] Hydrogenated graphene (HsGDY) is a new type of two-dimensional carbon material composed of sp and sp 2 The carbon hybrid composition has a typical mesoporous structure, which is conducive to the mass transfer of gas molecules. The presence of sp carbon makes the surface electrostatic potential of HsGDY uneven, which is beneficial to provide stronger electrostatic interaction. In addition, the special electronic structure gives it a good energy gap structure. The adsorption of gas molecules on the surface will cause changes in the electronic structure of HsGDY, and the energy gap value will also change accordingly. Therefore, it has good application potential in the field of gas sensing.
[0006] Furthermore, the hydrogenated graphene material is immersed in a solvent, and ultrasonic treatment is performed to disperse the material uniformly to obtain hydrogenated graphene slurry; the hydrogenated graphene slurry is drop-coated on the center of a gas-sensitive electrode chip, and the gas-sensitive electrode chip is dried and used for H2S gas sensing testing.
[0007] Furthermore, the material-liquid ratio of hydrogenated graphene to solvent is 1 mg: (1-5) μL.
[0008] Furthermore, the solvent is a mixed solution of isopropanol and water, and the volume ratio of the isopropanol to deionized water is (1-5):1.
[0009] Furthermore, the ultrasonic treatment time is 10 to 20 minutes.
[0010] Furthermore, the drying temperature is 50-100° C., and the drying time is 5-10 hours.
[0011] Furthermore, the temperature of the H2S gas sensing test is 10°C to 150°C.
[0012] Furthermore, in the H2S gas sensing test, the concentration of H2S is 1-50 ppm, and the total gas flow rate is 1 L / min.
[0013] Compared with the prior art, the present invention has the following advantages and technical effects:
[0014] The commonly used H2S gas sensing test materials in the prior art have problems such as high detection threshold, high working temperature, poor stability, etc. The present invention proposes a hydrogenated graphene material and uses it in H2S gas sensing. The hydrogenated graphene material used in the present invention has a regular mesoporous structure, which is conducive to the mass transfer of H2S molecules in the pores. The large conjugated π bond provides it with good structural stability. The highly active sp carbon hybrid structure provides electrostatic interaction for the binding of H2S molecules, which is conducive to the rapid response of the gas. Therefore, hydrogenated graphene has excellent application potential in H2S gas sensitive detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0016] Figure 1 This is a scanning electron microscope image of hydrogenated graphene attached to the gas-sensitive electrode chip substrate in Example 1;
[0017] Figure 2 The structural characterization diagram of hydrogenated graphene (HsGDY) material, (a) is the Raman spectrum, and b is the XPS C1s spectrum;
[0018] Figure 3 The test results of hydrogenated graphene materials in H2S gas sensing detection in Examples 1 to 5;
[0019] Figure 4 The test results of the response and recovery time of the hydrogenated graphene material in H2S gas sensing (a) and the cyclic response (b) in Example 3;
[0020] Figure 5 These are the test results of hydrogenated Graphene materials in H2S gas sensing detection in Examples 6 to 7 (a) and Comparative Examples 1 to 5 (b). DETAILED DESCRIPTION
[0021] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0022] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0023] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0024] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0025] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0026] The embodiment of the present invention provides an application of hydrogenated graphene material in the field of H2S gas sensing.
[0027] In a preferred embodiment of the present invention, the hydrogenated graphene material is prepared according to the following method:
[0028] 10 mg of cuprous iodide, 20 mg of bistriphenylphosphine palladium dichloride and 30 mL of redistilled triethylamine were added to a three-necked flask and stirred for 10 min under the condition of heating in an oil bath at 60°C to obtain a mixed solution. 400 mg of 1,3,5-alkynylbenzene was added to 50 mL of anhydrous tetrahydrofuran to dissolve and then transferred to a constant pressure titration funnel and added to the above mixed solution at a drop rate of 3-4 seconds per drop. The mixture was heated in an oil bath at 60°C and reacted in the dark for 24 hours to obtain a brown-black powder. The excess copper ions were further removed by heating under reflux with 2M HCl and NaOH to obtain hydrogenated graphene (HsGDY).
[0029] In a preferred embodiment of the present invention, the hydrogenated graphene material is immersed in a solvent, and ultrasonic treatment is performed to disperse the material uniformly to obtain hydrogenated graphene slurry; the hydrogenated graphene slurry is drop-coated on the center of a gas-sensitive electrode chip, and the gas-sensitive electrode chip is dried and used for H2S gas sensing testing.
[0030] In a preferred embodiment of the present invention, the material-liquid ratio of hydrogenated graphene to solvent is 1 mg: (1-5) μL.
[0031] In a preferred embodiment of the present invention, the solvent is a mixed solution of isopropyl alcohol and deionized water.
