Slurry, electrode and method for manufacturing electrode for lithium ion battery
Through a water-based adhesive system with high Ni content and electrochemically activated compounds, the problems of flammable and highly toxic materials in lithium-ion batteries are solved, the stability and energy density of the electrode are improved, the cost is reduced, and the cost is achieved is achieved. A more environmentally friendly manufacturing process.
Patent Information
- Application Number
- CN202380025429.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-04
- Filing Date
- 2023-03-03
- Publication Date
- 2024-11-05
AI Technical Summary
Existing lithium-ion batteries have challenges in improving energy density, safety, cost and charging speed, especially due to problems with flammable electrolytes and highly toxic materials.
Using a high Ni content water-based binder system and electrochemically activated compounds, Ni-rich and Li-rich cathode materials are prepared by adjusting the pH value of the slurry in the range of 9 to 10.5 to reduce the cobalt content. Improve the cohesive adhesion and chemical stability of the electrodes and replace traditional organic solvents with an environmentally friendly water-based adhesive.
The cycle stability and energy density of the electrode are significantly improved, manufacturing costs are reduced, the safety and recyclability of the battery are enhanced, while reducing the total adhesive content and PVdF content in the electrode.
Smart Images

Figure CN118901149A_ABST
Abstract
Description
[0001] The present invention relates to a slurry for making electrodes for lithium-ion cells, an electrode made with the slurry, and a method for making an electrode for a lithium-ion battery (LIB).
[0002] As a rechargeable battery, LIB plays a vital role in today's transition to sustainable energy production and consumption. For many years, LIB has been widely used in portable electronics and electric vehicles, and is increasingly being used in large-scale energy storage applications in trains, marine and aviation applications, as well as in wind and solar parks.
[0003] In batteries, lithium ions move from the negative electrode through the electrolyte to the positive electrode during discharge and vice versa during charging. LIBs use intercalated lithium ions as the positive electrode material and usually graphite as the negative electrode.
[0004] LIBs have high energy density, no memory effect, and low self-discharge. However, they can be a safety hazard because they contain flammable electrolytes that can cause explosions and fires if damaged or charged incorrectly.
[0005] Different types of LIBs have different chemical properties, performance, cost and safety characteristics. The concept of rechargeable lithium-ion batteries can be traced back to 1980, when lithium cobalt oxide (LiCoO2) was first introduced as an active material in the cathode. Due to the high toxicity, high cost and thermal instability of Co, the general trend is to partially or completely replace Co with other metals, such as reducing the cobalt content by increasing the Ni / metal ratio, thereby increasing the capacity (JB Goodenough, Y. Kim (2010), Chemistry of Materials 22, 587-603). LiNiMnCoO2 or NMC stands for lithium nickel (Ni) manganese (Mn) cobalt (Co) dioxide (LiNiMnCoO2), or simply lithium metal dioxide (LiMeO2), where the metal is represented by a certain proportion or ratio of Ni, Mn and Co. This is the most common cathode material for commercial lithium-ion battery cells, with the same structure as LiCoO2, where Ni:Mn:Co=1:1:1 (NMC111, equimolar metal content). Graphite-based cells using LCO, NMC 111 or conventional LiFePO4 (LFP) as cathode materials can achieve energy densities of 120-160Wh / kg. Today, large cells need to deliver energy densities in excess of 200Wh / kg. In order to meet market demands for lithium-ion batteries (LIBs), significant increases in energy density and / or power density at the cell level are required. On the cathode side, this can be achieved in a number of ways:
[0006] - Introduction of high capacity electrode materials (e.g. Ni-rich NMC, layered oxides, Li-rich layered oxides for use as positive electrode materials, cathode materials); and
[0007] -Introduction of high voltage cathode (>4.6V relative to metallic lithium) materials, such as high voltage LiNi 0.5 Mn 1.5 O2-, high nickel LiNi 1-x-y Mn x Al y O2(NMA) and / or olivine high voltage LiCoPO4 cathode.
[0008] As a binder material for LIB electrodes, the polymer currently widely used is PVdF (polyvinylidene fluoride).
[0009] Currently, the challenges facing LIBs are to improve lifespan, energy density, safety, cost, and increase charging speed. Development focuses on topics such as non-flammable electrolytes, which are ways to improve safety based on the flammability and volatility of organic solvents used in typical electrolytes. Strategies include aqueous lithium-ion batteries, ceramic solid electrolytes, polymer electrolytes, ionic liquids, and heavy fluorinated systems.
