Sulfide-doped material, preparation method thereof and lithium ion battery

By introducing nitrogen into the sulfide solid electrolyte to form Li3N, the stability problem between the sulfide solid electrolyte and the lithium metal anode is solved, achieving high ionic conductivity and stability, and improving the energy density and cycle life of lithium-ion batteries.

CN118899435APending Publication Date: 2024-11-05HUAWEI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310498682.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing sulfide solid electrolyte has a narrow electrochemical stability window between the lithium metal anode and the battery, which leads to severe lithium dendrite growth and poses a safety hazard. Furthermore, existing improvement methods often affect the ionic conductivity of the battery or increase complexity and cost.

Method used

By using doped sulfide materials, nitrogen is introduced into the unit cell of the sulfide material to form Li3N, which hinders side reactions. The unit cell volume is increased by using large-volume doping groups, thereby improving ionic conductivity and stability.

Benefits of technology

It achieves high ionic conductivity and good stability against metallic lithium, suppresses lithium dendrite growth, improves the energy density and cycle life of lithium-ion batteries, and reduces the complexity and cost of preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899435A_ABST
    Figure CN118899435A_ABST
Patent Text Reader

Abstract

The invention discloses a doped sulfide material, a preparation method thereof and a lithium ion battery. The crystal of the doped sulfide material comprises: a cubic crystal with a space point group of # imgabs0 #; at least one site in unit cells forming the crystal is doped with a doping group, and the doping group comprises a nitrogen element N. The sulfide-doped crystal disclosed by the invention comprises a cubic crystal form of which the space point group is # imgabs1 #, and the doped sulfide has relatively high ionic conductivity. Besides, at least one site in unit cells of the sulfide-doped material is doped with a doping group containing N, N can be combined with Li to form Li3N, and the existence of Li3N can hinder side reaction of the sulfide-doped material and metal lithium to a certain extent, so that the sulfide-doped material provided by the implementation mode has relatively good stability to the metal lithium. The sulfide-doped material disclosed by the implementation mode can be applied to the lithium ion battery as a sulfide solid electrolyte, so that the lithium ion battery has a relatively long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium-ion batteries, in particular to doped sulfide materials and preparation methods thereof, and lithium-ion batteries. Background Art

[0002] Lithium ion cells and batteries include: positive electrode, negative electrode and electrolyte. + ) The battery is charged or discharged by stripping or depositing back and forth between the positive electrode and the negative electrode. Usually, the positive electrode and the negative electrode are connected by an electrolyte. As an important component of lithium-ion batteries, the electrolyte plays a role in conducting Li between the positive electrode and the negative electrode. + and conduction current.

[0003] Currently disclosed electrolytes may include: liquid electrolytes and solid electrolytes. Solid electrolytes are widely used because of their high room temperature ionic conductivity. Existing solid electrolytes mainly include: oxide solid electrolytes, sulfide solid electrolytes, polymer solid electrolytes and halide solid electrolytes. Among them, sulfide solid electrolytes are solid electrolytes with high room temperature ionic conductivity.

[0004] The electrochemical stability window between the materials used in sulfide solid electrolytes and the metallic lithium negative electrode is relatively narrow, resulting in serious interfacial side reactions between the metallic lithium negative electrode and the sulfide electrolyte during battery charging and discharging. Summary of the invention

[0005] The present application discloses a doped sulfide material and a preparation method thereof, and a lithium-ion battery. The doping group of the doped sulfide material includes nitrogen element N, which can combine with Li to form Li3N. The presence of Li3N can hinder the side reaction between the doped sulfide material and metallic lithium to a certain extent, so that the doped sulfide material has better stability to metallic lithium.

[0006] In a first aspect, the present application provides a doped sulfide material, wherein a crystal of the doped sulfide material comprises: a space point group of Cubic crystal form; at least one site in the unit cell constituting the crystal is doped with a doping group, and the doping group includes: nitrogen element.

[0007] In this implementation, the sulfide-doped crystal includes: a space point group of In the cubic crystal form, the doped sulfide has a high ionic conductivity. Additionally, at least one site in the unit cell of the doped sulfide material is doped with a doping group containing N, and N can combine with Li to form Li3N. The presence of Li3N can, to a certain extent, hinder the side reaction between the doped sulfide material and metallic lithium. Therefore, the doped sulfide material disclosed in the embodiments of the present application has better stability towards metallic lithium.

[0008] In a possible implementation, the chemical formula of the doped sulfide material includes: Li6PS5Cl 1-n1 X n1 , where X is a doping group and 0 < n1 ≤ 0.2. Combining this implementation, the chemical formula of the doped sulfide material includes: Li6PS5Cl 1-n1 X n1 , which can achieve the high conductivity performance of the doped sulfide material. 0 < n1 ≤ 0.2 can balance the better stability performance (towards metallic lithium) and high conductivity performance of the doped sulfide material.

[0009] In a possible implementation, the chemical formula of the doped sulfide material includes: Li 7-n2 PS 6-n X n2 , which can achieve the high conductivity performance of the doped sulfide material. 0 < n2 ≤ 0.5 can balance the better stability performance (towards metallic lithium) and high conductivity performance of the doped sulfide material.

[0010] In a possible implementation, the doping amount of the doping group is between 0.01% - 20%.

[0011] In this implementation, the doping amount of the doping group being less than 20% can achieve the high conductivity performance of the doped sulfide material. The doping amount of the doping group in the doped sulfide material being greater than or equal to 0.01% enables the doped sulfide material to have better stability towards metallic lithium. The doping amount of the doping group being between 0.01% - 20% can balance the better stability performance (towards metallic lithium) and high conductivity performance of the doped sulfide material.

[0012] Combined with the fourth implementation of the first aspect, the volume of the doping group is larger than the volume of the sulfide ion.

[0013] In this implementation, the doping group with a volume larger than the S ion can be called a large - volume doping group. The introduction of the large - volume doping group can expand the unit cell volume, and the ion channels in the unit cell have larger sizes, which can alleviate the capacity attenuation during the ion transport in the unit cell, enabling the doped sulfide material to have a large ionic conductivity.

[0014] In addition, the introduction of bulky doping groups can improve the mechanical properties of doped sulfide materials, reduce the Young's modulus of doped sulfide materials, soften the doped sulfide materials, and improve the processability of doped sulfide materials.

[0015] In a possible implementation manner, the doping group includes at least one of thiocyanate ions and cyanide ions.

[0016] In this implementation, the doping group includes: at least one of thiocyanate ions and cyanide ions. N in the thiocyanate ions / cyanide ions can combine with Li to form Li3N. The presence of Li3N can hinder the side reaction of the doped sulfide material with metallic lithium to a certain extent. Therefore, the doped sulfide material disclosed in the embodiment of the present application has better stability to metallic lithium.

[0017] In addition, both thiocyanate ions and cyanide ions are large-volume doping groups. The introduction of large-volume doping groups can expand the unit cell volume. The ion channels in the unit cell have a larger size, which can alleviate the capacity attenuation during ion transmission in the unit cell, making the doped sulfide material have a larger ionic conductivity.

[0018] The second aspect of the present application provides a method for preparing a sulfide material, comprising: mixing raw materials; crystallizing the mixed raw materials to obtain a doped sulfide material, wherein the crystal of the doped sulfide material comprises: a space point group of Cubic crystal form; at least one site in the unit cell constituting the crystal is doped with a doping group, and the doping group includes: nitrogen element.

[0019] The method for preparing the doped sulfide material disclosed in this implementation mode, the crystal of the prepared sulfide material includes: the space point group is The doped sulfide has a cubic crystal form, and the doped sulfide has a high ionic conductivity. In addition, at least one site in the unit cell of the doped sulfide material is doped with a doping group containing N. N can combine with Li to form Li3N. The presence of Li3N can hinder the side reaction of the doped sulfide material with metallic lithium to a certain extent. Therefore, the doped sulfide material prepared by this implementation has better stability to metallic lithium.

[0020] In a possible implementation method, the raw materials include: lithium salt, and the lithium salt includes: doping groups and lithium ions. Before the step of mixing the raw materials, the preparation method also includes: heating the lithium salt to a first temperature for drying, the first temperature is greater than the melting point of the lithium salt, and the first temperature is less than the decomposition temperature of water; heating the dried lithium salt to a second temperature for drying, and the second temperature is higher than the first temperature.

[0021] In this implementation, the lithium salt is dried in two steps. The temperature of the first drying step is the first temperature. It is necessary to ensure that the first temperature is greater than the melting point of the lithium salt, so that the lithium salt is in a melting state at the first temperature, so that the crystal water inside the lithium salt can be released. The first temperature is lower than the decomposition temperature of water, so that the released crystal water exists in the form of water molecules, avoiding the introduction of interfering substances (Li2O) during the first drying process.

[0022] The temperature of the second drying step is the second temperature to further remove the crystal water in the lithium salt.

[0023] In a possible implementation, the step of mixing the raw materials is specifically as follows: using ball-milled extruded raw materials.

[0024] In this implementation, mixing the raw materials by ball milling can better introduce the doping atoms into the unit cell.

[0025] The third aspect of the present application provides a lithium ion battery, comprising: a metal lithium negative electrode, a sulfide solid electrolyte and a positive electrode; the sulfide solid electrolyte is arranged between the metal lithium negative electrode and the positive electrode; the material used for the sulfide solid electrolyte includes: a doped sulfide material, and the crystal of the doped sulfide material includes: a space point group of Cubic crystal form; at least one site in the unit cell constituting the crystal is doped with a doping group, and the doping group includes: nitrogen element.

[0026] In this implementation, the lithium-ion battery uses a metal lithium negative electrode. The material used for the metal lithium negative electrode includes: metal lithium. Since metal lithium has extremely high specific capacity and low redox potential, the lithium-ion battery has a high energy density.

[0027] The lithium-ion battery uses the doped sulfide disclosed in the first aspect as the material of the sulfide solid electrolyte. The sulfide solid electrolyte has a higher electrical conductivity, and the lithium-ion battery can have a higher energy density.