[0032] More preferably, the volume ratio of isopropanol to deionized water is (1-5):1.
[0033] The liquid-to-solvent ratio of hydrogenated graphene will affect the viscosity of the slurry, and the volume ratio of isopropyl alcohol to deionized water will affect the growth and adhesion of hydrogenated graphene on the gas-sensitive electrode chip during slurry coating, thereby affecting the performance of gas sensing detection.
[0034] In a preferred embodiment of the present invention, the ultrasonic treatment time is 10 to 20 minutes. In a preferred embodiment of the present invention, the drying temperature is 50 to 100° C. and the drying time is 5 to 10 hours.
[0035] In a preferred embodiment of the present invention, the temperature of the H2S gas sensing test is 10°C to 150°C.
[0036] In a preferred embodiment of the present invention, the concentration of H2S in the H2S gas sensing test is 1-50 ppm, and the total gas flow rate is 1 L / min.
[0037] The technical solution of the present invention is further illustrated by the following embodiments.
[0038] Example 1
[0039] An application of hydrogenated graphene material in H2S gas sensing detection comprises the following steps:
[0040] The hydrogenated graphene (HsGDY) material was immersed in a solvent, and the hydrogenated graphene slurry was obtained after ultrasonic treatment and uniform dispersion. The hydrogenated graphene slurry was coated on the center of the gas sensitive chip and placed in an oven for drying. Then, the corresponding gas was introduced for gas sensing test. The solvent was a mixed solution of isopropanol and deionized water, and the volume ratio of isopropanol to deionized water was 1:1. The amount of hydrogenated graphene was 10 mg, and the amount of solvent was 50 μL. The ultrasonic time was 20 min. The oven temperature was 60 ° C, and the drying time was 10 h.
[0041] The gas sensing test conditions are as follows: the gas sensing test temperature is 30°C, the gas sensing test atmosphere is 10ppmH2S, air balance, and the total flow rate is 1L / min.
[0042] Figure 1 This is a scanning electron microscope image of hydrogenated graphene attached to the gas-sensing electrode chip substrate in Example 1. It can be seen that the hydrogenated graphene is uniformly attached to the gas-sensing electrode chip, and the hydrogenated graphene is a block-like stacking structure.
[0043] Figure 2 This is the structural characterization diagram of hydrogenated graphene (HsGDY) material. Figure 2 (a) is the Raman spectrum at 2000cm -1 The characteristic peaks appearing near indicate the presence of acetylenic bonds. Figure 2 (b) is the XPS C1s spectrum of hydrogenated Graphene. By performing peak separation, the existence of sp carbon structure can be observed. Structural characterization confirms the sp-sp 2 Hybridized carbon structure.
[0044] Example 2
[0045] An application of hydrogenated graphene material in H2S gas sensing detection comprises the following steps:
[0046] The hydrogenated graphene (HsGDY) material was immersed in a solvent, and the hydrogenated graphene slurry was obtained after ultrasonic treatment and uniform dispersion. The hydrogenated graphene slurry was coated on the center of the gas sensitive chip and placed in an oven for drying. Then, the corresponding gas was introduced for gas sensing test. The solvent was a mixed solution of isopropanol and deionized water, and the volume ratio of isopropanol to deionized water was 3:1. The amount of hydrogenated graphene was 10 mg, and the amount of solvent was 50 μL. The ultrasonic time was 20 min. The oven temperature was 60 ° C, and the drying time was 10 h.
[0047] The gas sensing test conditions are as follows: the gas sensing test temperature is 30°C, the gas sensing test atmosphere is 10ppmH2S, air balance, and the total flow rate is 1L / min.
[0048] Example 3
[0049] An application of hydrogenated graphene material in H2S gas sensing detection comprises the following steps:
[0050] The hydrogenated graphene (HsGDY) material is immersed in a solvent, and is evenly dispersed by ultrasonic treatment to obtain a hydrogenated graphene slurry. The hydrogenated graphene slurry is coated on the center of a gas sensitive chip and placed in an oven for drying. Then, the corresponding gas is introduced for a gas sensing test. The solvent is a mixed solution of isopropanol and deionized water, and the volume ratio of isopropanol to deionized water is 2:1. The amount of hydrogenated graphene is 10 mg, and the amount of solvent is 50 μL. The ultrasonic time is 20 min. The oven temperature is 60 ° C, and the drying time is 10 h.
[0051] The gas sensing test conditions are as follows: the gas sensing test temperature is 30°C, the gas sensing test atmosphere is 10ppmH2S, air balance, and the total flow rate is 1L / min.