[0010] To realize more environmentally friendly and less toxic LIBs, aqueous binder-based cathodes with superior electrochemical performance, such as lithium nickel manganese cobalt oxide (LiNiMnCoO2)-NMC, lithium nickel cobalt aluminum oxide (LiNiCoAlO2)-NCA or high voltage LiNi 0.5 Mn 1.5 O4 electrode.
[0011] NMC, or lithium nickel manganese cobalt oxide (LiNiMnCoO2), is one of the most successful lithium-ion systems for cathodes. Similar to Li-manganese, these systems can be tailored to be energy cells or power cells. For example, under moderate load conditions, the capacity of NMC in an 18650 cell is about 2,800mAh and can provide a current of 4A to 5A; the capacity of NMC in the same cell optimized for a specific power is only about 2,000mAh, but can provide a continuous discharge current of 20A. Silicon-based anodes will reach 4,000mAh or more, but with reduced load capacity and shortened cycle life. The disadvantage of silicon added to graphite is that the anode will expand and contract with charging and discharging, making the battery cell mechanically unstable.
[0012] The secret of NMC is to combine nickel, cobalt and manganese. A similar example is table salt, where the main components sodium and chloride are toxic on their own, but when mixed together they can be used as a seasoning salt and food preservative. Nickel is known to have high specific energy but poor stability; manganese has the advantage of forming a spinel structure to achieve low internal resistance, but has low specific energy. Combining the metals can enhance each other's advantages.
[0013] NMC is the battery material of choice for power tools, e-bikes, and other electric powertrains. The cathode combination is typically one-third nickel, one-third manganese, and one-third cobalt in the metal (LiMeO2), also known as 1-1-1. This provides a unique blend that also reduces raw material costs due to the reduced cobalt content. Another successful combination is NCM532, which has 5 parts nickel, 3 parts cobalt, and 2 parts manganese (5-3-2). Other combinations using different amounts of cathode materials are also possible.
[0014] Due to the high cost of cobalt, battery manufacturers are switching from cobalt systems to high nickel content cathodes. Nickel-based systems have higher energy density, lower cost and longer cycle life than cobalt-based battery cells, but they have slightly lower voltage.
[0015] Lithium nickel cobalt aluminum oxide (LiNiCoAlO2) - Batteries containing NCA cathode materials were developed around 1999 for special applications. Batteries based on NCA cathodes have similarities to NCM cathode batteries: they have high specific energy, fairly good specific power, and long life, but are considered less economical and expensive. Aluminum is added to the chemical composition to improve stability.
[0016] High Voltage (LiNi 0.5 Mn 1.5 O4)-LNMO cathodes are expected to be used in next-generation high-performance lithium-ion batteries due to their high energy density, high operating voltage (~4.7 V relative to lithium), low manufacturing cost, and small environmental impact. However, the shortened cycle life of LNMO due to the rapid capacity decay during cycling remains a challenge.
[0017] Compared with conventional organic PVdF-based electrodes, the NCM, NCA, and LNMO electrodes have very uniform carbon particle distribution and strong adhesion between particles and between particles and current collector, which significantly mitigates crack formation and delamination of the electrodes during repeated delithiation / lithiation. In addition, these electrodes have enhanced Li + Diffusion dynamics, reduced polarization, and thus excellent high C-rate capability, and extremely stable cycling performance even at elevated temperatures such as >50°C. They also have the advantages of low cost, environmental protection, and easy handling and recycling.
[0018] Despite the progress in aqueous binder-based cathodes for lithium-ion batteries, there are still urgent needs to achieve sustainable lithium-ion batteries:
[0019] - avoid and / or reduce the PVdF content in the electrodes,
[0020] - reduce the total binder content in the electrode,
[0021] - Enhanced lamination between separator and electrodes made from aqueous solutions,
[0022] - Enhance the cohesive bonding between particles within the electrode structure,
[0023] - Improve the chemical and electrochemical stability of the cathode,
[0024] - Improve battery cell safety by using more stable water-based adhesives,
[0025] - Enhance the adhesion between the electrode mass and the current collector,
[0026] - Improve the recyclability of electrode materials and last but not least
[0027] - Reduce manufacturing costs.