[0028] At least one site in the unit cell of the doped sulfide material is doped with a doping group containing N. N can combine with Li in the metal lithium negative electrode to form Li3N. Li3N can hinder the side reaction between the sulfide solid electrolyte and the metal lithium negative electrode to a certain extent, inhibit the growth of lithium dendrites on the surface of the metal lithium negative electrode, and the lithium-ion battery has a long cycle life and high safety.

[0029] Li3N can stabilize the interface between the metal lithium negative electrode and the sulfide solid electrolyte, so that during the charge and discharge process of the lithium-ion battery: Li+ can be uniformly deposited or stripped, so that the lithium-ion battery disclosed in the embodiment of the present application has good stability.

[0030] In a possible implementation, the materials used for the positive electrode include: doped sulfide material, positive electrode material and conductive carbon.

[0031] In this implementation, the materials used for the positive electrode include: conductive carbon and the doped sulfide material provided in the first aspect. The doped sulfide material is a public reaction site for Li+. The conductive carbon has a porous structure, so that the contact area between the positive electrode and Li+ is large, and Li+ can be uniformly deposited or stripped on the surface of the positive electrode, thereby improving the stability of the lithium-ion battery.

[0032] In combination with the second implementation of the third aspect, among the materials used for the positive electrode, the mass fraction of the doped sulfide material is 10%-30%; the mass fraction of the positive electrode material is 65%-80%; and the mass fraction of the conductive carbon is 2%-5%.

[0033] In a possible implementation, the materials used for the positive electrode include: doped sulfide material, positive electrode material and adhesive.

[0034] In this implementation, the materials used for the positive electrode include: a binder and the doped sulfide material provided in the first aspect. The doped sulfide material is a public reaction site for Li+. The binder increases the adhesion between the positive electrode material and the doped sulfide material, thereby improving the mechanical strength of the positive electrode.

[0035] In a possible implementation, among the materials used for the positive electrode, the mass fraction of the doped sulfide material is 10%-30%; the mass fraction of the positive electrode material is 68%-80%; and the mass fraction of polytetrafluoroethylene is 0.5%-3%. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is a schematic diagram of a lithium-ion battery;

[0037] Figure 2 is the XRD pattern of sulfide solid electrolyte;

[0038] Figure 3 A diagram showing relevant experimental results in the related art disclosed in the first aspect;

[0039] Figure 4 It is a diagram of relevant experimental results in the disclosure of related technology 2;

[0040] Figure 5 It is a diagram of relevant experimental results in the third disclosure of related technology;

[0041] Figure 6 It is a diagram of relevant experimental results in the fourth disclosure of the related technology;

[0042] Figure 7 It is a diagram of relevant experimental results in the fifth disclosure of the related technology;

[0043] Figure 8 The doped sulfide material Li6PS5Cl provided in the embodiment of the present application 1-n1 (SCN) n1 Schematic diagram of the unit cell;

[0044] Fig. 9 Li6PS5Cl 1-n1 (SCN) n1 and XRD patterns of Li6PS5Cl;

[0045] Fig.10 Li6PS5Cl 1-n1 SCN n1 and lattice parameter diagram of Li6PS5Cl;

[0046] Fig.11 Li6PS5Cl 1-n1 SCN n1 and crystal size diagram of Li6PS5Cl;

[0047] Fig.12 Li6PS5Cl 1-n1 SCN n1 and the impedance curves of Li6PS5Cl;

[0048] Fig.13 Li6PS5Cl 1-n1 SCN n1 Schematic diagram of the conductivity of Li6PS5Cl;

[0049] Fig.14 This is a flow chart of the preparation method of the doped sulfide material disclosed in the embodiments of the present application;

[0050] Fig.15 A schematic diagram of a lithium-ion battery disclosed in an embodiment of the present application;

[0051] Fig.16 The cycle performance test results of the lithium-ion battery Li|Li6PS5Cl|Li disclosed in the examples of this application;

[0052] Fig.17 The test results of the cycle performance of the comparative lithium-ion battery Li|Li6PS5Cl|Li are shown;

[0053] Fig.18 Li|Li6PS5Cl 0.95 SCN 0.05 At 70℃, 0.1mA / cm 2 、0.5mAh / cm 2 Potential-cycle time curves under the following conditions;

[0054] Fig.19 Li|Li6PS5Cl 0.95 SCN 0.05 At 70℃, 0.2mA / cm 2 , 0.4mAh / cm 2 Potential-cycle time curves under the following conditions;

[0055] Fig. 20 Li|PE|Li6PS5Cl|PE|Li and Li|PE|Li6PS5Cl 0.95 SCN 0.05 |PE|Li's imaginary impedance-real impedance curve;

[0056] Fig.21 Li|PE|Li6PS5Cl|PE|Li at 0.2mA / cm 2 、1mAh / cm 2 Potential-cycle time curves under current density conditions;

[0057] Fig. 22 Li|PE|Li6PS5Cl 0.95 SCN 0.05 |PE|Li0.2mA / cm 2 、1mAh / cm 2 Potential-cycle time curves under the following conditions;

[0058] Fig.23 A flow chart of a lithium-ion battery preparation method disclosed in an embodiment of the present application;

[0059] Fig.24 This is a process flow chart of the lithium-ion battery disclosed in the embodiment of the present application. DETAILED DESCRIPTION

[0060] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.

[0061] In the following, the terms "first", "second", etc. are used only for descriptive purposes to distinguish between identical or similar items with substantially identical functions and effects, and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features.

[0062] Also, in the description of the present application, unless otherwise specified, “plurality” means two or more than two.

[0063] In addition, in this application, directional terms such as "upper", "lower", "left", "right", "horizontal" and "vertical" are defined relative to the positions of the components in the drawings. It should be understood that these directional terms are relative concepts. They are used for relative description and clarification, and they can change accordingly according to the changes in the positions of the components in the drawings. Unless otherwise clearly specified and limited, the term "connection" should be understood in a broad sense, for example: "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium.

[0064] Meanwhile, in the embodiments of the present application, words such as "exemplary" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "exemplary" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary" or "for example" is intended to present related concepts in a concrete manner for ease of understanding.

[0065] First, the concepts involved in the embodiments of the present application are explained:

[0066] Energy density refers to the amount of energy stored in a certain space or mass of material. Taking lithium-ion batteries as an example, energy density can be defined as the amount of electrical energy stored per unit mass / volume of lithium-ion batteries.

[0067] Specific capacity refers to the amount of electricity that can be discharged by a unit mass of lithium-ion battery / positive electrode / negative electrode. Specific capacity is positively correlated with energy density. Specific capacity can include surface capacity and gram capacity.

[0068] Coulombic efficiency is defined as the ratio of the discharge capacity of a lithium-ion battery to its charge capacity during the same cycle.

[0069] Lithium dendrites are dendrites of metallic lithium that are formed when lithium ions are reduced during the charging process of lithium-ion batteries.

[0070] Conductivity is defined as the ability of a substance to conduct electric current. The unit is expressed in Siemens per meter (S / m). Conductivity is an indicator for evaluating the performance of sulfide solid electrolytes / lithium-ion batteries. The greater the conductivity, the better the performance of the sulfide solid electrolyte / lithium-ion battery.

[0071] Lithium-ion batteries (lithium ion cells and batteries) are secondary batteries that use lithium-containing compounds as the positive electrode. During the charge and discharge process, the lithium ions (Li+) ionized from the positive electrode are stripped and deposited back and forth between the positive electrode and the negative electrode to achieve charge and discharge.

[0072] Room temperature, temperature is between 20℃-30℃.

[0073] See also Figure 1 The lithium-ion battery includes: a positive electrode 11, a negative electrode 12 and an electrolyte 13. The lithium-ion battery realizes charging / discharging by stripping and depositing Li+ back and forth between the positive electrode 11 and the negative electrode 12. The electrolyte 13 can be a liquid electrolyte or a solid electrolyte. The organic electrode liquid is a commonly used liquid electrolyte. The organic electrode liquid can include but is not limited to: an organic electrolyte, an electrolyte lithium salt, etc.

[0074] Please continue reading Figure 1 (a) in the figure shows a relatively mature lithium-ion battery including a ternary positive electrode material or a lithium iron phosphate (LiFePO4) positive electrode 11 | an organic electrolyte 13A | a graphite negative electrode 12. The energy density of the lithium-ion battery can reach 280Wh / kg-300Wh / kg. Among them, the ternary positive electrode material can be but is not limited to: lithium cobalt oxide (LiCoO2) lithium nickel cobalt manganese oxide (LiNi x Co y Mn 1-x-y O2).

[0075] Lithium-ion batteries using organic electrode liquid can be called organic electrode liquid system lithium-ion batteries. The energy density of existing organic electrode liquid system lithium-ion batteries has reached its limit and it is difficult to break through the bottleneck. On the one hand, the materials used in the positive electrode and the negative electrode have almost reached the limits of their respective theoretical specific capacities. On the other hand, the safety performance of lithium-ion batteries has decreased as the positive / negative electrodes use materials with high activity and high specific capacity.

[0076] With the continuous expansion of the electrochemical energy storage market and the power battery market, in order to meet the requirements of future application scenarios such as EV and energy storage for secondary battery performance, especially high energy density, the existing organic liquid system has reached a bottleneck and it is difficult to make a breakthrough.

[0077] In order to adapt to different application scenarios, the energy density of lithium-ion batteries needs to be further improved. For example: taking the application scenario of electric aircraft as an example, the energy density of lithium-ion batteries needs to reach more than 400Wh / kg. At this time, the materials used for the positive and negative electrodes can be further improved to further improve the energy density of lithium-ion batteries. Highly active substances can be used for electrodes / negative electrodes. Exemplarily, the materials used for the positive electrode (also referred to as positive electrode materials) may include but are not limited to: high nickel (Ni). The materials used for the negative electrode (also referred to as negative electrode materials) may include but are not limited to: silicon (Si), metallic lithium (Li) and other highly active materials. The use of the above materials can improve the energy density of lithium-ion batteries.

[0078] Among many highly active negative electrode materials, metallic lithium has extremely high specific capacity (the specific capacity of metallic lithium can reach 3860mAh / g) and low redox potential (the reduction potential of metallic lithium can reach -3.04Vvs). The use of metallic lithium as the negative electrode of lithium-ion batteries can greatly improve the energy density of lithium-ion batteries. However, due to the high chemical activity of metallic lithium, the application of metallic lithium as the negative electrode material in a specific lithium-ion battery system also needs to overcome many problems. For example: due to the active chemical properties of metallic lithium, side reactions are easily generated when it comes into contact with electrolytes, resulting in low coulombic efficiency of lithium-ion batteries.

