Multilayer film, packaging material, and packaging body
By designing a multi-layer structure in the polypropylene film, using materials such as propylene homopolymer, propylene copolymer resin and propylene-ethylene block copolymer resin, combined with titanium oxide, the concealment and cold resistance of the polypropylene film at low temperatures is solved. The problem of difficulty in taking into account both impact properties has achieved excellent performance of multi-layer films.
Patent Information
- Application Number
- CN202380028993.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-26
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-05
AI Technical Summary
The existing polypropylene films are difficult to take into account both concealment and cold impact resistance at low temperatures. The addition of pigment will affect cold impact resistance, and the heat sealing of a single material packaging material is insufficient.
A multi-layer film structure is adopted, in which the heat sealing layer consists of propylene homopolymer and propylene copolymer resin, and the hidden layer contains propylene-ethylene block copolymer resin, ethylene-propylene copolymer elastomer and titanium oxide, with a titanium oxide content of 0.10 to 30.00 % by mass to take into account both concealment and cold impact resistance.
The multilayer film has sufficient concealment and excellent cold impact resistance at low temperatures, while maintaining good heat resistance and low temperature sealing at high temperatures.
Smart Images

Figure CN118900770A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to multilayer films, packaging materials and packages. Background Art
[0002] Polypropylene films are sometimes used as sealant films in various packaging materials such as food packaging because they are excellent in rigidity and heat resistance and are inexpensive.
[0003] Patent Document 1 proposes a polypropylene composite film, characterized in that it is a three-layer polypropylene composite film, wherein the middle layer is formed of a propylene-ethylene block copolymer resin and both surface layers are formed of propylene random copolymers.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-132186 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] The polypropylene film used in the sealant film is required to have heat-sealability and cold-shock resistance so that the bag will not break even when stored at low temperatures. In addition, in order to impart concealment to packaging materials, materials other than the sealant film, such as aluminum substrates, have been used in the past. However, as long as the sealant film can be given a concealment function, it is necessary to promote the diversification of packaging materials.
[0009] In order to provide the film with a concealing function, it is considered to add a pigment such as titanium oxide. However, the addition of a pigment leads to a decrease in cold impact resistance, and it is difficult to achieve both concealing and cold impact resistance.
[0010] Therefore, one aspect of the present disclosure is to provide a multilayer film that can be used as a sealant film, has sufficient concealment, and has excellent cold shock resistance. In addition, other aspects of the present disclosure are to provide a packaging material having the multilayer film, and a packaging body made of the packaging material.
[0011] Means for solving technical problems
[0012] Several aspects of the present disclosure provide the following [1] to
[15] .
[0013] [1] A multilayer film comprising a heat-sealing layer and a concealing layer arranged on the heat-sealing layer, wherein the heat-sealing layer comprises a propylene homopolymer (A) and / or a propylene-based copolymer resin (B), and the concealing layer comprises a propylene-ethylene block copolymer resin (C), an ethylene-propylene copolymer elastomer (D), and titanium oxide (E), and the content of the titanium oxide (E) in the concealing layer is 0.10 to 30.00% by mass based on the total mass of the concealing layer.
[0014] [2] The multilayer film according to [1], wherein the heat seal layer contains a propylene copolymer resin (B), and the propylene copolymer resin (B) has a melting point of 132 to 150°C.
[0015] [3] The multilayer film according to [1] or [2], wherein the heat seal layer contains a propylene copolymer resin (B), and the ethylene content in the propylene copolymer resin (B) is 3.0 to 6.0% by mass based on the total mass of the propylene copolymer resin (B).
[0016] [4] A multilayer film according to any one of [1] to [3], wherein the content of the propylene homopolymer (A) in the heat seal layer is 10 to 70% by mass, based on the total mass of the heat seal layer, and the content of the propylene copolymer resin (B) in the heat seal layer is 30 to 90% by mass, based on the total mass of the heat seal layer.
[0017] [5] The multilayer film according to any one of [1] to [4], wherein the mass ratio of the content of the propylene-based copolymer resin (B) to the content of the propylene homopolymer (A) in the heat seal layer is 0.10 to 9.00.
[0018] [6] A multilayer film according to any one of [1] to [5], wherein the content of the propylene-ethylene block copolymer resin (C) in the concealing layer is 35 to 90% by mass based on the total mass of the concealing layer, and the content of the ethylene-propylene copolymer elastomer (D) in the concealing layer is 10 to 50% by mass based on the total mass of the concealing layer.
[0019] [7] The multilayer film according to any one of [1] to [6], wherein the mass ratio of the content of the ethylene-propylene copolymer elastomer (D) to the content of the propylene-ethylene block copolymer resin (C) in the concealing layer is 0.10 to 1.00.
[0020] [8] The multilayer film according to any one of [1] to [7], wherein the propylene content is 70% by mass or more based on the total mass of the multilayer film.
[0021] [9] The multilayer film according to any one of [1] to [8], wherein the thickness of the heat seal layer is 8 to 30% based on the thickness of the multilayer film.
[0022]
[10] The multilayer film according to any one of [1] to [9], wherein the concealing layer has a thickness of 20 μm or more.
[0023]
[11] The multilayer film according to any one of [1] to
[10] , which comprises the heat seal layer, the concealing layer, and a lamination layer in this order, wherein the lamination layer contains a propylene homopolymer (A) and / or a propylene copolymer resin (B).
[0024]
[12] The multilayer film according to
[11] , wherein the total thickness of the heat seal layer and the laminating layer is 16 to 42% based on the thickness of the multilayer film.
[0025]
[13] A packaging material comprising the multilayer film according to any one of [1] to
[12] .
[0026]
[14] The packaging material according to
[13] , further comprising a biaxially stretched polypropylene film on the side opposite to the heat seal layer side when viewed from the concealing layer of the multilayer film.
[0027]
[15] A packaging body made from the packaging material described in
[13] or
[14] .
[0028] Effects of the Invention
[0029] According to one aspect of the present disclosure, a multilayer film can be provided, which can be used as a sealant film, has sufficient concealment, and has excellent cold shock resistance. In addition, according to other aspects of the present disclosure, a packaging material having the multilayer film and a packaging body made of the packaging material can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic cross-sectional view showing one embodiment of the multilayer film disclosed herein.
[0031] Figure 2 FIG. 4 is a schematic cross-sectional view showing another embodiment of the multilayer film of the present disclosure.
[0032] Figure 3 It is a schematic cross-sectional view showing one embodiment of the packaging material disclosed herein.
[0033] Figure 4 It is a schematic cross-sectional view showing another embodiment of the packaging material disclosed herein. DETAILED DESCRIPTION
[0034] In this specification, the numerical range represented by "~" means a range that includes the numerical values recorded before and after "~" as the minimum and maximum values, respectively. In addition, except for the case where it is specifically stated, the units of the numerical values recorded before and after "~" are the same. In the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be replaced by the upper limit or lower limit of the numerical range of other stages. In addition, in the numerical range recorded in this specification, the upper limit or lower limit of the numerical range can also be replaced by the value shown in the embodiment. In addition, the upper limit and lower limit recorded separately can also be combined arbitrarily. In addition, the acquisition method of the polymerization raw materials of the resins (propylene homopolymer (A), propylene-based copolymer resin (B), propylene-ethylene block copolymer resin (C) and ethylene-propylene copolymer elastomer (D)) in this specification is not particularly limited, and all raw material sources such as existing components refined from petroleum, components generated by chemical regeneration methods, and plant-derived components can be used.