[0028] These objects are achieved by providing a slurry, a method for producing an electrode, an electrode and a battery containing said electrode, wherein elements, compositions and method steps are according to the independent claims, while preferred embodiments are described by elements, compositions and method steps according to the claims dependent thereon.
[0029] The present invention proposes a slurry for manufacturing electrodes for lithium-ion battery cells, wherein the slurry is a composite composed of: a water-based binder system, i.e., a mixture of one or more polymer binders dissolved in an aqueous solution; and an electrochemically activatable compound, i.e., a cathode material that converts electrical and chemical potentials through an electrochemical insertion reaction, wherein the electrochemically activatable compound has a Ni-containing Li metal oxide (also called a Ni-rich oxide) and a Li-rich oxide (i.e., a cathode material containing more Li than a conventional stoichiometric 1:1 LiMeO2-oxide compound), wherein the Ni content in the metal (LiMeO2) is at least 80 wt%, and wherein the pH value of the slurry is adjusted to 9 to 10.5.
[0030] An example of a lithium-rich layered oxide cathode material is Li 1.2 Mn 0.5100 Ni 0.2175 Co 0.0725 O2.
[0031] The technical advantage of using at least >80% Ni content in the metal over using lesser amounts of Ni is increased capacity due to reduced cobalt content in the cathode material and reduced cost.
[0032] In order to be able to use Ni contents of at least >80% in the metal (LiMeO2) to obtain a properly functioning battery cell, the recipe and steps of the mixing process must be adjusted to control the pH of the resulting slurry within a specific range of 9 to 10.5 in order to control the surface reactivity of the material, which is higher than that of cathode materials with low Ni contents.
[0033] Proper stabilization of Li-NMC slurries with a Ni content of at least 80% in the metal (LiMeO2) by strictly controlling the pH value of the slurry according to the present invention within the range between 9 and 10.5 will result in improved cohesive bonding between the particles within the electrode structure, resulting in significantly more stable electrodes.
[0034] Cathode active materials with high Ni content for Li-ion electrodes can have very high pH (pH>11.5) during slurry processing. Water-based slurries with higher pH are process critical due to corrosion reactions or / and agglomeration of active materials with conductive materials. High or uncontrolled pH can also lead to binder gelation. To avoid this behavior with water-based binder slurries, slurry pH control is also critical.
[0035] The pH of the prepared binder solution can be adjusted from acidic to neutral to alkaline, for example, by adding acrylates (polyacrylic acid (PAA), polyethylene-co-acrylic acid (PEAA), etc.), phosphoric acid, citric acid, LiH2SO4, LiH2PO4, ammonia, etc. A preferred method of using such a pH adjuster (buffer solution) compound in an electrode paste is to make the compound also binder and use it as a thickener for the prepared slurry solution.
[0036] For example, because acrylates contain acidic groups, they can correct (lower) the high pH of solutions containing higher pH materials and reduce the very high interfacial free energy between active and inactive particles, especially when using carbon black particles, which are known to be hydrophobic, as the conductive material. The acrylic acid groups also enhance the surface reaction with the current collector, thereby providing high adhesion of the electrode particles to the current collector. The first choice for lowering the pH and improving electrode adhesion is PAA (polyacrylic acid), which is used as both a binder and a pH adjuster.
[0037] For the water-based binder slurry according to the present invention, the binder combination is used in such a way that the pH of the slurry can be controlled and the active surfaces of the active cathode material and the conductive material are protected from electrolytic corrosion and electrochemical decomposition on the active material surface.
[0038] By coating the electrode with a pH controlled slurry (pH = 9-10.5), corrosion of the (aluminum) current collector can be avoided.
[0039] Higher Ni content in LiMe oxide also enhances the capacity (Ah / kg) of cathode materials used as Li-ion batteries. For example, NCM111 has a capacity of about 150 Ah / kg, while NCM cathode materials containing more than 80% Ni have a capacity of more than 190 Ah / kg.
[0040] Furthermore, this allows the electrode (cathode) to be manufactured with an environmentally friendly water-based adhesive, the electrode prepared with the water-based adhesive to be laminated to the separator, improving the interfacial stability and reducing the risk of dendrite formation. The Ni-rich cathode manufactured according to the present invention shows good chemical and electrochemical cycling stability.