[0079] Another example: Lithium-ion batteries with a metal lithium negative electrode and an organic electrolyte system have potential safety hazards, specifically:

[0080] Please continue reading Figure 1 In (a), in a lithium-ion battery using an organic electrolyte as an electrolyte, a separator 14 needs to be provided between the positive electrode 11 and the negative electrode 12. The separator 14 allows Li+ to pass through and isolates e-, thereby ensuring electrical isolation between the positive electrode 11 and the negative electrode 12.

[0081] During the charge and discharge process of the lithium-ion battery, the Li+ in the metal lithium negative electrode 12 can combine with e- to form lithium atoms. As the number of lithium atoms gradually increases, lithium dendrites will grow on the surface of the metal lithium negative electrode 12. Lithium dendrites are branch-like metal lithium. The growth of lithium dendrites will penetrate the diaphragm 14, causing the positive electrode 11 to be conductive with the metal lithium negative electrode 12, causing the lithium-ion battery to short-circuit. Therefore, lithium-ion batteries with metal lithium negative electrode / organic electrolyte systems have potential safety hazards.

[0082] In order to improve the safety performance of lithium-ion batteries, a feasible implementation method is to use a solid electrolyte electrode (SSE) instead of an organic electrolyte to form an all-solid-state lithium-ion battery.

[0083] In the subsequent embodiments, unless otherwise specified, the lithium-ion battery refers to an all-solid-state lithium-ion battery. Figure 1 (b) Figure 1 (c) and Figure 1 (d) in the figure exemplarily introduces several all-solid-state lithium-ion batteries. The all-solid-state lithium-ion battery comprises: a metal lithium negative electrode 12 and a solid electrolyte 13B. Figure 1 In (b), the material used for the positive electrode may include: LiFePO4. Figure 1 In (c), the material used for the positive electrode may include: sulfide. Figure 1 In (d), the material used for the positive electrode may include: oxide. The solid electrolyte 13B mainly includes: oxide solid electrolyte, sulfide solid electrolyte, polymer solid electrolyte and halide solid electrolyte.

[0084] Among them, sulfide solid electrolytes are solid electrolytes with high room temperature ionic conductivity, and the room temperature ionic conductivity of some sulfide solid electrolytes is even higher than that of organic liquid electrolytes. Argentite-type Li6PS5Cl and argentite-type Li7PS6 are two typical sulfide solid electrolyte materials. Li6PS5Cl and Li7PS6 involved in subsequent embodiments refer to argentite-type Li6PS5Cl and argentite-type Li7PS6 unless otherwise specified.

[0085] The crystals of Li6PS5Cl and Li7PS6 include: the space point group is Cubic crystal form. Li6PS5Cl and Li7PS6 are considered to be the two most promising sulfide solid electrolyte materials for commercialization due to their advantages of high ionic conductivity and low synthesis cost, as well as their excellent electrochemical properties.

[0086] The main problem facing sulfide solid electrolytes at this stage is that sulfide solid electrolytes are easily oxidized, and their chemical and electrochemical stability is poorer than that of oxide solid electrolytes and polymer solid electrolytes. When sulfide solid electrolytes are applied to lithium-ion batteries, the electrochemical stability window between the sulfide solid electrolyte and the metal lithium negative electrode is narrow, resulting in serious interfacial side reactions between the metal lithium negative electrode and the sulfide electrolyte during the charging and discharging process of lithium-ion batteries. The side reaction products and the generation of cracks inside the solid electrolyte will aggravate the growth of lithium dendrites, ultimately leading to an internal short circuit in the battery.

[0087] For example, see Figure 2 . Figure 2 (A) is a scanning electron microscope (SEM) image of Li6PS5Cl sulfide solid electrolyte before battery cycling. Figure 2 (a) is the SEM image of Li6PS5Cl sulfide solid electrolyte after 100h of battery cycle. Figure 2 (B) is Li6PS5Cl-Li 10 GeP2S 12 (21, 22) SEM images before battery cycling. (b) in 2 is Li6PS5Cl-Li 10 GeP2S 12 SEM image of solid electrolyte after 100h of battery cycle. Figure 2 It can be seen that after the battery cycles for a period of time, the sulfide solid electrolyte (Li6PS5Cl, Li6PS5Cl-Li 10 GeP2S 12 ) internal cracks 23 and generate by-products.

[0088] Sulfide solid electrolytes cannot fundamentally prevent the growth of lithium dendrites. The side reaction products and the generation of cracks inside the sulfide solid electrolyte will aggravate the growth of lithium dendrites. Lithium dendrites may eventually penetrate the sulfide solid electrolyte to make the positive electrode 11 and the metal lithium negative electrode 12 conductive, causing a short circuit in the lithium-ion battery. In summary, the compatibility between the sulfide solid electrolyte 13B and the metal lithium negative electrode 12 is poor.

[0089] In one example, the main method for solving the incompatibility (side reaction) problem between the sulfide solid electrolyte 13B and the metal lithium negative electrode 12 includes: compounding the sulfide solid electrolyte with an inorganic organic electrolyte. Exemplarily, an organic polymer electrolyte that is relatively stable to metal lithium can be mixed with the sulfide solid electrolyte to reduce the side reaction between the sulfide solid electrolyte and metal lithium.

[0090] Although the above method can solve the incompatibility problem between the sulfide solid electrolyte 13B and the metal lithium negative electrode 12, it will bring other new problems. For example, due to the addition of a large amount of organic polymer electrolyte, the greatest advantage of the sulfide material itself, the high room temperature ionic conductivity, is weakened. The room temperature ionic conductivity of the organic-inorganic composite material is between 10- 4 S / cm-10- 5 S / cm, low ionic conductivity will lead to excessive overpotential during battery cycling, resulting in reduced battery energy efficiency. Figure 3 , Figure 4 Take this method as an example to illustrate:

[0091] See also Figure 3 , Figure 3 (a) is a schematic diagram of the synthesis process of sulfide solid electrolyte materials; Figure 3 (b) in the figure is the molecular structure formula of Li3PS4. Figure 3(c) is the molecular structure of organic-inorganic ceramic mixed sulfide solid electrolyte material formed by Li3PS4-PEO blending, such as Figure 3 As shown in (c) in FIG. 3 , an organic-inorganic ceramic mixed sulfide solid electrolyte material 33 is formed by blending Li3PS431 with polyethylene glycol (PEO) 32.

[0092] Although, Figure 3 The sulfide solid electrolyte 33 shown is relatively stable to metallic lithium. However, there are the following problems: (1) The room temperature ionic conductivity of the sulfide solid electrolyte material is between 10- 4 S / cm-10- 5 S / cm, the room temperature ionic conductivity of sulfide solid electrolyte materials is low. The low ionic conductivity will lead to a large overpotential during the battery cycle, which will eventually reduce the energy efficiency of lithium-ion batteries. (2) Most of the components in the phase sulfide solid electrolyte material are organic polymers (PEO) and lithium salts (Li3PS4) composed of skeletons, and the safety performance of sulfide solid electrolytes is poor. (3) The sulfide solid electrolyte formed by sulfide solid electrolyte materials needs to be at a higher temperature (60°C) to be able to circulate stably.

[0093] See also Figure 4 , Figure 4 (a) is a schematic diagram of the synthesis process of sulfide solid electrolyte. Figure 4 (b) is the SEM image of PVDF-PTrFE. Figure 4 (c) in the figure is the SEM image of Li6PS5Cl. Figure 4 (d) is the SEM image of the sulfide solid electrolyte. Figure 4 (e) in the figure is the SEM image of S; the distribution of S can be seen, and the distribution of S can reflect the distribution of Li6PS5Cl in the sulfide solid electrolyte. Figure 4 (f) in the figure is the SEM image of fluorine (F); the distribution of F can be seen, and the distribution of F can reflect the distribution of PTrFE in the sulfide solid electrolyte. Figure 4 (g) in the figure is the mass-temperature relationship curve of sulfide solid electrolyte and Li6PS5Cl; it can be seen that the sulfide solid electrolyte has good thermal stability. Figure 4 (h) is the XRD pattern of PVDF-PTrFE, sulfide solid electrolyte, and Li6PS5Cl. It can be seen that the sulfide solid electrolyte contains: PVDF-PTrFE and Li6PS5Cl.

[0094] Figure 4In the method shown, a copolymer of polyvinylidene fluoride (PVDF) 41 and polytrifluoroethylene (PTrFE) 42 is spun by electrospinning to form a porous three-dimensional skeleton 43, and then Li6PS5Cl is dispersed in toluene, and Li6PS5Cl particles 44 are dispersed in the porous skeleton 43 of (PVDF-TrFE) by coating and drying to form an organic-inorganic ceramic composite sulfide solid electrolyte 45. However, Figure 4 The method shown has the following problems: (1) PVDF is used as the raw material for the synthesis of sulfide solid electrolyte 45. The decomposition of PVDF in alkaline environment may affect the battery cycle. (2) The room temperature ionic conductivity of sulfide solid electrolyte 45 is low, and the assembled battery needs to be at a higher temperature (60°C) to be able to circulate stably. (3) The electrospinning process is not suitable for the preparation of large-area films.

[0095] In another example, an organic / inorganic protective layer is added between the metallic lithium negative electrode and the sulfide solid electrolyte. By adding a protective layer between the sulfide solid electrolyte powder and the metallic lithium, the side reactions between the sulfide solid electrolyte and the metallic lithium negative electrode are blocked. Although the above method can solve the incompatibility problem between the sulfide solid electrolyte 13B and the metallic lithium negative electrode 12, it will bring other new problems, such as: the protective layer strategy has no advantage in the thickness of the solid electrolyte layer, greatly increases the process complexity in the preparation of the solid electrolyte membrane, and the material cost is also relatively high. The thickening of the solid electrolyte layer will directly lead to a decrease in the energy density of the battery. The following is an example of a method for reducing the thickness of the solid electrolyte layer. Figure 5-Figure 7 Take this method as an example to illustrate:

[0096] See also Figure 5 , Figure 5 (a) is a schematic diagram of a sulfide solid electrolyte. Figure 5 (b) is the Li|LGPS|Li battery at 0.25mA / cm 2 Time-voltage curve under current density. Figure 5 (c) is Li|LPSCl|Li at 0.25 mA / cm 2 Time-voltage curve under current density. Figure 5 (d) is Li|LPSCl-LGPS-LPSCl|Li at 0.25 mA / cm 2 Time-voltage curve under current density. Figure 5 (e) is Li|LPSCl-LGPS-LPSCl|Li at 20 mA / cm 2 Battery capacity-voltage relationship curve under current density.