[0035] <Multilayer film>
[0036] Figure 1 This is a cross-sectional view of a multilayer film according to an embodiment of the present disclosure. The multilayer film 10 comprises a heat seal layer 1 and a concealing layer 2 disposed on the heat seal layer 1. The heat seal layer comprises a propylene homopolymer (A) and / or a propylene copolymer resin (B), and the concealing layer 2 comprises a propylene-ethylene block copolymer resin (C), an ethylene-propylene copolymer elastomer (D), and titanium oxide (E). The content of titanium oxide (E) in the concealing layer 2 is 0.10 to 30.00% by mass based on the total mass of the concealing layer 2.
[0037] Figure 2 1 is a cross-sectional view of a multilayer film according to another embodiment of the present disclosure. The multilayer film 11 comprises a heat seal layer 1, a concealing layer 2, and a laminating layer 3 in sequence. The heat seal layer 1 and the concealing layer 2 are the same as the heat seal layer 1 and the concealing layer 2 in the multilayer film 10. The laminating layer 3 comprises a propylene homopolymer (A) and / or a propylene copolymer resin (B).
[0038] The multilayer film (10, 11) can be used as a sealant film (e.g., a polypropylene-based unstretched sealant film), has sufficient concealment, and has excellent cold shock resistance. Therefore, the multilayer film (10, 11) can be preferably used in a packaging material (e.g., a packaging sealant film, or a packaging film having a packaging sealant film and a substrate). The multilayer film (10, 11) can be used as a single film or can be used after being laminated with a substrate. When the multilayer film (10, 11) is used as a packaging material, there is no particular limitation on the method of using the packaging material.
[0039] The cold impact resistance of the multilayer film (10, 11) can be evaluated by the impact strength of the film when stored at low temperature. Specifically, the impact strength of the film is measured using a film impact tester at a temperature of -5°C, an impact energy of 1.5J, and an impact head size of 1 / 2 inch. The impact strength of the film measured under the above conditions is, for example, 6.00J / mm or more (e.g., 6.00 to 12.00J / mm), and by adjusting the composition and thickness of each layer, it can also be 7.00J / mm or more, 8.00J / mm or more, 9.00J / mm or more, 10.00J / mm or more, or 11.00J / mm or more.
[0040] The concealment of the multilayer film (10, 11) can be evaluated by the transmission concentration. The transmission concentration is the common logarithm of the reciprocal of the transmittance, and can be measured using a transmission concentration meter (e.g., a portable transmission concentration meter manufactured by X-RITE). The transmission concentration of the multilayer film (10, 11) is, for example, 0.20 or more (e.g., 0.20 to 0.80), and can be 0.30 or more, 0.40 or more, 0.50 or more, 0.60 or more, or 0.70 or more by adjusting the composition and thickness of each layer.
[0041] However, in the field of packaging materials for food and the like, attempts to "single material" to form packaging materials with a single raw material have been promoted. The multilayer film has sufficient concealment even without containing non-polypropylene-based materials such as aluminum substrates that have been used in the past to impart concealment to packaging materials, and is therefore particularly preferably used in single-material packaging materials that require concealment.
[0042] In the attempt to make a single material, since the sealant film and the substrate are made of the same raw material, the melting point of the sealant film is inevitably close to that of the substrate, and the substrate is easily melted together with the sealant film in the heat sealing process. Therefore, the sealant film used in the packaging material of a single material is sometimes required to have excellent heat sealing properties at low temperatures (hereinafter also referred to as "low-temperature sealing properties"). From this point of view, the above-mentioned multilayer film also has excellent low-temperature sealing properties by using a low-melting point material (for example, a propylene copolymer resin (B) having a melting point of 150°C or less) as the material of the heat sealing layer.
[0043] Each layer of the multilayer film (10, 11) will be described in detail below. In the following description, reference numerals are omitted.
[0044] (Heat seal layer)
[0045] The heat seal layer contains, for example, a propylene homopolymer (A) and / or a propylene-based copolymer resin (B).
[0046] [Propylene homopolymer (A)]
[0047] The propylene homopolymer (A) is, for example, a homopolymer of propylene that can be obtained by homopolymerizing propylene using a Ziegler-Natta catalyst, a metallocene catalyst, or a semi-metallocene catalyst. When the heat seal layer contains the propylene homopolymer (A), the multilayer film has excellent heat resistance (hereinafter also simply referred to as "heat resistance") such as being able to withstand a pressure treatment at a high temperature of 120 to 135° C. for sterilization and boiling treatment. Therefore, it can be said that the multilayer film having a heat seal layer containing the propylene homopolymer (A) can be preferably used in packaging materials that are subjected to severe treatments such as boiling water treatment or boiling treatment.
[0048] As the propylene homopolymer (A), for example, a material having a melting start temperature of 150°C or higher and a melting point (melting peak temperature) of 155°C or higher can be used. When both the melting start temperature and the melting point are within this range, the material has more excellent heat resistance, and for example, even after a retort treatment at a high temperature, melt adhesion is less likely to occur on the inner surface of the packaging bag. Furthermore, from the viewpoint of obtaining more excellent heat resistance, the melting start temperature of the propylene homopolymer (A) may be 151°C or higher or 152°C or higher, and the melting point of the propylene homopolymer (A) may be 156°C or higher or 158°C or higher. The melting start temperature of the propylene homopolymer (A) is, for example, 160°C or lower, and from the viewpoint of obtaining more excellent low-temperature sealing properties, it may be 155°C or lower or 153°C or lower. The melting point of the propylene homopolymer (A) is, for example, 170°C or lower, and from the viewpoint of obtaining more excellent low-temperature sealing properties, it may be 165°C or lower or 160°C or lower. From the above viewpoints, the melting start temperature of the propylene homopolymer (A) may be, for example, 150 to 160° C., and the melting point of the propylene homopolymer (A) may be, for example, 155 to 170° C. In the present specification, the melting start temperature and the melting point are values obtained by differential scanning calorimetry according to JIS K 7121.
[0049] As the propylene homopolymer (A), one having a melt flow rate (MFR) in the range of 2.0 to 7.0 g / 10 minutes can be used. When the melt flow rate is above the above lower limit, the load on the extruder during the molding process is reduced, the processing speed is difficult to decrease, and it is easy to maintain excellent productivity. In addition, when the melt flow rate is below the upper limit, the heat seal layer tends to have better cold impact resistance. From these viewpoints, the melt flow rate of the propylene homopolymer (A) can also be 2.5 to 6.0 g / 10 minutes or 3.0 to 5.0 g / 10 minutes. In addition, in this specification, the melt flow rate is a value measured under the conditions of a temperature of 230°C and a load of 2.16 kg according to ISO 1133.
[0050] [Propylene copolymer resin (B)]
[0051] The propylene-based copolymer resin (B) is a resin obtained by copolymerizing propylene with other comonomers.