[0041] In a preferred embodiment, the electrochemically activatable compound may be selected from: NCM type, NCA type, NCMA type (nickel cobalt manganese aluminum oxide) and high voltage Li-NMO (LiNi 0.5 Mn 1.5 O4) type.
[0042] The technical advantage of using NCMA type is that it has high capacity and low cost due to higher nickel content and lower cobalt content compared to NCM type or NCA type. In addition, NCMCA type has improved cycle stability compared to NCM type.
[0043] In equally preferred embodiments of the electrode according to the invention, the PVdF content of the water-based binder (WBB) system may be chosen between 0% and 2%, with 0.5% to 1%, 1% to 2% or even 0% being more preferred embodiments.
[0044] All % values in this application are given as weight percent.
[0045] In order to be able to laminate the separator to the electrode prepared from a water-based solution, the most preferred binder content is 3-4%. This enables a stable interface to be formed between the separator and the electrode and improves the safety of the battery cell. However, lamination is not necessary in the processing of WBB electrodes. The purpose of lamination is to make the separator more uniform and enhance the stability within the battery cell, which helps to form a uniform solid electrolyte interface (SEI) on the interface anode / separator. Due to the improvement in SEI formation on the anode side, the degree of degradation of the battery cell during cycling is lower. Due to the different chemical interfacial interactions between the active material and the water-based binder, higher reversible insertion / deintercalation is achieved compared to PVdF binder electrodes, improving the chemical stability and electrochemical stability of the cathode.
[0046] In the case where no lamination is performed, lower levels of adhesive are preferred, with the most preferred WBB content being 2-3%.
[0047] The technical advantage of using a WBB amount of 2-3% is to increase the energy density of the battery cell, while increasing the power density (battery cell power performance) due to less segregation of active material particles due to the large binder content.
[0048] The water-based binder system is preferably a binder system based on carboxymethyl cellulose (CMC), a styrene-butadiene rubber (SBR) binder system or an acrylic-based binder system. WBB, such as CMC-based, SBR-based and / or acrylic-based binders, exhibits a higher binding capacity than PVdF binders, enhances the adhesion between the electrode block and the current collector and the cohesive adhesion between the particles, thereby making it possible to manufacture electrodes with a lower binder amount.
[0049] The absence of organic solvents makes the process more environmentally friendly, which in turn reduces manufacturing costs. Environmental protection is given high priority at every stage of the product life cycle: it is characterized by saving resources through the reduction of waste during manufacturing, the use of separation technologies in all areas of chemical processing, water / gas treatment through systematic recycling and recovery of raw materials.
[0050] The battery cell assembly method starts with electrode manufacturing based entirely on a water-based binder (WBB) method, which improves the manufacturing environment by eliminating expensive and toxic organic solvents. NMP and / or acetone are widely used as solvents for electrode preparation in lithium-ion battery manufacturing, but efforts have been made to replace it with solvents with less environmental impact, such as water. Unlike chemical solvents used in traditional industrial coatings that must be recovered or burned afterwards, water does not require recovery, steam removal or ATEX (Controlled Explosive Atmospheres) treatment lines. Therefore, the machinery is simplified as there is no potential risk from explosive environments. In addition, NMP was included in the list of substances of very high concern that may cause serious and irreversible harm to human health and the environment in April 2018. The use of NMP has been restricted by the European Commission (Restriction entry 71 of REACH Annex XVII): NMP “After May 9, 2020, the substance itself, or mixtures containing it in a concentration equal to or greater than 0.3% shall not be produced or used unless producers and downstream users take appropriate risk management measures and provide appropriate operating conditions to ensure that workers’ exposure levels are below the presumed no effect level (DNEL), i.e. exposure by inhalation below 14.4 mg m -3 , skin exposure is less than 4.8 mg kg -1 / day, which means additional costs for the electrode processing chain from mixing the slurry to the final solvent recovery.
[0051] The water-based binder in the slurry used to make the electrode according to the present invention can be selected from carboxymethyl cellulose (CMC) binder, styrene butadiene rubber (SBR) binder, acrylic binder or a mixture thereof. Using a more stable water-based binder can improve battery cell safety.