[0097] The three-layer sulfide solid electrolyte material is formed by protecting the sulfide 53 in the middle with two layers of garnet-type lithium lanthanum zirconium oxide ceramic oxide material (LGPS) or lithium silicon phosphorus sulfur chloride (LSPS) material (51, 52) which is unstable to metallic lithium. Then, the surface of metallic lithium 54 is modified with a graphite layer to obtain a stable symmetrical structure.

[0098] Figure 5 The principle of the design is to use the interface between LGPS / LSPS (51, 52) and metal lithium 54. Since the overall volume of the side reaction products of LGPS / LSPS (51, 52) and metal lithium 54 is larger than the raw materials, the resulting expansion positive stress will hinder the lithium dendrites from continuing to grow and penetrate the sulfide solid electrolyte layer, thereby inhibiting the growth of lithium dendrites. Figure 5 (d) and Figure 5 By comparing (b) and (c) in Figure 5 The disclosed sulfide solid electrolyte is applied in lithium-ion batteries, and the lithium-ion batteries can have better cycle performance. Figure 5 As can be seen from (e), Figure 5 The published solution is at 20 mA / cm 2 It also has better cycling performance at a current density of 2.5 %.

[0099] Figure 5 The disadvantages of the method shown are: (1) Figure 5 The preparation and synthesis process of the disclosed sulfide solid electrolyte is complicated. (2) Figure 5 The disclosed solution is equivalent to adding a protective layer on both sides of the sulfide solid electrolyte. In addition, the presence of the protective layer will increase the complexity of the lithium-ion battery structure.

[0100] See also Figure 6 , Figure 6 (a) is the SEM image of Li6PS5Cl; Figure 6 (b) is a SEM image (top view) of the LiPON-Li6PS5Cl sulfide solid electrolyte; Figure 6 (c) is the SEM image (cross-section) of LiPON-Li6PS5Cl; Figure 6 (d) in the figure is the SEM image of S; it can be seen that the distribution of S in the sulfide solid electrolyte can reflect the distribution of Li6PS5Cl in the sulfide solid electrolyte. Figure 6 (e) in the figure is the SEM image of Cl; it can be seen that the distribution of Cl in the sulfide solid electrolyte can reflect the distribution of Li6PS5Cl in the sulfide solid electrolyte. Figure 6(f) in the figure is the SEM image of P. It can be seen that the distribution of P in the sulfide solid electrolyte can reflect the distribution of Li6PS5Cl in the sulfide solid electrolyte. Figure 6 (g) in the figure is the SEM image of O. It can be seen that the distribution of O in the sulfide solid electrolyte can reflect the distribution of LiPON in the sulfide solid electrolyte.

[0101] Figure 6 (h) in the figure is the SEM image of N. It can be seen that the distribution of N in the sulfide solid electrolyte can reflect the distribution of LiPON in the sulfide solid electrolyte.

[0102] Figure 6 (I) is a schematic diagram of a metallic lithium negative electrode and a Li6PS5Cl sulfide solid electrolyte. Figure 6 (i) is the SEM image of the metallic lithium anode and Li6PS5Cl sulfide solid electrolyte.

[0103] Figure 6 (J) is a schematic diagram of the metal lithium anode and Li6PS5Cl-LiPON sulfide solid electrolyte. Figure 6 (j) in the figure is the SEM image of the metallic lithium anode and Li6PS5Cl-LiPON sulfide solid electrolyte.

[0104] Figure 6 A layer of amorphous lithium phosphorus oxynitride (LiPON) 62 is deposited on the surface of the argyrodite particles (Li6PS5Cl) 61 by radio frequency sputtering (RF) for protection. By introducing LiPON 62, the interface resistance between the sulfide solid electrolyte (61+62) and the metal lithium 63 can be reduced to 1.3Ω / cm 2 .

[0105] Through the section Figure 6 As can be seen from (I) and (i) in FIG, the introduction of LiPON 62 on the surface of Li6PS5Cl 61 can form a more effective interface contact between metallic lithium 63 and Li6PS5Cl 61, thereby improving the wetting behavior between the surface of Li6PS5Cl61 and metallic lithium 63.

[0106] Figure 6 The problems of the method shown are as follows: (1) It is impossible to avoid the RF sputtering process to obtain nanoscale LiPON, because the room temperature ionic conductivity of LiPON itself is low (10- 6 S / cm-10- 7S / cm), the introduction of LiPON will increase the thickness of the sulfide solid electrolyte, and the increase in thickness will affect the ionic conductivity of the sulfide solid electrolyte. (2) The RF sputtering process is not suitable for mass production and is expensive.

[0107] See also Figure 7 , Figure 7 (a) in Figure 7 SEM image of the disclosed sulfide solid electrolyte.

[0108] Figure 7 (b) in Figure 7 SEM image (top view) of the disclosed sulfide solid electrolyte.

[0109] Figure 7 (c) in Figure 7 SEM image of the disclosed sulfide solid electrolyte (bottom view).

[0110] Figure 7 (d) in Figure 7 Schematic diagram of the disclosed sulfide solid-state electrolyte.

[0111] Figure 7 In the disclosed solution, a β-polyvinylidene fluoride (PVDF) protective layer 73 is added to separate the sulfide solid electrolyte 71 and the metallic lithium 72 so as to avoid the side reaction between the metallic lithium and the sulfide.

[0112] Figure 7 Problems with the method shown: (1) Figure 7 The disclosed solution adds a β-PVDF protective layer 73. The presence of the protective layer will have a certain impact on the chemical and electrochemical stability between the sulfide and the metallic lithium. (2) Adding the protective layer 73 will increase the complexity of the system and the complexity of the preparation process. In addition, adding the protective layer 73 is not conducive to analyzing the performance of the battery.

[0113] Above Figure 3 and Figure 4 The method shown reduces the side reaction between sulfide and metallic lithium by adding a large amount of organic polymer. Due to the addition of a large amount of organic polymer to the electrolyte, the greatest advantage of the sulfide material itself, the high room temperature ionic conductivity, is weakened. Figure 5 , Figure 6 and Figure 7 In the disclosed solution, a protective layer is added between the sulfide solid electrolyte and the metal lithium (lithium electrode). The introduction of the protective layer will increase the size of the lithium-ion battery, directly leading to a decrease in the battery energy density. In addition, the introduction of the protective layer will increase the structural complexity of the lithium-ion battery system and the complexity of the preparation process.

[0114] In order to solve the technical problems existing in the above method, the embodiment of the present application discloses a doped sulfide material, the crystal of the sulfide material includes: the space point group is Cubic crystal form; at least one site in the unit cell constituting the crystal is doped with a doping group, and the doping group includes: nitrogen element (N).

[0115] The sulfide-doped crystal disclosed in the embodiment of the present application includes: the space point group is The cubic crystal form of the doped sulfide has a high ionic conductivity. In addition, at least one site in the unit cell of the doped sulfide material is doped with a doping group containing N, and N can combine with Li to form a Li3N solid electrolyte interface. The presence of Li3N can hinder the side reaction between the doped sulfide material and metallic lithium to a certain extent. Therefore, the doped sulfide material disclosed in the embodiment of the present application has better stability to metallic lithium.

[0116] In the subsequent embodiments, the crystals involved refer to crystals doped with sulfide materials unless otherwise specified. The unit cells involved refer to unit cells doped with sulfide materials unless otherwise specified. The conductivity involved refers to electronic conductivity unless otherwise specified.

[0117] In the application examples themselves, there is no specific limitation on the types of doping groups, and any group containing N and that can be doped into the unit cell of the sulfide material can be used as a doping group in the application examples.

[0118] Exemplary, doping groups may include, but are not limited to: thiocyanate ions (SCN - ), cyanide ion (CN - ) at least one of.

[0119] Considering that the larger the unit cell volume of the doped sulfide material, the lower the capacity decay during the shuttling of ions in the unit cell, and accordingly, the greater the ionic conductivity of the doped sulfide material.

[0120] In order to further improve the ionic conductivity of the doped sulfide material, as a feasible implementation method, the volume of the doping group is larger than the volume of the S ion. The doping group with a volume larger than the S ion may include but is not limited to: SCN - , CN - In the embodiment of the present application, the doping group whose volume is larger than that of the S ion may also be referred to as a large-volume doping group.

[0121] In this implementation, the volume of the doping group is larger than the volume of the S ion. The introduction of a large-volume doping group can expand the unit cell volume, and the ion channel in the unit cell has a larger size, which can alleviate the capacity decay during the transmission of ions in the unit cell. The doped sulfide material disclosed in this implementation has a larger ionic conductivity. In addition, the introduction of a large-volume doping group can improve the mechanical properties of the doped sulfide material, reduce the Young's modulus of the doped sulfide material, soften the doped sulfide material, and improve the processability of the doped sulfide material.

[0122] In the embodiment of the present application, the doping amount of the doping group can be defined as the molar ratio of the doping group to the halogen element binding site.

[0123] Considering that the introduction of doping groups will affect the crystal form of doped sulfide materials, when the doping amount of the doping groups is greater than a certain range, the introduction of the doping groups causes the crystal of the doped sulfide materials to deviate from the space point group The cubic crystal form reduces the conductivity of the doped sulfide material.

[0124] In order to ensure that the doped sulfide material has a high conductivity, as a feasible implementation, the doping amount of the doping group is less than 20%. In this implementation, the doping amount of the doping group in the heterosulfide material is less than 20%, which can achieve high conductivity performance of the doped sulfide material.