[0052] The propylene copolymer resin (B) may have a lower melting point than the propylene homopolymer (A). The melting point of the propylene copolymer resin (B) is preferably below 150°C. When the heat seal layer contains a propylene resin having such a melting point, the multilayer film also has excellent low-temperature sealing properties. Such a multilayer film is more preferably used as a sealant film for a single-material packaging material. From the viewpoint of better heat resistance and cold shock resistance, the melting point of the propylene copolymer resin (B) may be above 132°C, above 135°C, above 140°C, or above 145°C. From the above viewpoints, the melting point of the propylene copolymer resin (B) may be, for example, 132-150°C, 135-150°C, 140-150°C, or 145-150°C. The melting start temperature of the propylene copolymer resin (B) may be 120 to 145° C., 125 to 145° C., or 135 to 145° C. from the viewpoint of achieving a better balance between heat resistance and low-temperature sealing properties. The melting point of the propylene copolymer resin (B) after the heat seal layer is formed can be obtained, for example, by separating the heat seal layer by a high temperature LC method using graphite carbon as an adsorbent and measuring the melting points of each layer.
[0053] The propylene copolymer resin (B) can be a resin obtained by copolymerization of propylene and a comonomer containing ethylene (a resin containing a copolymer of propylene and ethylene). From the viewpoint that the low-temperature sealing property of the multilayer film is more excellent, the propylene copolymer resin (B) can contain a propylene-ethylene random copolymer. The propylene-ethylene random copolymer can be obtained, for example, by adding ethylene as a comonomer to the main monomer formed by propylene using a Ziegler-Natta catalyst, a metallocene catalyst, or a semi-metallocene catalyst and copolymerizing them. The copolymer constituting the propylene copolymer resin (B) can be one or more. When the propylene copolymer resin (B) is a mixture of multiple copolymers, the melting point of the mixture is used as the melting point of the propylene copolymer resin (B).
[0054] The ethylene content in the propylene copolymer resin (B) can be 6.0% by mass or less based on the total mass of the propylene copolymer resin (B). By having an ethylene content of 6.0% by mass or less, the heat resistance can be maintained while maintaining low-temperature sealing performance without excessively reducing the heat resistance, and after the retort treatment, the melt adhesion on the inner surface of the packaging bag can also be suppressed. From the viewpoint of more significantly obtaining this effect, the ethylene content can be 5.5% by mass or less or 4.5% by mass or less. The lower limit of the ethylene content is not particularly limited, and from the viewpoint of low-temperature sealing performance, it can be 3.0% by mass. From these viewpoints, the ethylene content in the propylene copolymer resin (B) can be 3.0 to 6.0% by mass, 3.0 to 5.5% by mass, or 3.0 to 4.5% by mass based on the total mass of the propylene copolymer resin (B).
[0055] The ethylene content of the propylene copolymer resin (B) can be measured according to the quantitative method (IR method) for ethylene content described in "Handbook of Polymer Analysis Edited by the Japan Society for Analytical Analysis (3rd edition, May 10, 2013)" (Handbook of Polymer Analysis Edited by the Japan Society for Analytical Analysis (3rd edition, May 10, 2013)).
[0056] The melt flow rate (MFR: ISO 1133) (temperature is 230°C, load is 2.16 kg) of the propylene-based copolymer resin (B) can be 1.0 to 10.0 g / 10 minutes. When the melt flow rate is above the above lower limit, the load on the extruder during the molding process is reduced, the processing speed is difficult to reduce, and it is easy to maintain excellent productivity. When the melt flow rate is below the above upper limit, the heat seal layer tends to have excellent cold impact resistance. From these viewpoints, the melt flow rate of the propylene-based copolymer resin (B) can also be 2.0 to 9.0 g / 10 minutes or 3.0 to 8.0 g / 10 minutes.
[0057] The components contained in the heat seal layer are described above, but the heat seal layer may also contain components other than the propylene homopolymer (A) and the propylene copolymer resin (B). However, from the viewpoint of using the heat seal layer in a single material packaging material composed of the same raw material of the polypropylene system, the propylene content in the heat seal layer is preferably 70% by mass or more. In addition, the propylene content in the heat seal layer can be measured by Raman spectroscopy.
[0058] The heat seal layer preferably contains both a propylene homopolymer (A) and a propylene copolymer resin (B) from the viewpoint of achieving both excellent heat resistance and excellent low-temperature sealing properties, and more preferably contains a propylene homopolymer (A) and a propylene copolymer resin (B) having a melting point of 132 to 150° C. When the heat seal layer contains both a propylene homopolymer (A) and a propylene copolymer resin (B), from the viewpoint of achieving both heat resistance and low-temperature sealing properties in a better balance, it is preferred that the content of the propylene homopolymer (A) in the heat seal layer is 10 to 70% by mass based on the total mass of the heat seal layer, and the content of the propylene copolymer resin (B) (preferably a propylene copolymer resin (B) having a melting point of 132 to 150° C.) in the heat seal layer is 30 to 90% by mass based on the total mass of the heat seal layer.
[0059] The content of the propylene homopolymer (A) in the heat seal layer may be 10% by mass or more, 15% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, or 50% by mass or more based on the total mass of the heat seal layer from the viewpoint of better heat resistance. The content of the propylene homopolymer (A) in the heat seal layer may be 70% by mass or less, 65% by mass or less, 60% by mass or less, 55% by mass or less, or 50% by mass or less based on the total mass of the heat seal layer from the viewpoint of better low-temperature sealing performance and cold shock resistance. From these viewpoints, the content of the propylene homopolymer (A) in the heat seal layer may be 10 to 70% by mass, 15 to 65% by mass, 20 to 60% by mass, 30 to 55% by mass, 40 to 55% by mass, 10 to 50% by mass, or 50 to 70% by mass based on the total mass of the heat seal layer. The content of the propylene homopolymer (A) in the heat seal layer may be 75 to 100% by mass based on the total mass of the heat seal layer from the viewpoint of achieving more excellent low-temperature sealability.
[0060] The content of the propylene copolymer resin (B) in the heat seal layer can be 30% by mass or more, 35% by mass or more, 40% by mass or more, 45% by mass or more, or 50% by mass or more, based on the total mass of the heat seal layer, from the viewpoint of better low-temperature sealing performance and cold shock resistance. The content of the propylene copolymer resin (B) in the heat seal layer can be 90% by mass or less, 85% by mass or less, 80% by mass or less, 70% by mass or less, 60% by mass or less, or 50% by mass or less, based on the total mass of the heat seal layer, from the viewpoint of better heat resistance. From these viewpoints, the content of the propylene copolymer resin (B) in the heat seal layer can be 30 to 90% by mass, and can also be 35 to 85% by mass, 40 to 80% by mass, 45 to 70% by mass, 45 to 60% by mass, 50 to 90% by mass, or 35 to 50% by mass, based on the total mass of the heat seal layer. The content of the propylene homopolymer (B) in the heat seal layer may be 0 to 25% by mass based on the total mass of the heat seal layer from the viewpoint of achieving more excellent low-temperature sealability.