[0052] Polyvinylidene fluoride (PVdF) is currently the most widely used adhesive in lithium-ion batteries due to its excellent electrochemical stability, good bonding ability, high adhesion and versatility. Despite toxicity issues and high processing costs, PVdF adhesives are dissolved in volatile, flammable, explosive and highly toxic organic solvents such as traditional N-methylpyrrolidone (NMP), resulting in serious environmental pollution. PVdF is very sensitive to moisture and can lead to a variety of battery failure mechanisms, including volume changes, mechanical stress (including active material pulverization), loss of contact with the current collector, cracking and regeneration of the solid electrolyte interface (SEI) passivation layer, and loss of electrode porosity that limits ion conduction. In addition, both PVdF and NMP are expensive, which leads to higher production costs for lithium-ion batteries.
[0053] In recent years, aqueous or water-based binders have attracted increasing attention due to their low cost and environmentally friendly advantages. Many publications have reported the improvement of electrochemical stability of electrodes containing aqueous binders, for example, the cycling stability of Li / SiOx electrodes containing different binder types (conventional PVdF binder) is inferior to that of aqueous Na-CMC and Li-PAA binders. Due to the different chemical interactions between the active materials and aqueous binders, higher reversible intercalation / deintercalation is achieved compared to PVdF binder electrodes.
[0054] Finally, according to the present invention, there is also proposed a method for manufacturing an electrode of an electrochemical cell containing lithium ions, the method comprising the steps of preparing a slurry as described above, coating or laminating the slurry on a current collector, and drying the slurry.
[0055] Therefore, considering all the above factors, using the present invention, the PVdF content in the electrode can be avoided and / or reduced due to the use of a water-based binder in the slurry.
[0056] According to the present invention, the overall binder content in the electrode can be reduced by controlling the pH of the slurry between 9 and 10.5 through improved formulation, improved binder type, and improved mixing techniques.
[0057] According to the present invention, lamination between a separator and an electrode made from an aqueous solution can be enhanced because the type of binder used and an appropriate surfactant can enhance dispersion of the binder in the slurry.
[0058] The cohesive bonding between particles within the electrode structure manufactured according to the present invention can be enhanced because the type of binder used and the increase in the solid content in the slurry result in a decrease in the amount of water carried away during drying of the electrode, thereby resulting in a decrease in the porosity and increase in the elasticity of the electrode.
[0059] The chemical and electrochemical stability of cathodes made according to the present invention can be enhanced because of the lower porosity and better inter-particle contact of the electrode.
[0060] According to the present invention, the safety of the battery cell can be improved by using a more stable water-based adhesive because the water-based adhesive has a higher stability compared to PVDF adhesives which are known to decompose (resulting in HF release) at elevated temperatures and high voltages.
[0061] Electrodes are manufactured by increasing the solid content (i.e., the content of all non-aqueous components) in the slurry to 60% to 85%, or better 75% to 85%. The adhesion of the electrode block to the current collector can be enhanced by improving the formulation, improving the binder type, and improving the mixing technology to control the pH value of the slurry between 9 and 10.5.
[0062] The recyclability of the electrode materials can be improved because the water-based binder can be diluted in water.
[0063] Finally, the manufacturing cost of the electrode (cathode) can be reduced based on the present invention because the coating process can be run at much lower temperatures using water as a solvent (NMP is a traditional solvent used to produce electrodes, which requires higher temperatures due to its high boiling point). This results in a shorter drying section of the coater and uses less energy to extract the solvent, which is water in the present invention. It enables the use of smaller, faster, more cost-effective machines, making the battery cheaper and more widely available. There is also no need for a solvent recovery system because the emissions from the coater are steam, which can be released into the atmosphere without any further treatment.
[0064] Other aspects, features and advantages of the present invention will be readily understood from the description of the preferred embodiments and implementations in the following detailed description. The present invention can also be implemented in other different embodiments, and its details can be modified in various obvious aspects without departing from the spirit and scope of the present invention. Therefore, the drawings and description should be regarded as illustrative rather than restrictive. Other objects and advantages of the invention will be set forth in part in the subsequent description, and in part will be apparent from the description, or can be understood by practicing the present invention.