[0125] It is considered that the introduction of doping groups will improve the stability of the doped sulfide material to metallic lithium, and within a certain range, the greater the doping amount of the doped sulfide material, the better the stability of the doped sulfide material to metallic lithium.

[0126] In order to ensure that the doped sulfide material has a higher stability to metallic lithium, as a feasible implementation, the doping amount of the doping group in the doped sulfide material is greater than or equal to 0.01%. In this implementation, the doping amount of the doping group in the doped sulfide material is greater than or equal to 0.01%, and the doped sulfide material has better stability to metallic lithium.

[0127] In order to take into account the better stability (towards metallic lithium) and high conductivity of the doped sulfide material, as a feasible implementation method, the doping amount of the doping group in the doped sulfide material is 0.01%-20%. Exemplarily, the doping amount of the doping group in the doped sulfide material can be: 0.5%, 1%, 2%, etc.

[0128] In some possible implementations, the chemical formula of the doped sulfide material includes: Li 7-n2 PS 6-n X n2 , where X is a doping group. The chemical formula includes: Li 7-n2 PS6-n X n2 The doped sulfide material has the advantages of high ionic conductivity and low synthesis cost.

[0129] Considering that the introduction of the doping group will improve the stability of the doped sulfide material against metallic lithium, as a feasible implementation method, as a feasible implementation method, Li 7-n2 PS 6-n X n2 In it, 0 < n2, so that the doped sulfide material contains N. When the doped sulfide material contacts metallic lithium, N in the doped sulfide material can form Li3N with metallic lithium, and Li3N can hinder the side reaction between the doped sulfide material and metallic lithium, making the doped sulfide material have better stability against metallic lithium.

[0130] Considering that the introduction of the doping group will affect the crystal form of the doped sulfide material, in order to ensure that the doped sulfide material has high conductivity performance, as a feasible implementation method, Li 7-n2 PS 6-n X n2 In it, n2 ≤ 0.2, so that the doped sulfide material has high conductivity performance.

[0131] In order to take into account the better stability performance (against metallic lithium) and high conductivity performance of the doped sulfide material, as a feasible implementation method Li 7-n2 PS 6-n X n2 In it, 0 < n2 ≤ 0.5.

[0132] In some feasible implementation methods, the chemical formula of the sulfide material includes: Li6PS5Cl 1-n1 X n1 , where X is the doping group. The chemical formula includes Li6PS5Cl 1-n1 X n1 The doped sulfide material has the advantages of high ionic conductivity and low synthesis cost.

[0133] Considering that the introduction of the doping group will improve the stability of the doped sulfide material against metallic lithium, as a feasible implementation method, Li6PS5Cl 1-n1 X n1 In it, 0 < n1, so that the doped sulfide material contains N. When the doped sulfide material contacts metallic lithium, N in the doped sulfide material can form Li3N with metallic lithium, and Li3N can hinder the side reaction between the doped sulfide material and metallic lithium, making Li6PS5Cl 1-n1 X n1 have better stability against metallic lithium.

[0134] Considering that the introduction of doping groups will affect the crystal form of doped sulfide materials, in order to ensure that the doped sulfide materials have high conductivity, as a feasible implementation method, Li6PS5Cl 1-n1 X n1 Here n1≤0.2, which makes the doped sulfide material have high electrical conductivity performance.

[0135] In order to take into account the better stability (towards metallic lithium) and high conductivity of doped sulfide materials, Li6PS5Cl is used as a feasible method. 1-n1 X n1 Middle 0 <n1≤0.2。

[0136] In conjunction with the specific drawings, the doping group is thiocyanate ion (SCN - ) as an example, the doped sulfide material (Li6PS5Cl 1-n1 (SCN) n1 ) for further explanation:

[0137] See also Figure 8 , Figure 8 Li6PS5Cl 1-n1 (SCN) n1 Schematic diagram of the unit cell. Li6PS5Cl 1-n1 (SCN) n1 The space point group of Cubic crystal form. Li6PS5Cl 1-n1 (SCN) n1 The ions may include: P ions 81, S ions 82, Li ions 83, chloride (Cl) ions 84, thiocyanate ions (SCN - ) 85. It can be seen that the P ion 81 in the unit cell is in the regular tetrahedral space composed of the S ions 82. The P ion 81 and the four S ions 82 form a PS4 tetrahedron 86, and the PS4 tetrahedron occupies the edge center. The Li ion 83 and the three planar S ions 82 form a planar triangle configuration, the Cl ion 84 and the doped SCN ion 85 occupy the unit cell vertices (Cl binding sites), and the PS4 tetrahedron 86 occupies the edge center.

[0138] Li6PS5Cl 1-n1 (SCN) n1 SCN is included - Li6PS5Cl 1-n1 (SCN) n1 When in contact with Li, SCN- can combine with Li to form Li3N. The presence of Li3N can hinder the side reaction between doped sulfide materials and Li to a certain extent. Therefore, Li6PS5Cl 1-n1 (SCN) n1It has better stability to Li.

[0139] In addition, SCN - The volume of SCN is larger than that of undoped sulfide materials. - The introduction of can expand Li6PS5Cl 1-n1 (SCN) n1 Unit cell volume, relieving ions in Li6PS5Cl 1-n1 (SCN) n1 The capacity decay during the transmission process in the unit cell makes Li6PS5Cl 1-n1 (SCN) n1 It has a large ionic conductivity.

[0140] The doped sulfide material (Li6PS5Cl) disclosed in the embodiment of the present application is described below in conjunction with the specific drawings. 1-n1 SCN n1 ) are used to illustrate the structural characterization results:

[0141] (1) In terms of crystal form, the introduction of doping groups did not change the original crystal form.

[0142] See also Fig. 9 , shows the XDR of doped sulfide materials and undoped sulfide materials at different doping levels. For example, Fig. 9 (a) is Li6PS5Cl 0.99 (SCN) 0.01 XRD pattern of . Fig. 9 (b) is Li6PS5Cl 0.95 (SCN) 0.05 XRD pattern of Fig. 9 (c) is Li6PS5Cl 0.9 (SCN) 0.1 XRD pattern of Fig. 9 (d) in the figure is the XRD pattern of the sulfide material Li6PS5Cl without SCN doping. Fig. 9 91 in the middle is the standard caliper.

[0143] pass Fig. 9 (a), (b), and (c) are respectively Fig. 9 (d) in comparison, Li6PS5Cl 0.99 (SCN) 0.01 、Li6PS5Cl 0.95 (SCN) 0.05 、Li6PS5Cl 0.9 (SCN) 0.1 The XRD curve of Li6PS5Cl almost overlaps with that of Li6PS5Cl. 0.99 (SCN)0.01 The crystal form of Li6PS5Cl is similar to that of Li6PS5Cl, and the original crystal form has not changed. The known crystals of Li6PS5Cl include: It is known that Li6PS5Cl 0.99 (SCN) 0.01 、Li6PS5Cl 0.95 (SCN) 0.05 、Li6PS5Cl 0.9 (SCN) 0.1 Includes: The space point group is Cubic crystal form, Li6PS5Cl 0.99 (SCN) 0.01 Has a higher electrical conductivity.

[0144] (2) In terms of lattice parameters, SCN - Doping can expand the unit cell volume:

[0145] See also Fig.10 , Fig.10 Li6PS5Cl 1-n1 SCN n1 And the lattice parameter diagram of Li6PS5Cl. The lattice parameter can characterize the size of the unit cell.

[0146] Fig.10 The vertical axis in is the lattice parameter. Fig.10 The horizontal axis is Li6PS5Cl 1-n1 SCN n1 SCN - The 0 in the horizontal axis corresponds to Li6PS5Cl(SCN - The doping amount is 0%); 1 in the abscissa corresponds to Li6PS5Cl 0.99 (SCN) 0.01 (SCN - The doping amount is 1%); the 5 in the horizontal axis corresponds to Li6PS5Cl 0.95 (SCN) 0.05 (SCN - The doping amount is 5%); 10 in the abscissa corresponds to Li6PS5Cl 0.9 (SCN) 0.1 (SCN - The doping amount is 10%).

[0147] from Fig.10 By comparing the data with abscissa 1, 5, 10 and 0, we can see that: Li6PS5Cl 0.99 (SCN) 0.01、Li6PS5Cl 0.95 (SCN) 0.05 、Li6PS5Cl 0.9 (SCN) 0.1 The lattice parameter of SCN is greater than 9.825 (the lattice parameter of Li6PS5Cl). - The doping can expand the unit cell volume, so that the unit cell has a larger ion transmission channel, which can alleviate the capacity decay during the ion transmission process in the unit cell, making Li6PS5Cl 0.99 (SCN) 0.01 、Li6PS5Cl 0.95 (SCN) 0.05 、Li6PS5Cl 0.9 (SCN) 0.1 It has a large ionic conductivity.

[0148] (3) The grain (crystal) size of the doped sulfide material (Li6PS5Cl 1-n1 SCN n1 ) are used to illustrate the characterization results:

[0149] See also Fig.11 , Fig.11 Li6PS5Cl 1-n1 SCN n1 and crystal size diagram of Li6PS5Cl. Fig.11 The ordinate in the graph is the crystal size. Fig.11 The horizontal axis is Li6PS5Cl 1-n1 SCN n1 SCN - For details, please refer to Fig.10 The description of the horizontal axis will not be repeated here.

[0150] from Fig.11 In the figure, the data with abscissa 1, 5, 10 and 0 show that: Li6PS5Cl 0.99 (SCN) 0.01 、Li6PS5Cl 0.95 (SCN) 0.05 、Li6PS5Cl 0.9 (SCN) 0.1 It has similar crystal size to Li6PS5Cl.

[0151] The performance of the doped sulfide material disclosed in the embodiments of the present application is described below in combination with specific experimental data:

[0152] (1) The impedance of the doped sulfide material (Li6PS5Cl) of the present application embodiment is compared 1-n1 SCN n1 ) is used to illustrate the performance:

[0153] See also Fig.12 , Fig.12 Li6PS5Cl 1-n1 SCN n1 The impedance curves of Li6PS5Cl and Li6PS5Cl. The impedance includes real impedance and imaginary impedance. The ordinate in 12 is the imaginary impedance. Fig.12 The ordinate in is the real impedance.