[0061] The mass ratio [(B) / (A)] of the content of the propylene copolymer resin (B) to the content of the propylene homopolymer (A) in the heat seal layer may be 0.10 to 9.00 from the viewpoint of better heat resistance and cold shock resistance. The mass ratio [(B) / (A)] may be 0.20 or more, 0.40 or more, or 0.80 or more, and may be 5.00 or less, 2.50 or less, or 1.50 or less from the viewpoint of further better heat resistance and cold shock resistance.
[0062] (Hidden Layer)
[0063] The concealing layer comprises a propylene-ethylene block copolymer resin (C), an ethylene-propylene copolymer elastomer (D), and titanium oxide (E). Since the concealing layer comprises more than 0.10% by mass of titanium oxide (E), the multilayer film has concealment. In addition, by comprising the propylene-ethylene block copolymer resin (C) and the ethylene-propylene copolymer elastomer (D) in the concealing layer, while suppressing the content of titanium oxide (E) to less than 30.00% by mass, both concealment brought by titanium oxide (E) and excellent cold impact resistance can be taken into account.
[0064] [Propylene-ethylene block copolymer resin (C)]
[0065] The propylene-ethylene block copolymer resin (C) is a resin obtained by block copolymerization of propylene and ethylene.
[0066] Propylene-ethylene block copolymer resin (C) for example comprises a propylene homopolymer component (c1), an ethylene-propylene copolymer component (c2) as a copolymer of ethylene and propylene (e.g., a random copolymer). Such a propylene-ethylene block copolymer resin (C) can be obtained, for example, by manufacturing a propylene homopolymer component (c1) in a first step, and then manufacturing an ethylene-propylene copolymer component (c2) by gas phase polymerization in the presence of a propylene homopolymer component (c1) in a second step. For example, a Ziegler-Natta catalyst, a metallocene catalyst, a semi-metallocene catalyst, etc. can be used during polymerization. In addition, it is generally believed that the propylene-ethylene block copolymer resin (C) obtained by this method is not a block copolymer formed by bonding a propylene homopolymer end to an ethylene-propylene copolymer end (a block copolymer formed by repetition of a block formed by a propylene homopolymer component (c1) and a block formed by an ethylene-propylene copolymer component (c2)), but a mixture of a propylene homopolymer component (c1) and an ethylene-propylene copolymer component (c2).
[0067] The propylene-ethylene block copolymer resin (C) may contain 60.0 to 90.0% by mass of the propylene homopolymer component (c1) and 10.0 to 40.0% by mass of the ethylene-propylene copolymer component (c2) based on the total mass of the propylene-ethylene block copolymer resin (C). By having the content of each component in the above range, it is easy to obtain more excellent cold impact resistance. From the above viewpoint, the content of the propylene homopolymer component (c1) in the propylene-ethylene block copolymer resin (C) may be 65.0 to 87.5% by mass, or 70.0 to 85.0% by mass, based on the total mass of the propylene-ethylene block copolymer resin (C). Similarly, the content of the ethylene-propylene copolymer component (c2) in the propylene-ethylene block copolymer resin (C) may be 12.5 to 35.0% by mass, or 15.0 to 30.0% by mass, based on the total mass of the propylene-ethylene block copolymer resin (C).
[0068] The ethylene content in the ethylene-propylene copolymer component (c2) can be 20.0 to 40.0% by mass based on the total mass of the ethylene-propylene copolymer component (c2). When the ethylene content is below the upper limit, the viscosity of the product can be suppressed, and it is difficult to cause contamination caused by the viscosity of the product during manufacturing, and it is easy to maintain excellent productivity. When the ethylene content is above the lower limit, it is easy to obtain more excellent cold impact resistance.
[0069] The ethylene content of the ethylene-propylene copolymer component (c2) can be measured according to the quantitative method (IR method) for ethylene content described on pages 412 to 413 of the Handbook of Polymer Analysis compiled by the Japan Society for Analytical Analysis (3rd edition, May 10, 2013) (Handbook of Polymer Analysis compiled by the Japan Society for Analytical Analysis (3rd edition, May 10, 2013)).
[0070] As the propylene-ethylene block copolymer resin (C), one having a melt flow rate (MFR: ISO 1133) (temperature: 230°C, load: 2.16 kg) of 0.5 to 2.5 g / 10 min can be used. When the melt flow rate is above the above lower limit, the load on the extruder during the molding process is reduced, the processing speed is difficult to decrease, and excellent productivity is easy to maintain. When the melt flow rate is below the above upper limit, the concealing layer tends to have excellent cold impact resistance. From these viewpoints, the melt flow rate of the propylene-ethylene block copolymer resin (C) can also be 1.0 to 2.2 g / 10 min or 1.5 to 2.0 g / 10 min.
[0071] [Ethylene-propylene copolymer elastomer (D)]
[0072] The ethylene-propylene copolymer elastomer (D) is an elastomer obtained by block copolymerization of propylene and ethylene.
[0073] The ethylene-propylene copolymer elastomer (D) can be obtained, for example, by a slurry polymerization method carried out in the presence of an inert hydrocarbon such as hexane, heptane, kerosene, or a liquefied α-olefin solvent such as propylene, or a gas phase polymerization method without a solvent. Specifically, the ethylene-propylene copolymer elastomer (D) can be obtained using a known multi-stage polymerization method. That is, it can be a polypropylene resin containing a polymerized high rubber obtained by polymerizing propylene and / or propylene-α-olefin polymer in a reactor of the first stage and then copolymerizing propylene with α-olefin in a reactor of the second stage. The polymerization can be carried out using, for example, a Ziegler-Natta catalyst, a metallocene catalyst, a semi-metallocene catalyst, etc.
[0074] The melt flow rate (MFR: ISO 1133) of the ethylene-propylene copolymer elastomer (D) (temperature: 230°C, load: 2.16 kg) can be 0.5 to 3.5 g / 10 min. When the melt flow rate is above the above lower limit, the extruder load during the molding process is reduced, the processing speed is difficult to decrease, and it is easy to maintain excellent productivity. When the melt flow rate is below the above upper limit, the compatibility of the propylene-ethylene block copolymer resin (C) and the ethylene-propylene copolymer elastomer (D) becomes good, and it is easy to obtain more excellent cold impact resistance.
[0075] The mass ratio of the propylene content to the ethylene content in the ethylene-propylene copolymer elastomer (D) [propylene content / ethylene content] may be 1.5 to 4.0, 2.0 to 3.5 or 2.5 to 3.0 from the viewpoint of obtaining more excellent cold-resistant impact properties.
[0076] The propylene content of the ethylene-propylene copolymer elastomer (D) can be measured by Raman spectroscopy. In addition, the ethylene content of the ethylene-propylene copolymer elastomer (D) can be measured by the quantitative method (IR method) of ethylene content described in the polymer analysis handbook compiled by the Japan Society for Analytical Studies (May 10, 2013, 3rd edition) on pages 412 to 413.
[0077] [Titanium oxide (E)]
[0078] Titanium oxide (E) is, for example, in the form of particles and dispersed in the heat seal layer. The average particle size of titanium oxide may be 0.10 to 0.50 μm, 0.15 to 0.40 μm, or 0.20 to 0.30 μm. The average particle size of titanium oxide is a value measured by a laser diffraction-scattering method.