[0065] The present invention will be described below based on the accompanying drawings. It should be understood that the embodiments and aspects of the present invention described in the accompanying drawings are only examples and do not limit the scope of protection of the claims in any way. The present invention is defined by the claims and their equivalents. It should be understood that the features of one aspect or embodiment of the present invention may be combined with the features of one or more different aspects of other embodiments of the present invention, wherein:
[0066] Figure 1 An example of an electrochemical cell according to a preferred embodiment of the present invention is shown;
[0067] Figure 2a A second example of an electrochemical cell according to a preferred embodiment of the present invention is shown;
[0068] Figure 2b shows how electrochemical cells according to a preferred embodiment of the present invention are stacked to form a battery;
[0069] Figure 3 A battery consisting of a plurality of stacked electrochemical cells is shown filled with an electrolyte;
[0070] Figure 4 Shows the filled Figure 3 batteries; and
[0071] Figure 5 Comparison of the cycling stability plots of G / NMC622 and G / NMCA containing 88% Ni is shown.
[0072] according to Figures 1 to 4 The preferred embodiment of the invention is shown.
[0073] Figure 1 1a and 1b show examples of electrochemical cells 2 that can be used according to the present disclosure. The electrochemical cell 2 includes two electrodes, an anode 10 and a cathode 20. The anode 10 and the cathode 20 are separated by a separator 30. The anode 10 and the cathode 20 shown are made of a slurry comprising a water-based binder system and an electrochemically active compound having a Li metal oxide containing Ni, wherein the Ni content in the metal (LiMeO2) is at least 80%.
[0074] In the preferred embodiment shown, the layered oxide cathode material is Li 1.2 Mn 0.5100 Ni 0.2175 Co 0.0725 O2, where the Ni content in the metal (LiMeO2) is 90%.
[0075] The electrochemically activatable compound of the preferred embodiment shown is selected from the group consisting of NMC type, NCA type, NCMA type and high voltage Li-NMO (LiNi0.5 Mn 1.5 O4) type.
[0076] Furthermore, the electrode according to the preferred embodiment shown is made of a slurry having a PVdF content of 0-2% of a water-based binder system, a pH value between 9 and 10.5, and a solid content, ie, all non-aqueous components, of 75% to 85%.
[0077] The water-based binder system used in the preferred embodiment shown is a carboxymethyl cellulose (CMC) based binder system.
[0078] The anode 10 and cathode 20 have electrical contacts 12, 22 for making electrical contact with the respective electrodes. The separator 30 shown is a ceramic separator as is known in the art.
[0079] The electrochemical cell 2a shown is a large electrochemical cell. If at least one of the electrodes 10, 20 and the separator 30 between the electrodes has a length A and / or a width B of at least about 10 cm or more, the electrochemical cell can be called a large electrochemical cell. For example, the length A and width B of the electrodes 10, 20 can be from about 10 cm to about 20 cm. The length A can be different from the width B, allowing for a rectangular or any other desired shape. The shape of the electrode can be adapted to the application of the electrochemical cell or battery and can be adapted to a specific housing.
[0080] In the example shown, the distance D between the anode 10 and the cathode 20 is less than 1 mm. For example, the distance between the anode current collector of the anode 10 and the cathode connector of the cathode 20 may be about 400 μm or less.
[0081] Each of the electrodes 10 , 20 of the anode 10 and the cathode 20 may be made of a foil material having a thickness of less than about 50 μm. In particular, the foil may have a thickness of about 10 μm to 20 μm. For example, aluminum foil may be used for the cathode, and copper foil may be used for the anode 10 .
[0082] The electrochemical cell 2 a is filled with an electrolyte 4 which is in contact with the anode 10 and the cathode 20 .
[0083] Figure 2a An electrochemical cell 2b is shown which differs from the electrochemical cell 2a in that a separator 30 and an anode 10 are provided on both sides of the cathode 20. An electrolyte 4 is injected between each anode 10 and cathode 20. This enables the electrochemical cells 2b in the battery 1 to be stacked more closely and requires less cathode material. For clarity, the electrical contacts 12, 22 are omitted in the figure.
[0084] Multiple Figure 1 a and Figure 1b shows an electrochemical cell 2a or a plurality of Figure 2a The electrochemical cells 2 b shown can be stacked on top of one another to form a rechargeable battery 1 . Figure 2b It is shown how a plurality of electrochemical cells 2b can be stacked in a housing, pack or pouch 5. The number of stacked electrochemical cells 2 may vary depending on the application of the rechargeable battery 1. In the example shown, for ease of illustration, three electrochemical cells 2b are shown stacked together to form the rechargeable battery 2, but the number of electrochemical cells 2a, 2b may be much higher. For example, the battery 2 may include up to about 500 electrochemical cells 2a, 2b.