[0154] Fig.12 In the figure, curve a is the imaginary impedance-real impedance curve of Li6PS5Cl.

[0155] Curve b is Li6PS5Cl 0.99 (SCN) 0.01 The imaginary impedance-real impedance curve.

[0156] Curve c is Li6PS5Cl 0.95 (SCN) 0.05 The imaginary impedance-real impedance curve.

[0157] Curve d is Li6PS5Cl 0.9 (SCN) 0.1 The imaginary impedance-real impedance curve.

[0158] Curve e is Li6PS5Cl 0.8 (SCN) 0.2 The imaginary impedance-real impedance curve.

[0159] from Fig.12 In the figure, curve a and curve b are compared to show that Li6PS5Cl 0.99 (SCN) 0.01 The impedance is similar to that of Li6PS5Cl.

[0160] from Fig.12 In the figure, the data of curve a and curve c are compared to show that Li6PS5Cl 0.95 (SCN) 0.05 The impedance is similar to that of Li6PS5Cl.

[0161] from Fig.12 In the figure, the data of curve a and curve d are compared to show that Li6PS5Cl 0.9 (SCN) 0.1 The impedance is similar to that of Li6PS5Cl.

[0162] from Fig.12In the figure, the data of curve a and curve e are compared to show that Li6PS5Cl 0.8 (SCN) 0.2 The impedance deviates significantly from that of Li6PS5Cl.

[0163] The above impedance test results show that SCN - The doping amount of Li6PS5Cl is between 0.01% and 0.10%. 1-n1 SCN n1 It has similar impedance to Li6PS5Cl. - The doping amount is 0.01%-0.10%, SCN - Doping of Li6PS5Cl 1- n1 SCN n1 The impedance of SCN is less affected. - The doping amount of Li6PS5Cl is between 1% and 10%. 1-n1 SCN n1 Can have higher ionic conductivity. SCN - The doping amount of Li6PS5Cl reaches 20%, 1-n1 SCN n1 The impedance changes significantly.

[0164] See also Fig.13 , Fig.13 Li6PS5Cl 1-n1 SCN n1 Schematic diagram of the electrical conductivity of Li6PS5Cl. Fig.13 The vertical coordinate is Li6PS5Cl 1-n1 SCN n1 Or the conductivity of Li6PS5Cl. Fig.13 The horizontal axis is Li6PS5Cl 1-n1 SCN n1 SCN - For details, please refer to Fig.10 The description of the horizontal axis is not repeated here. The 20 in the horizontal axis corresponds to Li6PS5Cl 0.8 (SCN) 0.2 (SCN - The doping amount is 20%).

[0165] from Fig.13 In the figure, the data with the horizontal axis of 1 shows that Li6PS5Cl 0.99 (SCN) 0.01 The conductivity can reach 0.75mS / cm. The data with the horizontal axis of 5 shows that Li6PS5Cl 0.95 (SCN) 0.05The conductivity can reach 0.8mS / cm. The data with the horizontal axis of 10 shows that Li6PS5Cl 0.9 (SCN) 0.1 The conductivity can reach 0.9mS / cm. The data with the horizontal axis of 20 shows that Li6PS5Cl 0.8 (SCN) 0.2 The conductivity is only 0.3mS / cm.

[0166] The above conductivity test results show that: SCN - The doping amount of Li6PS5Cl is between 0.01% and 0.10%. 1-n1 SCN n1 The conductivity of SCN can reach more than 0.75mS / cm. - The doping amount of Li6PS5Cl is between 0.01% and 0.10%. 1-n1 SCN n1 The conductivity can be maintained above 0.75mS / cm. - The doping amount of Li6PS5Cl reaches 20%, 1-n1 SCN n1 The conductivity decreased significantly.

[0167] Among the currently disclosed sulfide solid electrolyte materials, the conductivity is 1*10 -4 mS / cm-1*10 -2 mS / cm. The electrical conductivity of the doped sulfide material disclosed in the embodiment of the present application can be maintained above 0.75mS / cm. The electrical conductivity of the doped sulfide material disclosed in the embodiment of the present application is at a relatively high value. In addition, there are doping groups in the unit cell of the doped sulfide material disclosed in the embodiment of the present application, and the N of the doping group can combine with Li to form Li3N. The presence of Li3N can hinder the side reaction of the doped sulfide material with metallic lithium to a certain extent. Therefore, the doped sulfide material disclosed in the embodiment of the present application has better stability to metallic lithium.

[0168] The present application also discloses a method for preparing a doped sulfide material. Fig.14 ; The preparation method of the sulfide material may include: S141-S142:

[0169] S141. Mix raw materials.

[0170] In the embodiment of the present application, the raw materials may include: a first raw material and a second raw material. The first raw material includes: a raw material that can form a sulfide solid electrolyte. The second raw material includes: a raw material that can provide a doping group. Among them, the sulfide solid electrolyte may include but is not limited to: Li6PS5Cl and Li7PS6.

[0171] In one example, the first raw material may include: lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5). In another example, the first raw material may include: Li2S, P2S5 and lithium chloride (LiCl). It is worth noting that the embodiments of the present application are only exemplary introductions of two first raw materials, and the above first raw materials do not constitute a specific limitation.

[0172] As a feasible implementation method, the first raw material may be dried. The embodiment of the present application does not specifically limit the drying method of the first raw material, and a drying method commonly used in the art may be adopted, such as vacuum drying.

[0173] The embodiments of the present application do not specifically limit the second raw material, and any raw material that can provide a doping group can be used as the second raw material in the embodiments of the present application.

[0174] As a feasible implementation, the second raw material may include: a lithium salt formed by lithium ions and doping groups. Exemplarily, the second raw material may include: lithium thiocyanate (LiSCN) or lithium cyanide (LiCN).

[0175] It is worth noting that the embodiments of this application are only exemplary introductions of two Li + The lithium salt formed with the doping group. The above lithium salt does not constitute a specific limitation.

[0176] In this implementation, Li + The lithium salt formed with the doping group is used as the second raw material, so that no additional interfering substances are introduced during the preparation of the doped sulfide material, and the step of removing the interfering substances can be omitted, which simplifies the preparation process of the doped sulfide material to a certain extent.

[0177] Typically, lithium salts contain water of crystallization. For example, taking lithium thiocyanate (LiSCN) as an example, lithium thiocyanate usually exists in the form of LiSCN·xH2O, where xH2O is water of crystallization. The presence of water of crystallization will affect the crystallization process of subsequent doped sulfide materials. In order to avoid the influence of water of crystallization contained in lithium salts on the crystallization of subsequent doped sulfide materials, it is necessary to remove the water of crystallization in the lithium salt in advance. The embodiment of the present application also discloses a method for removing water of crystallization in lithium salts. For details, please continue to refer to Fig.14 If the raw material contains lithium salt, before S141, the preparation method further includes:

[0178] SA: The lithium salt is heated to a first temperature for drying, wherein the first temperature is greater than the melting point of the lithium salt and is less than the temperature at which water decomposes.

[0179] SA can also be understood as the first drying, specifically: the lithium salt is heated to a first temperature (the first temperature is greater than the melting point of the lithium salt) in advance to melt the lithium salt, and the crystal water in the lithium salt escapes from the lithium salt in the form of water vapor. During the first drying process, most of the crystal water in the lithium salt is removed.

[0180] The embodiment of the present application does not specifically limit the value of the first temperature. It is necessary to ensure that the first temperature is greater than the melting point of the lithium salt, so that the lithium salt is in a melting state at the first temperature, so that the crystal water inside the lithium salt can be released. The first temperature is lower than the decomposition temperature of water, so that the released crystal water exists in the form of water molecules, avoiding the introduction of interfering substances (Li2O) during the first drying process. The interfering substances can be: the reaction products of the decomposition products (O2) of water molecules and Li+ in the lithium salt.

[0181] Exemplarily, the first temperature may be: 130°C, 140°C, 150°C, 160°C.

[0182] SB: The dried lithium salt is heated to a second temperature for drying.

[0183] SB can also be understood as the second drying, and the temperature of the second drying is the second temperature. The second temperature is higher than the first temperature, and the lithium salt after the first drying is heated to the second temperature (the second temperature is higher than the first temperature). The lithium salt after the first drying is heated to the second temperature, which can accelerate the release of crystal water in the lithium salt.

[0184] As a feasible implementation method, the second temperature can be higher than the decomposition temperature of water. Since most of the crystalline water in the lithium salt has been released during the first drying process, even if the second temperature is higher than the decomposition temperature of water, more O2 will not be produced.

[0185] As a feasible implementation method, the second temperature may be lower than the decomposition temperature of water, so that water exists in the form of water molecules at the second temperature, thereby avoiding the introduction of interfering substances during the second drying process.

[0186] Illustratively, the second temperature may be 180° C., 190° C., 200° C., etc.

[0187] The following is a specific example, taking lithium salt LiSCN·xH2O as an example to further illustrate the method for removing crystal water disclosed in the embodiment of the present application.

[0188] Place LiSCN·xH2O in a vacuum oven, maintain the vacuum oven at 100 mBar, heat to 150°C to melt LiSCN·xH2O, heat at a rate of 25°C / h, maintain 150°C temperature and dry for 24h; then heat to 200°C, heat at a rate of 25°C / h, dry for 20h, and obtain dried LiSCN white powder as a reaction precursor raw material (second raw material).

[0189] The embodiment of the present application does not specifically limit the mixing method of the first raw material and the second raw material. For example, the first raw material and the second raw material can be mixed by ball milling and extrusion.

[0190] In a feasible embodiment, Li2S, P2S5, LiCl and dried LiSCN white powder in a certain stoichiometric ratio can be uniformly mixed in an inert gas atmosphere, and then ball milled at 600 rpm for 20 hours to obtain a uniform doped sulfide material.

[0191] It is worth noting that the above embodiment is only an exemplary introduction of the ball milling speed and ball milling time in a ball milling extrusion process. In the actual application process, the speed and ball milling time can be adjusted according to the needs, and the applicant does not make too many restrictions here.

[0192] For example, in some feasible implementations, the ball milling speed can be appropriately increased to reduce the ball milling time. For example, in some feasible implementations, the ball milling time can be appropriately extended to reduce the ball milling speed.