[0079] The above describes the components contained in the concealing layer, but the concealing layer may also contain components other than the propylene-ethylene block copolymer resin (C), the ethylene-propylene copolymer elastomer (D) and the titanium oxide (E). Among them, from the viewpoint of using in a packaging material of a single material composed of the same raw material of the polypropylene system, the propylene content in the concealing layer is preferably 70% by mass or more. In addition, the propylene content in the concealing layer can be measured by Raman spectroscopy.
[0080] From the viewpoint of better heat resistance, the content of the propylene-ethylene block copolymer resin (C) in the concealing layer can be 35% by mass or more, 50% by mass or more, or 60% by mass or more, based on the total mass of the concealing layer. From the viewpoint of better cold impact resistance, the content of the propylene-ethylene block copolymer resin (C) in the concealing layer can be 90% by mass or less, 80% by mass or less, or 70% by mass or less, based on the total mass of the concealing layer. From these viewpoints, the content of the propylene-ethylene block copolymer resin (C) in the concealing layer can be 35 to 90% by mass, 50 to 80% by mass, 50 to 70% by mass, or 60 to 80% by mass, based on the total mass of the concealing layer.
[0081] From the viewpoint of better cold-resistance and impact resistance, the content of the ethylene-propylene copolymer elastomer (D) in the concealing layer can be 10% by mass or more, 15% by mass or more, or 20% by mass or more, based on the total mass of the concealing layer. From the viewpoint of better heat resistance, the content of the ethylene-propylene copolymer elastomer (D) in the concealing layer can be 50% by mass or less, 40% by mass or less, or 30% by mass or less, based on the total mass of the concealing layer. From these viewpoints, the content of the ethylene-propylene copolymer elastomer (D) in the concealing layer can be 10 to 50% by mass, 10 to 40% by mass, 15 to 40% by mass, or 20 to 30% by mass, based on the total mass of the concealing layer.
[0082] The mass ratio [(D) / (C)] of the content of the ethylene-propylene copolymer elastomer (D) to the content of the propylene-ethylene block copolymer resin (C) in the concealing layer is preferably 0.10 to 1.00 from the viewpoint of better heat resistance and cold impact resistance. The mass ratio [(D) / (C)] may be 0.20 or more, 0.30 or more, or 0.40 or more from the viewpoint of better cold impact resistance. The mass ratio [(D) / (C)] may be 0.80 or less, 0.60 or less, or 0.40 or less from the viewpoint of better heat resistance.
[0083] The content of titanium oxide (E) in the concealing layer is 0.10 to 30.00 mass %. From the viewpoint of better concealment, the content of titanium oxide (E) in the concealing layer can be 1.00 mass % or more, 5.00 mass % or more, 7.00 mass % or more, or 10.00 mass % or more based on the total mass of the concealing layer. From the viewpoint of better cold impact resistance, the content of titanium oxide (E) in the concealing layer can be 23.00 mass % or less, 20.00 mass % or less, 15.00 mass % or less, 12.00 mass % or less, or 8.00 mass % or less based on the total mass of the concealing layer.
[0084] (Lamination layer)
[0085] The laminating layer is a layer having laminating properties with respect to a substrate, etc. The laminating layer contains the propylene homopolymer (A) and / or the propylene copolymer resin (B) described in the heat seal layer. By providing the laminating layer, deformation or curling of the multilayer film can be easily suppressed.
[0086] The mixing ratio of the propylene homopolymer (A) and the propylene copolymer resin (B) in the laminate layer is not particularly limited. From the viewpoint of suppressing the curling of the film after film formation, it is preferably the same mixing ratio as the heat seal layer. That is, the content of the propylene homopolymer (A) in the laminate layer is 10 to 70% by mass based on the total mass of the laminate layer, and the content of the propylene copolymer resin (B) in the laminate layer is preferably 30 to 90% by mass based on the total mass of the laminate layer. Other features in the laminate layer may also be the same as those of the above-mentioned heat seal layer. For example, the melting point of the propylene copolymer resin (B) contained in the laminate layer can be 132 to 150°C. In addition, for example, the propylene content in the laminate layer can be 70% by mass or more. In addition, the propylene content in the laminate layer can be measured according to Raman spectroscopy.
[0087] (Thickness of layer)
[0088] The thickness of the multilayer film is not particularly limited as long as it is within a range that allows the film to be used as a packaging material, but excessive thickness may result in cost disadvantages. Therefore, the thickness of the multilayer film may be 100 μm or less (e.g., 50 to 100 μm), or 70 μm or less (e.g., 50 to 70 μm).
[0089] The thickness of the heat seal layer can be 8 to 30% based on the thickness of the multilayer film. When the thickness ratio of the heat seal layer is above the above lower limit, it is easy to obtain more excellent cold impact resistance. In addition, when the thickness ratio of the heat seal layer is below the above upper limit, it is easy to obtain more excellent low-temperature sealing. From these viewpoints, the thickness of the heat seal layer can be 8 to 25%, 10 to 25%, 8 to 21% or 10 to 21% based on the thickness of the multilayer film. The thickness of the heat seal layer can be, for example, 5 to 20 μm.
[0090] The thickness of the concealing layer can be 20 μm or more from the perspective of better balancing concealment and cold impact resistance. From this perspective, the thickness of the concealing layer can be 25 μm or more, 30 μm or more, 35 μm or more, or 40 μm or more. The upper limit of the thickness of the concealing layer is not particularly limited, but it can be set to 60 μm or less or 50 μm or less because it becomes a cost disadvantage.
[0091] The thickness of the concealing layer may be 50 to 92% based on the thickness of the multilayer film from the viewpoint of better balancing concealment and cold impact resistance. The thickness of the concealing layer may be 58%, 60%, 65%, 70%, 75%, or 79% based on the thickness of the multilayer film, and may be 90%, 84%, 80%, or 85% or less.
[0092] When the laminated layer is provided, the total thickness of the heat seal layer and the laminated layer can be 16% or more, 20% or more, or 25% or more based on the thickness of the multilayer film, and can be 42% or less, 40% or less, or 35% or less. When the ratio of the total thickness of the heat seal layer and the laminated layer is above the above lower limit, it is easy to obtain more excellent cold impact resistance. In addition, when the ratio of the total thickness of the heat seal layer and the laminated layer is below the above upper limit, it is easy to obtain more excellent low-temperature sealing. From these viewpoints, the total thickness of the heat seal layer and the laminated layer can be 16-42%, 20-40%, or 25-35% based on the thickness of the multilayer film. The total thickness of the heat seal layer and the laminated layer can be, for example, 10-40 μm.
[0093] The method for manufacturing the above-mentioned multilayer film is not particularly limited, and a known method can be used. For example, as a method for thermoforming processing, a melt kneading method using a common mixer such as a single-axis screw extruder, a twin-axis screw extruder, and a multi-axis screw extruder can be cited; a method of removing the solvent by heating after dissolving or dispersing and mixing each component, etc. Considering operability, a single-axis screw extruder or a twin-axis screw extruder can be used. When using a single-axis extruder, as a screw, a full-thread screw, a screw with a mixing element, a separation type screw, a groove screw, etc. can be cited, and they can be used without particular restrictions. As a twin-axis kneading device, a co-rotating twin-axis screw extruder, a counter-rotating twin-axis screw extruder, etc. can be used. In addition, as a screw shape, a full-thread screw, a kneading disk type, etc. can be used without particular restrictions.