[0052] Example 4
[0053] An application of hydrogenated graphene material in H2S gas sensing detection comprises the following steps:
[0054] The hydrogenated graphene (HsGDY) material is immersed in a solvent, and is evenly dispersed by ultrasonic treatment to obtain a hydrogenated graphene slurry. The hydrogenated graphene slurry is coated on the center of a gas sensitive chip and placed in an oven for drying. Then, the corresponding gas is introduced for a gas sensing test. The solvent is a mixed solution of isopropanol and deionized water, and the volume ratio of isopropanol to deionized water is 2:1. The amount of hydrogenated graphene is 10 mg, and the amount of solvent is 50 μL. The ultrasonic time is 20 min. The oven temperature is 60 ° C, and the drying time is 10 h.
[0055] The gas sensing test conditions are as follows: the gas sensing test temperature is 50°C, the gas sensing test atmosphere is 10ppmH2S, air balance, and the total flow rate is 1L / min.
[0056] Example 5
[0057] An application of hydrogenated graphene material in H2S gas sensing detection comprises the following steps:
[0058] The hydrogenated graphene (HsGDY) material was immersed in a solvent, and the hydrogenated graphene slurry was obtained after ultrasonic treatment and uniform dispersion. The hydrogenated graphene slurry was coated on the center of the gas sensitive chip and placed in an oven for drying. Then, the corresponding gas was introduced for gas sensing test. The solvent was a mixed solution of isopropanol and deionized water, and the volume ratio of isopropanol to deionized water was 2:1. The amount of hydrogenated graphene was 10 mg, and the amount of solvent was 30 μL. The ultrasonic time was 20 min. The oven temperature was 60 ° C, and the drying time was 10 h.
[0059] The gas sensing test conditions are as follows: the gas sensing test temperature is 100°C, the gas sensing test atmosphere is 10ppmH2S, air balance, and the total flow rate is 1L / min.
[0060] Gas sensing performance test
[0061] The response value is calculated as:
[0062]
[0063] Where S is the response value, R A is the resistance value in air, R G is the resistance value in the test gas.
[0064] The test results of hydrogenated graphene materials in H2S gas sensing detection in Examples 1 to 5 are shown in Figure 3 Among them, the response value S in Example 1 (HsGDY-S1) is 71.4%, the response value S in Example 2 (HsGDY-S2) is 54.6%, the response value S in Example 3 (HsGDY-S3) is 214.1%, the response value S in Example 4 (HsGDY-S4) is 98.6%, and the response value S in Example 5 (HsGDY-S5) is 92.2%. It can be seen that each embodiment has a good response value to H2S gas, among which the highest response value in Example 3 is 214.1%, which has good gas sensing performance.
[0065] The test results of the response and recovery time of the hydrogenated graphene material in H2S gas sensing detection and the test results of the cyclic response are shown in Example 3. Figure 4 , Figure 4 The response time of H2S gas in (a) is 18s and the recovery time is 27s. Figure 4 After 5 cycles of response in (b), the hydrogenated Graphene material still maintains good gas sensing performance.
[0066] Example 6
[0067] An application of hydrogenated graphene material in H2S gas sensing detection comprises the following steps:
[0068] The hydrogenated graphene (HsGDY) material was immersed in a solvent, and the hydrogenated graphene slurry was obtained after ultrasonic treatment and uniform dispersion. The hydrogenated graphene slurry was coated on the center of the gas sensitive chip and placed in an oven for drying. Then, the corresponding gas was introduced for gas sensing test. The solvent was a mixed solution of isopropanol and deionized water, and the volume ratio of isopropanol to deionized water was 2:1. The amount of hydrogenated graphene was 1 mg, and the amount of solvent was 10 μL. The ultrasonic time was 10 min. The oven temperature was 50 ° C, and the drying time was 6 h.
[0069] The gas sensing test conditions are as follows: the gas sensing test temperature is 10°C, the gas sensing test atmosphere is 1ppmH2S, air balance, and the total flow rate is 1L / min.
[0070] Example 7
[0071] An application of hydrogenated graphene material in H2S gas sensing detection comprises the following steps:
[0072] The hydrogenated graphene (HsGDY) material was immersed in a solvent, and the hydrogenated graphene slurry was obtained after ultrasonic treatment and uniform dispersion. The hydrogenated graphene slurry was coated on the center of the gas sensitive chip and placed in an oven for drying. Then, the corresponding gas was introduced for gas sensing test. The solvent was a mixed solution of isopropanol and deionized water, and the volume ratio of isopropanol to deionized water was 2:1. The amount of hydrogenated graphene was 8 mg, and the amount of solvent was 40 μL. The ultrasonic time was 15 min. The oven temperature was 100 ° C, and the drying time was 5 h.