[0193] S142: Crystallize the mixed raw materials to obtain a doped sulfide material.

[0194] Among them, the crystals of sulfide materials include: the space point group is A cubic crystal form; at least one site in the unit cell constituting the crystal is doped with a doping group, and the doping group includes an N element.

[0195] The embodiment of the present application does not specifically limit the crystallization location of the raw material. As a feasible implementation method, the raw material can be crystallized in a muffle furnace.

[0196] For example, the mixed raw materials can be transferred to a muffle furnace and placed in a crystallization temperature of 400° C.-500° C. for a crystallization time of 15 hours to obtain a pure phase and high crystallinity doped sulfide material.

[0197] As a feasible implementation method, in order to facilitate the transfer of raw materials, the raw materials obtained by ball milling can be pressed into a powder cake under an axial pressure of 2 tons for 5 minutes in an inert gas atmosphere, and then the powder cake can be transferred to a muffle furnace for crystallization.

[0198] It is worth noting that the above embodiment is only an exemplary introduction of a crystallization time and a crystallization temperature. In the actual application process, the crystallization time and crystallization temperature can be determined according to the requirements, and the applicant does not make too many restrictions here.

[0199] For example, in some feasible implementations, the crystallization time can be appropriately extended and the crystallization temperature can be lowered. For example, in some feasible implementations, the crystallization temperature can be appropriately increased and the crystallization time can be shortened.

[0200] The method for preparing a doped sulfide material disclosed in the embodiment of the present application, wherein the crystal of the prepared sulfide material comprises: The cubic crystal form of the doped sulfide has a higher ionic conductivity. In addition, at least one site in the unit cell of the doped sulfide material is doped with a doping group containing N. N can combine with Li to form Li3N. The presence of Li3N can hinder the side reaction of the doped sulfide material with metallic lithium to a certain extent. Therefore, the doped sulfide material prepared in the embodiment of the present application has better stability to metallic lithium.

[0201] The present application also discloses a lithium-ion battery, which may include: a lithium-ion battery and an all-solid-state lithium-sulfur battery. Fig.15 The lithium-ion battery includes: a metallic lithium negative electrode 1, a sulfide solid electrolyte 2 and a positive electrode 3; the sulfide solid electrolyte is arranged between the metallic lithium and the positive electrode, and the material used for the sulfide solid electrolyte includes: the doped sulfide material disclosed in the embodiment of the present application.

[0202] The lithium-ion battery disclosed in the embodiment of the present application uses a metal lithium negative electrode. The material used for the metal lithium negative electrode includes: metal lithium. Since metal lithium has an extremely high specific capacity (3860mAh / g) and a low redox potential (-3.04V vs standard hydrogen potential), the metal lithium negative electrode can greatly improve the energy density of the lithium-ion battery.

[0203] The lithium-ion battery uses the doped sulfide disclosed in the embodiment of the present application as the material of the sulfide solid electrolyte. The crystals doped with sulfide include: The cubic crystal form, the doped sulfide has higher ion conductivity, the sulfide solid electrolyte has higher conductivity, and the lithium ion battery including the sulfide solid electrolyte can have higher energy density.

[0204] At least one site in the unit cell of the doped sulfide material is doped with a doping group containing N. N can combine with Li in the metal lithium negative electrode to form Li3N, which can hinder the side reaction between the sulfide solid electrolyte and the metal lithium negative electrode to a certain extent, and inhibit the growth of lithium dendrites on the surface of the metal lithium negative electrode, so that the lithium ion battery disclosed in the embodiment of the present application has a longer cycle life and higher safety.

[0205] Li3N can stabilize the interface between the metal lithium anode and the sulfide solid electrolyte, making the lithium-ion battery charge and discharge: Li + It can be uniformly deposited or stripped, so that the lithium-ion battery disclosed in the embodiment of the present application has good stability.

[0206] In summary, the lithium-ion battery disclosed in the embodiments of the present application has the characteristics of high energy density, high safety, long cycle life (also referred to as cycle performance), high stability performance, etc., and can meet the requirements of future EV, energy storage and other application scenarios for lithium-ion batteries with continuously improving performance.

[0207] In some feasible implementations, a large volume doping group can be doped into the doped sulfide material. In this implementation, the doped sulfide material used in the sulfide solid electrolyte is doped with a large volume doping group. The large volume doping group can expand the unit cell parameters without changing the crystal form, so that the sulfide solid electrolyte has a larger Li + Transmission window, improving Li+ in sulfide solid electrolytes + The lithium-ion battery disclosed in this implementation also solves the problem of polysulfide (LiS x ) Shuttle traffic leads to a bottleneck problem with serious capacity decay.

[0208] The present application does not specifically limit the material used for the positive electrode of the lithium-ion battery. Any material with conductive properties can be used as a positive electrode material (positive electrode material) in the present application. For example, the positive electrode material can include but is not limited to: metallic lithium, metallic tungsten (W), metallic copper (Cu), etc.

[0209] In order to increase the Li + As a feasible implementation method, the positive electrode material may include: positive electrode material and the doped sulfide material disclosed in the embodiment of the present application. - The role of transport, doping sulfide materials is Li + Further, the doped sulfide material is added with a bulky doping group, and the bulky doping group can make the positive electrode have a larger Li + Transfer window.

[0210] As a feasible implementation method, the materials used for the positive electrode may include: positive electrode material, conductive carbon and the doped sulfide material disclosed in the embodiment of the present application. Among them, the conductive carbon has a porous structure, so that the positive electrode and Li + The contact area is larger, Li + It can be evenly deposited or stripped on the surface of the positive electrode, thereby improving the stability of the lithium-ion battery.

[0211] As a feasible implementation method, the materials used for the positive electrode may include: 10%-30% by weight of doped sulfide material, 65%-80% by weight of positive electrode material, and 2%-5% by weight of conductive carbon.

[0212] As a feasible implementation method, the materials used for the positive electrode may include: a positive electrode material, a binder and a doped sulfide material disclosed in the embodiments of the present application. The binder increases the adhesion between the positive electrode material and the doped sulfide material, so that the mechanical strength of the positive electrode is improved. Among them, the binder may include but is not limited to: polytetrafluoroethylene (PTFE).

[0213] As a feasible implementation method, the materials used for the positive electrode may include: 10%-30% by weight of doped sulfide material, 68%-80% by weight of positive electrode material, and 0.5%-3% by weight of PTFE.

[0214] The performance of the lithium-ion battery disclosed in the embodiment of the present application is described below in combination with specific experimental data:

[0215] (1) In terms of cycle performance, the performance of lithium-ion batteries using doped sulfide materials has been greatly improved:

[0216] See also Fig.16 and Fig.17 , Fig.16 (a) is a lithium-ion battery Li|Li6PS5Cl|Li without using the doped sulfide material provided by the present application Fig.16 (a) is the lithium-ion battery Li|Li6PS5Cl|Li at room temperature and 0.1mA / cm 2 , 0.2mAh / cm 2 Cyclic performance test results. Fig.16 (b) is the lithium-ion battery Li|Li6PS5Cl|Li at room temperature and 0.1mA / cm 2 , 0.2mAh / cm 2 Potential-cycle time curves.

[0217] Fig.17 A lithium-ion battery Li|Li6PS5Cl using the doped sulfide material provided by the present application0.95 SCN 0.05 |Li at room temperature, 0.1mA / cm 2 , 0.2mA / cm 2 Potential-cycle time curves at different current densities.

[0218] from Fig.16 (a) and Fig.16 As can be seen from (b), the Li|Li6PS5Cl|Li of the lithium-ion battery with sulfide solid electrolyte using Li6PS5Cl is 0.1mA / cm 2 、0.2mAh / cm 2 Under the condition of Li|Li6PS5Cl|Li cycle, the potential changed significantly after 20h of cycling. It can be seen that the Li|Li6PS5Cl|Li short circuit phenomenon occurred within 20h of Li|Li6PS5Cl|Li cycle.

[0219] from Fig.17 It can be seen that Li|Li6PS5Cl 0.95 SCN 0.05 |Li at room temperature, 0.1mA / cm 2 、0.2mAh / cm 2 Under these conditions, it can cycle stably for 500 hours, and the battery overpotential is stable at around 40mV.

[0220] Li|Li6PS5Cl 0.95 SCN 0.05 | SCN doped in Li-sulfide solid electrolyte - The interfacial stability between the sulfide solid electrolyte and the metallic lithium anode can be significantly enhanced, making the deposition and stripping of lithium more uniform during the cycle. 0.95 SCN 0.05 |The overpotential of Li can be stabilized at about 40mV. In addition, SCN - The N in the negative electrode can form Li3N with the Li in the metal lithium anode. Li3N can effectively inhibit the growth of lithium dendrites, making Li6PS5Cl 0.95 SCN 0.05 Able to cycle stably for 500h.

[0221] See also Fig.18 , Fig.18 Li|Li6PS5Cl 0.95 SCN 0.05 At 70°C, 0.1 mA / cm 2 、0.5mAh / cm 2 The potential-cycle time curve under the conditions. It can be seen that Li|Li6PS5Cl 0.95 SCN 0.05|Li can be stably cycled for 1400h at 70℃ with an overpotential between 13mV and 130mV.

[0222] See also Fig.19 , Fig.19 Li|Li6PS5Cl 0.95 SCN 0.05 At 70℃, 0.2mA / cm 2 , 0.4mAh / cm 2 The potential-cycle time curve under the conditions. It can be seen that Li|Li6PS5Cl 0.95 SCN 0.05 At 70℃, 0.2mA / cm 2 , 0.4mAh / cm 2 Under the same conditions, the overpotential can be stably cycled between 13mV-130mV for 300h.

[0223] See also Fig. 20 , Fig. 20 Curve a in the figure is the imaginary impedance-real impedance curve of Li|PE|Li6PS5Cl|PE|Li; Curve b is the imaginary impedance-real impedance curve of Li|PE|Li6PS5Cl 0.95 SCN 0.05 |PE|Li's imaginary impedance-real impedance curve. It can be seen that Li|PE|Li6PS5Cl 0.95 SCN 0.05 |PE|Li has smaller interface impedance.