[0094] Among the above methods, a method of forming a film by using a feed block or a multi-channel T-die after melting a multi-layer film by using a single screw extruder or a twin screw extruder can be used.
[0095] The obtained multilayer film may also be subjected to a surface modification treatment to improve the adaptability of the subsequent process as required. For example, in order to improve the printing adaptability when the monomer film is used or the lamination adaptability when it is used in a stacked manner, the printed surface or the surface in contact with the substrate may be subjected to a surface modification treatment. Examples of surface modification treatments include treatments such as corona discharge treatment, plasma treatment, and flame treatment to oxidize the film surface to generate functional groups; and modification treatments using a wet process to form an easy-adhesion layer by coating.
[0096] The multilayer film of the present invention has been described above, but the multilayer film of the present invention is not limited to the above-mentioned embodiments. For example, the multilayer film may also have other layers besides the heat-sealing layer, the concealing layer and the laminating layer. Among them, from the viewpoint of using the multilayer film in a packaging material of a single material composed of the same raw materials of the polypropylene system and obtaining a better low-temperature sealing property, it is preferred that the propylene content in the multilayer film (based on the total mass of the multilayer film) is 70% by mass or more. In addition, the propylene content in the multilayer film can be measured according to Raman spectroscopy.
[0097] <Packaging materials>
[0098] Another embodiment of the present disclosure relates to a packaging material having a multilayer film. The multilayer film used in the packaging material is characterized in that it has a heat seal layer and a concealing layer arranged on the heat seal layer, the heat seal layer comprises a propylene homopolymer (A) and / or a propylene copolymer resin (B), the concealing layer comprises a propylene-ethylene block copolymer resin (C), an ethylene-propylene copolymer elastomer (D), and titanium oxide (E), and the content of titanium oxide (E) in the concealing layer is 0.10 to 30.00% by mass based on the total mass of the concealing layer. The multilayer film can be the multilayer film of the above embodiment. The packaging material can be formed only by the multilayer film, or it can be provided with a multilayer film and a substrate.
[0099] The packaging material with a multilayer film and a substrate can be obtained by, for example, forming a laminate by laminating at least one layer of biaxially stretched polyamide film (ONy), biaxially stretched polyester film (PET), biaxially stretched polypropylene film (OPP), printing paper, metal foil (AL foil), transparent vapor-deposited film and other substrates on the multilayer film. The substrate can be arranged on the side opposite to the above-mentioned heat-sealing layer side from the concealing layer of the multilayer film. From the viewpoint of making the packaging material a packaging material of a single material (single raw material packaging material), a biaxially stretched polypropylene film (OPP) is preferably used as a substrate. In other words, the packaging material can be a single raw material packaging material with a biaxially stretched polypropylene film and a multilayer film. In the past, when giving concealment to the packaging material, an aluminum substrate was used, but the packaging material of the present embodiment has the above-mentioned multilayer film, so even if a substrate with concealment such as an aluminum substrate is not used, it also has sufficient concealment.
[0100] When the packaging material is a laminate, the layer composition is not particularly limited and can be appropriately adjusted according to the required characteristics of the packaging body, such as barrier properties that meet the shelf life of the packaged food, size / impact resistance that can cope with the weight of the contents, visibility of the contents, etc. The packaging material can be, for example, Figure 3 The packaging material 100 shown in the figure comprises a multilayer film 10, an adhesive layer 4, a transparent vapor-deposited film 5, an adhesive layer 6, and a substrate (substrate film) 7 in order. The multilayer film 10 comprises a heat-sealing layer 1 and a concealing layer 2 in order from the outer layer side of the packaging material 100. That is, the concealing layer 2 is located on the inner layer side relative to the heat-sealing layer 1. The packaging material may also be, for example, Figure 4The packaging material 101 shown in the figure comprises a multilayer film 11, an adhesive layer 4, a transparent vapor-deposited film 5, an adhesive layer 6, and a substrate (substrate film) 7 in sequence. The multilayer film 11 comprises a heat seal layer 1, a concealing layer 2, and a laminating layer 3 in sequence from the outer layer side of the packaging material 101. That is, the concealing layer 2 and the laminating layer 3 are located on the inner layer side relative to the heat seal layer 1. These packaging materials (100, 101) are used in such a manner that the multilayer film (10, 11) side becomes the content side.
[0101] The manufacturing method of the packaging material (100, 101) can preferably adopt the conventional dry lamination method of using an adhesive to stick on the film constituting the packaging material (100, 101), and can also adopt a method of directly extruding and laminating a multilayer film on a substrate as needed.
[0102] <Packaging>
[0103] Another embodiment of the present disclosure relates to a package made of a packaging material. The packaging material used in the package has a multilayer film, which is characterized in that it has a heat seal layer and a concealing layer arranged on the heat seal layer, the heat seal layer contains a propylene homopolymer (A) and / or a propylene copolymer resin (B), and the concealing layer contains a propylene-ethylene block copolymer resin (C), an ethylene-propylene copolymer elastomer (D), and titanium oxide (E), and the content of titanium oxide (E) in the concealing layer is 0.10 to 30.00% by mass based on the total mass of the concealing layer. The packaging material can be the packaging material implemented above.
[0104] The bagging style of the packaging body is not particularly limited. For example, the packaging body can be a flat bag, a three-side sealed bag, a gas-seal bag, a gusseted bag, a self-supporting bag, a bag with a nozzle, a spout bag, etc., using the above-mentioned multilayer film of the packaging material as a sealing material.
[0105] Example
[0106] The present disclosure will be described in more detail below using examples and comparative examples, but the present disclosure is not limited to the following examples.
[0107] <Material preparation>
[0108] The following propylene homopolymer (A), propylene copolymer resin (B), propylene-ethylene block copolymer resin (C), and ethylene-propylene copolymer elastomer (D) were prepared. The melting start temperature and melting point of the materials shown below are values obtained by differential scanning calorimetry according to JIS K7121. The melt flow rate is a value measured under the conditions of a temperature of 230°C and a load of 2.16 kg according to ISO 1133. The ethylene content was measured according to the quantitative method (IR method) of ethylene content described on pages 412 to 413 of the Polymer Analysis Handbook compiled by the Polymer Analysis Forum of the Japan Analytical Society (May 10, 2013, 3rd edition) (The Polymer Analysis Handbook compiled by the Polymer Analysis Forum of the Japan Analytical Society (May 10, 2013, 3rd printing)). The propylene content of the materials shown below was measured according to Raman spectroscopy.
[0109] (Propylene homopolymer (A))
[0110] Resin (A): A propylene homopolymer having a melting start temperature of 153°C, a melting point (melting peak temperature) of 159°C and a melt flow rate of 3.0 g / 10 min.
[0111] (Propylene copolymer resin (B))
[0112] Resin (B1): A propylene-ethylene random copolymer having a melting start temperature of 142°C, a melting point (melting peak temperature) of 147°C, a melt flow rate of 7.5 g / 10 min, and an ethylene content of 3.4% by mass.