[0073] The gas sensing test conditions are as follows: the gas sensing test temperature is 150°C, the gas sensing test atmosphere is 50ppmH2S, air balance, and the total flow rate is 1L / min.
[0074] Comparative Example 1
[0075] The application of hydrogenated graphene in H2S gas sensing detection includes the following steps:
[0076] The hydrogenated graphene (HsGDY) material was immersed in a solvent, and the hydrogenated graphene slurry was obtained after ultrasonic treatment and uniform dispersion. The hydrogenated graphene slurry was coated on the center of the gas sensitive chip and placed in an oven for drying. Then, the corresponding gas was introduced for gas sensing test. The solvent was deionized water. The amount of hydrogenated graphene was 10 mg, and the amount of solvent was 50 μL. The ultrasonic time was 20 min. The oven temperature was 60 ° C, and the drying time was 10 h.
[0077] The gas sensing test conditions are as follows: the gas sensing test temperature is 30°C, the gas sensing test atmosphere is 10ppmH2S, air balance, and the total flow rate is 1L / min.
[0078] Comparative Example 2
[0079] An application of hydrogenated graphene material in H2S gas sensing detection is the same as Example 3, except that the amount of hydrogenated graphene used is 10 mg and the amount of solvent used is 100 μL.
[0080] Comparative Example 3
[0081] An application of hydrogenated graphene material in H2S gas sensing detection is the same as Example 3, except that the volume ratio of isopropanol to deionized water is 6:1.
[0082] Comparative Example 4
[0083] An application of hydrogenated graphene material in H2S gas sensing is the same as Example 3, except that the oven temperature is 150°C and the drying time is 10 hours.
[0084] Comparative Example 5
[0085] An application of hydrogenated graphene material in H2S gas sensing detection is the same as Example 3, except that the gas sensing test temperature is 200°C.
[0086] The performance test results of Examples 6 to 7 and Comparative Examples 1 to 5 are as follows Figure 5 As shown. It can be seen that the response value S=61.3% in Example 6 (HsGDY-S6) and the response value S=132.4% in Example 7 (HsGDY-S7), and there are still considerable response values under low temperature and low concentration / high temperature and high concentration environments. There is almost no response value in the tests of Comparative Example 1 (HsGDY-D1) and Comparative Example 5 (HsGDY-D5). This is because the solvent in Comparative Example 1 is only deionized water, and the hydrogenated graphene material cannot be well coated and grown on the gas-sensitive electrode chip. After drying, the hydrogenated graphene will fall off, so the response phenomenon is abnormal; the gas sensing test temperature in Comparative Example 5 is too high, which causes the physical and chemical structure of the hydrogenated graphene material to be destroyed, so no response value can be generated. The response value S in Comparative Example 2 (HsGDY-D2) is 40.7%, the response value S in Comparative Example 3 (HsGDY-D3) is 38.5%, and the response value S in Comparative Example 4 (HsGDY-D4) is 85.2%, which are significantly lower than those in Example 3.
[0087] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. Application of hydrogenated graphene materials in H2S gas sensing field.
2. The application of the hydrogenated graphene material according to claim 1 in the field of H2S gas sensing, characterized in that: The hydrogenated graphene material is immersed in a solvent, and the hydrogenated graphene slurry is prepared after being dispersed evenly by ultrasonic treatment; the hydrogenated graphene slurry is drop-coated on the center of a gas-sensitive electrode chip, and the gas-sensitive electrode chip is dried and used for H2S gas sensing test.
3. The application of the hydrogenated graphene material according to claim 2 in the field of H2S gas sensing, characterized in that: The material-liquid ratio of the hydrogenated graphene material to the solvent is 1 mg: (1-5) μL.
4. The use of the hydrogenated graphene material according to claim 3 in the field of H2S gas sensing, characterized in that: The solvent is a mixed solution of isopropanol and water.
5. The use of the hydrogenated graphene material according to claim 4 in the field of H2S gas sensing, characterized in that: The volume ratio of the isopropanol to water is (1-5):
1.
6. The use of the hydrogenated graphene material according to claim 2 in the field of H2S gas sensing, characterized in that: The ultrasonic treatment time is 10 to 20 minutes.
7. The use of hydrogenated graphene material according to claim 2 in the field of H2S gas sensing, characterized in that: The drying temperature is 50-100° C., and the drying time is 5-10 hours.
8. The use of hydrogenated graphene material according to claim 2 in the field of H2S gas sensing, characterized in that: The temperature of the H2S gas sensing test is 10°C to 150°C.
9. The use of hydrogenated graphene material in the field of H2S gas sensing according to claim 2, characterized in that: In the H2S gas sensing test, the concentration of H2S is 1-50 ppm, and the total gas flow rate is 1 L / min.