[0224] See also Fig.21 and Fig. 22 , Fig.21 (a) is Li|PE|Li6PS5Cl|PE|Li at 0.2mA / cm 2 、1mAh / cm 2 Potential-cycle time curves under different conditions. Fig.21 (b) is a partial enlarged view of region A. The overpotential is -0.3V-0.2V after 800 cycles.

[0225] Fig. 22 (a) is Li|PE|Li6PS5Cl 0.95 SCN 0.05 |PE|Li at 0.2mA / cm 2 、1mAh / cm 2 Potential-cycle time curves under . Fig. 22 (b) is a partial enlarged view of area B. Before 800h, the overpotential was (-0.15V-0.15V). After 1000h, the overpotential was

[0226] Fig.21 and Fig. 22 It can be seen that Li|PE|Li6PS5Cl 0.95 SCN 0.05 |PE|Li has a more stable overpotential during the cycle. It can be inferred that Li6PS5Cl 0.95 SCN 0.05 The electrochemical stability of lithium metal is high, making Li|PE|Li6PS5Cl 0.95 SCN 0.05 |PE|L The deposition / stripping of Li during charge and discharge is more stable.

[0227] The performance of the lithium-ion battery disclosed in the embodiments of the present application is further described below in conjunction with specific embodiments 1 to 6.

[0228] The performance parameters of the lithium-ion batteries disclosed in Examples 1 to 6 and the lithium-ion batteries disclosed in the comparative examples are shown in Table 1:

[0229] The lithium-ion battery disclosed in the comparative example has a similar structure to the lithium-ion battery disclosed in Examples 1 to 6, except that the sulfide solid electrolyte in the lithium-ion battery uses a different material. See Table 1 for details:

[0230] Table 1

[0231]

[0232] It is worth noting that, in addition to the comparative examples disclosed in Table 1, the related art also discloses some lithium-ion batteries using sulfide solid electrolytes.

[0233] Among the currently disclosed sulfide solid electrolyte materials, the conductivity is 1*10 -4 mS / cm-1*10 -2 The conductivity of the lithium-ion battery disclosed in the embodiment of the present application can be maintained above 0.54 mS / cm. The conductivity of the lithium-ion battery disclosed in the embodiment of the present application is at a relatively high value.

[0234] The lithium-ion batteries disclosed in the related art need to be tested for cycle performance at high temperatures, while the lithium-ion batteries disclosed in Examples 1, 2, 4, 5, and 6 can be stably cycled at room temperature.

[0235] Most of the lithium-ion batteries disclosed so far can stably cycle for 2h-3000h. The lithium-ion battery disclosed in Example 6 has a capacity of 0.2mAh / cm 2 Under the current density, it can stably cycle for more than 1800 hours. The cycle time of the lithium-ion battery disclosed in the embodiment of the present application is at a relatively high value.

[0236] The lithium-ion battery disclosed in Example 3 is subjected to a relatively harsh environment (0.2 mA / cm 2 , 0.4mAh / cm 2 ) can be cycled for 200h.

[0237] The lithium-ion batteries disclosed in Examples 2 and 6 can be cycled more than 100 times.

[0238] In summary, the lithium-ion battery disclosed in the embodiment of the present application can be stably cycled at room temperature and has advantages such as a long cycle life. One of the reasons why lithium-ion batteries have the above advantages may be that the sulfide solid electrolyte of the lithium-ion battery is doped with N-containing doping groups, and N can form Li3N with Li in the metal lithium negative electrode. The presence of Li3N can hinder the Li6PS5Cl 0.95 SCN 0.05 The side reaction with Li inhibits the formation of lithium dendrites, making the lithium-ion battery have a longer cycle life. Another reason is that Li3N can stabilize the interface between the sulfide solid electrolyte and the metal lithium negative electrode. Li+ can be evenly deposited or stripped on the metal lithium negative electrode surface, thereby improving the cycle life of the lithium-ion battery.

[0239] The present application also discloses a method for preparing a lithium-ion battery. Fig.23 , the preparation method of the lithium ion battery comprises: S231-S233:

[0240] S231: forming a doped sulfide material.

[0241] The crystals of doped sulfide materials include: Cubic crystal form; at least one site in the unit cell constituting the crystal is doped with a doping group, and the doping group includes: N element.

[0242] The preparation process of the doped sulfide material may refer to the above embodiments and will not be described again here.

[0243] S232: Forming a sulfide solid electrolyte using a doped sulfide material.

[0244] The sulfide solid electrolyte adopts the doped sulfide material disclosed in the embodiments of the present application.

[0245] In the embodiment of the present application, S232 may be performed by using a method for forming a sulfide solid electrolyte commonly used in the art. Exemplarily, the sulfide solid electrolyte may be formed by pressing.

[0246] S233: Assemble a metallic lithium negative electrode, a sulfide solid electrolyte and a positive electrode to obtain a lithium-ion battery.

[0247] The embodiments of the present application may adopt the lithium-ion battery assembly method commonly used in the art. For example, a Swagelok mold or a solid mold may be used to assemble the lithium-ion battery.

[0248] See also Fig.24 The preparation method of the lithium-ion battery is further described below with reference to a specific example:

[0249] Step 1: Place the LiSCN·xH2O crystal in a vacuum oven under 100 mBar vacuum conditions, slowly heat it to 150°C to melt, with a heating rate of 25°C / hr, and dry it at 150°C for 24 hours.

[0250] Step 2: Further increase the temperature to 200°C at a heating rate of 25°C / hr and dry for 20 hours to obtain LiSCN white powder.

[0251] Step 3: In an inert gas atmosphere, Li2S, P2S5, LiCl and dried LiSCN white powder in a certain stoichiometric ratio are mixed evenly, and then a uniform phase is obtained by high-speed ball milling at 600 rpm for 20 h.

[0252] Step 4: Press the sulfide powder obtained by ball milling under 2 tons axial pressure for 5 minutes in an inert gas atmosphere to form a powder cake, and then sinter it in a muffle furnace at 400℃-500℃ for 15 hours to obtain a pure phase and high crystallinity doped sulfide material. The morphology of doped sulfide materials can be found in Fig.24 (a) in .

[0253] Step 5: Place 0.100g of the modified doped sulfide material obtained by sintering in a uniaxial pressure mold and press it into a dense (relative density above 95%) sulfide solid electrolyte under a pressure of 2 tons for five minutes. The morphology of sulfide solid electrolyte can be found in Fig.24 (b) in .

[0254] Step 6: Cut two lithium metal sheets of the same diameter and place them at both ends of the pressed sulfide solid electrolyte to form a lithium-ion battery. Fig.24 (c) in .

[0255] The effects brought about by the preparation method can refer to the effects brought about by any possible implementation method of the above-mentioned doped sulfide material and lithium-ion battery.

[0256] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.

[0257] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A doped sulfide material, characterized in that: The crystal of the doped sulfide material comprises: the space point group is Cubic crystal form; At least one site in a unit cell constituting the crystal is doped with a doping group, and the doping group includes nitrogen.

2. The sulfide material according to claim 1, characterized in that The chemical formula of the doped sulfide material includes: Li6PS5Cl 1-n1 X n1 , wherein X is a doping group, 0 <n1≤0.2。 3. The sulfide material according to claim 1, characterized in that The chemical formula of the doped sulfide material includes: Li 7-n2 PS 6-n X n2 , 0 <n2≤0.5。 4. The sulfide material according to claim 1, characterized in that The doping amount of the doping group is between 0.01% and 20%.

5. The sulfide material according to any one of claims 1 to 4, characterized in that: The unit cell of the crystal also includes sulfur ions, and the volume of the doping group is greater than the volume of the sulfur ions.

6. The sulfide material according to any one of claims 1 to 5, characterized in that: The doping group includes at least one of thiocyanate ions and cyanide ions.

7. The sulfide material according to any one of claims 1 to 6, characterized in that: The doping groups are doped at the vertices of the unit cell.

8. A method for preparing a sulfide material, characterized in that: include: Mixing raw materials; The mixed raw materials are crystallized to obtain a doped sulfide material, wherein the crystal of the doped sulfide material comprises: a space point group of A cubic crystal form; at least one site in the unit cell constituting the crystal is doped with a doping group, and the doping group includes: nitrogen element.

9. The preparation method according to claim 8, characterized in that: The raw material includes: lithium salt, and the lithium salt includes: the doping group and lithium ions. Before the step of mixing the raw materials, the preparation method further includes: Drying the lithium salt by heating it to a first temperature, wherein the first temperature is greater than the melting point of the lithium salt and less than the decomposition temperature of water; The dried lithium salt is heated to a second temperature for drying, and the second temperature is higher than the first temperature.

10. The preparation method according to claim 8 or 9, characterized in that: The steps of mixing the raw materials are specifically as follows: The raw materials were extruded using a ball mill.

11. A lithium ion battery, characterized in that: include: Metal lithium anode, sulfide solid electrolyte and cathode; The sulfide solid electrolyte is arranged between the metal lithium negative electrode and the positive electrode; The materials used in the sulfide solid electrolyte include: doped sulfide materials, and the crystals of the doped sulfide materials include: space point groups are A cubic crystal form; at least one site in the unit cell constituting the crystal is doped with a doping group, and the doping group includes: nitrogen element.

12. The lithium ion battery according to claim 11, characterized in that: The materials used for the positive electrode include: the doped sulfide material, positive electrode material and conductive carbon.

13. The lithium ion battery according to claim 12, characterized in that: Among the materials used for the positive electrode, the mass fraction of the doped sulfide material is 10%-30%; the mass fraction of the positive electrode material is 65%-80%; and the mass fraction of the conductive carbon is 2%-5%.

14. The lithium ion battery according to claim 11, characterized in that: The materials used for the positive electrode include: the doped sulfide material, a positive electrode material and a binder.

15. The lithium ion battery according to claim 14, characterized in that: Among the materials used for the positive electrode, the mass fraction of the doped sulfide material is 10%-30%; the mass fraction of the positive electrode material is 68%-80%; and the mass fraction of the adhesive is 0.5%-3%.

Citation Information

Cited By

  • Preparation method of lithium-germanium-phosphorus-sulfur solid-state battery

    CN120341400A