[0113] Resin (B2): A propylene-ethylene random copolymer having a melting start temperature of 122°C, a melting point (melting peak temperature) of 133°C, a melt flow rate of 7.0 g / 10 min, and an ethylene content of 5.8% by mass.
[0114] Resin (B3): A propylene-ethylene random copolymer having a melting start temperature of 120°C, a melting point (melting peak temperature) of 131°C, a melt flow rate of 6.5 g / 10 min, and an ethylene content of 23.7% by mass.
[0115] (Propylene-ethylene block copolymer resin (C))
[0116] Resin (C): A propylene-ethylene block copolymer resin having a melt flow rate of 1.8 g / 10 min, comprising 81.5% by mass of a propylene homopolymer component (c1) and 18.5% by mass of an ethylene-propylene copolymer component (c2), wherein the ethylene content of the ethylene-propylene copolymer component (c2) is 36.2% by mass.
[0117] (ethylene-propylene copolymer elastomer (D))
[0118] Elastomer (D): an ethylene-propylene copolymer elastomer having a melt flow rate of 0.6 g / 10 min and a mass ratio of propylene content to ethylene content [propylene content / ethylene content] of 2.7.
[0119] (Titanium oxide (E))
[0120] Titanium oxide PEONY HP WHITE series manufactured by DIC Corporation Model: L-11232-MPT
[0121] <Example 1>
[0122] (Production of laminated film)
[0123] In order to form a heat seal layer, 50% by mass of resin (A) as a propylene homopolymer (A) and 50% by mass of resin (B1) as a propylene copolymer resin (B) were mixed in a pellet state to prepare a mixture (I). In addition, in order to form a concealing layer, resin (C) as a propylene-ethylene block copolymer resin (C) and elastomer (D) as an ethylene-propylene copolymer elastomer (D) were mixed in a pellet state so that the mass ratio of elastomer (D) to resin (C) (ratio [elastomer (D) / resin (C)]) was 0.20 to prepare a mixture (II), and the mixture (II) and titanium oxide (E) were mixed so that the content of titanium oxide (E) in the whole was 11.25% by mass to prepare a mixture (III).
[0124] The mixture (I) and the mixture (III) were supplied to an extruder whose temperature was adjusted to 250° C., kneaded in a molten state, and laminated using a T-die extruder with a feed block so that the thickness of the heat seal layer reached 15 μm and the thickness of the concealing layer reached 45 μm to produce the film of Example 1. The propylene content in the heat seal layer and the propylene content in the concealing layer in the obtained film were both 70% by mass or more.
[0125] <Examples 2 to 4>
[0126] Films of Examples 2 to 4 were prepared in the same manner as in Example 1 except that the mixing ratio of the resin (A) to the resin (B1) in the mixture (I) was changed as shown in Table 1. The propylene content in the heat seal layer and the propylene content in the concealing layer of the obtained films were both 70% by mass or more.
[0127] <Example 5>
[0128] The film of Example 5 was prepared in the same manner as in Example 1 except that the mixing ratio of the resin (C) and the elastomer (D) in the mixture (II) (ratio [elastomer (D) / resin (C)]) was changed as shown in Table 1. The propylene content in the heat seal layer and the propylene content in the concealing layer of the obtained film were both 70% by mass or more.
[0129] <Examples 6 and 7>
[0130] Films of Examples 6 and 7 were prepared in the same manner as in Example 5 except that the mixing ratio of titanium oxide (E) in the mixture (III) was changed as shown in Table 1. The propylene content in the heat seal layer and the propylene content in the concealing layer of the obtained films were both 70% by mass or more.
[0131] <Example 8>
[0132] A film of Example 8 was prepared in the same manner as in Example 1 except that the resin (B2) was used instead of the resin (B1). The propylene content in the heat seal layer and the propylene content in the concealing layer of the obtained film were both 70% by mass or more.
[0133] <Examples 9 and 10>
[0134] Films of Examples 9 and 10 were prepared in the same manner as in Example 8, except that the mixing ratio of the resin (A) and the resin (B2) in the mixture (I) was changed as shown in Table 2. The propylene content in the heat seal layer and the propylene content in the concealing layer of the obtained films were both 70% by mass or more.
[0135] <Example 11>
[0136] The film of Example 11 was prepared in the same manner as in Example 1 except that the resin (A) was used alone instead of the mixture (I) to form the heat seal layer (i.e., the resin (B1) was not used). The propylene content in the heat seal layer and the propylene content in the concealing layer of the obtained film were both 70% by mass or more.
[0137] <Example 12>
[0138] The film of Example 12 was prepared in the same manner as in Example 1 except that the resin (B1) was used alone instead of the mixture (I) to form the heat seal layer (i.e., the resin (A) was not used). The propylene content in the heat seal layer and the propylene content in the concealing layer of the obtained film were both 70% by mass or more.
[0139] <Example 13>
[0140] A film of Example 13 was prepared in the same manner as in Example 3 except that resin (B3) was used instead of resin (B1). The propylene content in the heat seal layer and the propylene content in the concealing layer of the obtained film were both 70% by mass or more.
[0141] <Example 14>
[0142] The film of Example 14 was prepared in the same manner as in Example 1 except that the thicknesses of the heat seal layer and the concealing layer were changed as shown in Table 2. The propylene content in the heat seal layer and the propylene content in the concealing layer of the obtained film were both 70% by mass or more.
[0143] <Comparative Example 1>
[0144] A film of Comparative Example 1 was prepared in the same manner as in Example 1 except that the resin (C) was used instead of the mixture (II) to prepare the mixture (III) (ie, the elastomer (D) was not used).
[0145] <Comparative Example 2>
[0146] A film of Comparative Example 2 was prepared in the same manner as in Example 1 except that the mixture (II) was used instead of the mixture (III) to form the concealing layer (ie, titanium oxide (E) was not used).
[0147] <Example 15>
[0148] As in Example 1, a mixture (I) was prepared to form a heat seal layer, and a mixture (III) was prepared to form a concealing layer. In addition, a mixture (IV) having the same composition as the mixture (I) for forming the heat seal layer was prepared to form a laminating layer.
[0149] The mixture (I), mixture (III) and mixture (IV) were supplied to an extruder adjusted to 250°C, kneaded in a molten state, and laminated using a T-die extruder with a feed block so that the thickness of the heat seal layer and the laminating layer were 10 μm and the thickness of the concealing layer was 40 μm, respectively, to produce a film of Example 15. The propylene content in the heat seal layer, the propylene content in the concealing layer and the propylene content in the laminating layer in the obtained film were all 70% by mass or more.
[0150] <Examples 16, 17, 23 and 24>
[0151] Films of Examples 16, 17, 23 and 24 were prepared in the same manner as in Example 15, except that the mixing ratio of the resin (A) to the resin (B1) in the mixture (I) and the mixture (IV) was changed as shown in Table 3. The propylene content in the heat seal layer, the propylene content in the concealing layer and the propylene content in the laminating layer in the obtained films were all 70% by mass or more.
[0152] <Example 18>
[0153] The film of Example 18 was prepared in the same manner as in Example 15 except that the mixing ratio of the resin (C) and the elastomer (D) in the mixture (II) (ratio [elastomer (D) / resin (C)]) was changed as shown in Table 3. In the obtained film, the propylene content in the heat seal layer, the propylene content in the concealing layer, and the propylene content in the laminating layer were all 70% by mass or more.
[0154] <Examples 19 to 22 and Comparative Example 3>
[0155] Films of Examples 19 to 22 and Comparative Example 3 were prepared in the same manner as in Example 18, except that the mixing ratio of titanium oxide (E) in the mixture (III) was changed as shown in Table 3. The propylene content in the heat seal layer, the propylene content in the concealing layer, and the propylene content in the laminating layer of the obtained films were all 70% by mass or more.
[0156] <Various Reviews>
[0157] The following evaluations were performed on the films obtained in each example. The results are shown in Tables 1 to 3.
[0158] [Evaluation of cold impact resistance]
[0159] The impact strength of the film obtained in each example during low temperature storage was measured using a film impact tester manufactured by Toyo Seiki Co., Ltd. at a temperature of -5°C, an impact energy of 1.5 J, and an impact head size of 1 / 2 inch. When the impact strength (film impact) was 6.00 J / mm or more, it was judged to be excellent in cold impact resistance.
[0160] [Concealment]
[0161] The concealing property of the film obtained in each example was evaluated using a portable transmission density meter (Model 341C) manufactured by X-RITE Co., Ltd. When the measured transmission density was 0.20 or more, it was determined that sufficient concealing property was obtained.
[0162] [Evaluation of low temperature sealing performance]
[0163] A laminate having the following structure was prepared by using a urethane adhesive and a conventional dry lamination method to adhere a biaxially stretched polyester film (PET) having a thickness of 12 μm, an AL foil having a thickness of 9 μm, a biaxially stretched polyamide film (ONy) having a thickness of 15 μm, and the film obtained in each example (polypropylene film).
[0164] Laminated structure: PET / adhesive / AL foil / adhesive / ONy / adhesive / polypropylene film
[0165] The film of each example was bonded to ONy so that the heat seal layer was located on the outer layer side (outermost layer of the laminate).
[0166] Prepare 2 laminates obtained above, and use a heat sealer manufactured by Tester Industry Co., Ltd. to heat seal the polypropylene films of these laminates to each other at a sealing temperature of 140°C to 160°C at 5°C scales under the conditions of a sealing pressure of 0.2MPa, a sealing time of 1 second, and a sealing width of 5mm. After heat sealing at each temperature, cut the sealed portion into 15mm wide × 80mm, and measure the heat seal strength using a tensile testing machine manufactured by Shimadzu Corporation at a tensile speed of 300mm / min. The lower the temperature (sealing temperature) at which the heat seal strength reaches 40N / 15mm or more, the better the low-temperature sealing property is judged to be. In addition, the sealing temperatures shown in Tables 1 to 3 are the temperatures at which the heat seal strength reaches 40N / 15mm or more.
[0167] [Heat resistance evaluation]
[0168] The film obtained in each example was used to make a bag of 130 mm × 180 mm, and the inner surfaces of the bag were directly sealed without putting the contents, and the bag was retorted at 135°C for 40 minutes. After that, the sealed parts on the three sides were cut, and the film was peeled off by hand, and the melt adhesion after retorting was evaluated. The film was evaluated as A if it was easy to peel off, B if it felt sticky, and C if the film was deformed when peeled off.
[0169]
[0170]
[0171]
[0172] Explanation of symbols
[0173] 1 heat sealing layer, 2 concealing layer, 3 laminating layer, 4 adhesive layer, 5 transparent vapor-deposited film, 6 adhesive layer, 7 base film, 10, 11 multilayer film, 100, 101 packaging material.
Claims
1. A multilayer film comprising: Heat seal layer; and A concealing layer is provided on the heat sealing layer, in, The heat seal layer comprises a propylene homopolymer (A) and / or a propylene copolymer resin (B), The concealing layer comprises a propylene-ethylene block copolymer resin (C), an ethylene-propylene copolymer elastomer (D), and titanium oxide (E). The content of the titanium oxide (E) in the concealing layer is 0.10 to 30.00% by mass based on the total mass of the concealing layer.
2. The multilayer film according to claim 1, wherein The heat seal layer comprises a propylene copolymer resin (B), The melting point of the propylene copolymer resin (B) is 132 to 150°C.
3. The multilayer film according to claim 1, wherein The heat seal layer comprises a propylene copolymer resin (B), The ethylene content in the propylene copolymer resin (B) is 3.0 to 6.0% by mass based on the total mass of the propylene copolymer resin (B).
4. The multilayer film according to any one of claims 1 to 3, wherein The content of the propylene homopolymer (A) in the heat seal layer is 10 to 70% by mass based on the total mass of the heat seal layer. The content of the propylene copolymer resin (B) in the heat seal layer is 30 to 90% by mass based on the total mass of the heat seal layer.
5. The multilayer film according to any one of claims 1 to 3, wherein The mass ratio of the content of the propylene-based copolymer resin (B) to the content of the propylene homopolymer (A) in the heat seal layer is 0.10 to 9.
00.
6. The multilayer film according to any one of claims 1 to 3, wherein The content of the propylene-ethylene block copolymer resin (C) in the concealing layer is 35 to 90% by mass based on the total mass of the concealing layer. The content of the ethylene-propylene copolymer elastomer (D) in the concealing layer is 10 to 50% by mass based on the total mass of the concealing layer.
7. The multilayer film according to any one of claims 1 to 3, wherein The mass ratio of the content of the ethylene-propylene copolymer elastomer (D) to the content of the propylene-ethylene block copolymer resin (C) in the concealing layer is 0.10 to 1.
00.
8. The multilayer film according to any one of claims 1 to 3, wherein The propylene content is 70% by mass or more based on the total mass of the multilayer film.
9. The multilayer film according to any one of claims 1 to 3, wherein The thickness of the heat-sealing layer is 8 to 30% based on the thickness of the multi-layer film.
10. The multilayer film according to any one of claims 1 to 3, wherein The concealing layer has a thickness of 20 μm or more.
11. The multilayer film according to any one of claims 1 to 3, It comprises the heat seal layer, the concealing layer, and the laminating layer in sequence, The lamination layer contains a propylene homopolymer (A) and / or a propylene-based copolymer resin (B).
12. The multilayer film according to claim 11, wherein The total thickness of the heat-sealing layer and the laminating layer is 16 to 42% based on the thickness of the multi-layer film. 13 . A packaging material comprising the multilayer film according to claim 1 .
14. The packaging material according to claim 13, wherein The multilayer film further includes a biaxially stretched polypropylene film on the side opposite to the heat seal layer side when viewed from the concealing layer.
15. A package body made from the packaging material according to claim 14.
Citation Information
Patent Citations
Film, laminate and package
CN1852804A
Package
JP2003312718A
Light barrier film, laminate and container
JP2006212785A
Biaxially stretched multilayered propylene polymer film
JP2007044930A
Light-shielding polypropylene-based sealant film and laminate thereof
JP2020049898A