[0085] like Figure 1 a and Figure 1 The electrochemical cells 2a shown in b can be simply stacked together, while the electrodes 10, 20 can be separated from each other using a separator material.
[0086] However, other stacking methods are possible and suitable for use in the present invention. Figure 4 The electrochemical cell 2b is shown in a dual cell configuration. The cell can also be implemented as a single cell configuration, a bipolar configuration, a wound or zigzag stacked cell.
[0087] The active substance or active material can be coated on one side or both sides of the current collector. Other stacking methods can also be applied, such as alternately stacking anodes and cathodes with a separator material between each anode and cathode. In this way, both surfaces of the anode and cathode can be used.
[0088] Figure 2b A plurality of electrochemical cells 2b are shown stacked in a pack or pouch 5 in a bi-cell configuration before electrolyte is filled into the electrochemical cells 2b.
[0089] Figure 3 It is shown how the electrolyte 4 can be injected into the electrochemical cells 2a, 2b. The electrochemical cells 2a, 2b can be enclosed in a pouch 5 which is closed at all except the top side 6 using a dosing device 8 such as a needle. Figure 3 A dual cell configuration of three pairs of electrochemical cells 2b is shown, wherein contacts 12, 22 are omitted for clarity. A dosing device 8 can inject a predetermined amount of electrolyte 4 into the electrochemical cells 2a, 2b. The electrolyte 4 can be injected into the electrochemical cells 2a, 2b encapsulated in the soft pack 5 under vacuum conditions, for example, at an absolute pressure of about 10mbr to 500mbr. The electrolyte 4 can be injected from only one side, which greatly simplifies the injection process.
[0090] It is important that the electrolyte 4 is distributed very evenly between the anode 10 and the cathode 20, and in particular, there should be no bubbles or other errors between the anode 10 and the cathode 20, as this will lead to undesirable defects and lower battery capacity. The electrolyte 4 in the battery 1 according to the present invention may contain a non-aqueous solvent, such as a cyclic carbonate, a cyclic ester, a linear carbonate, an ether or a combination thereof, and other organic solvents may be used.
[0091] Electrolyte 4 includes a conductive lithium salt, such as LiClO4, LiPF6, LiBF4, LiAsF6 and LiPF3(CF2CF3), lithium bis[1,2-oxalato(2-)-O,O']borate (LiBOB)-based electrolyte, LiF4C2O4, LiFOP, LiPF4(C2O4), LiF4OP, LiCF3SO3, LiC4F9SO3, Li(CF3SO2)2N, Li(C2F5SO2)2N, LiSCN and LiSbF6, LiAlO4, LiAlC14, LiCl and LiI or a combination thereof, and other known lithium salts may also be used.
[0092] The electrolyte 4 contains a wetting agent. The wetting agent is used to uniformly wet the surfaces of the anode 10, cathode 20 and separator 30 and to achieve uniform distribution of the electrolyte 4 within the electrochemical cells 2a, 2b. The wetting agent may be or may contain a fluorinated polymer, in particular a fluorinated surfactant.
[0093] Possible examples of fluorinated polymers include commercially available perfluoroalkyl ethoxylates such as Zonyl SFO, Zonyl SFN and Zonyl SF300 (EIDuPont), lithium 3-[(1H,1H,2H,2H-fluoroalkyl)thio]-propionate, Zonyl FSA Du Pont).
[0094] Examples of commercially available fluorosurfactants that can be used according to the present disclosure include, but are not limited to, those distributed by DuPont under the product names Zonyl SFK, Zonyl SF-62, or by 3M Company under the product names FLURAD FC 170, FC 123, or L-18699A. Other commercially available products that can be used as fluorosurfactants include 3M Company products distributed under the product names Novec F-C4300, 3M FC-4430, 3M FC-4442, or 3M FC-4434.
[0095] Other wetting agents that can be used according to the present disclosure include semi-fluorinated acrylic polymer EGC-1700, fluoromethyl acrylate, long chain perfluoro acrylate, tetrafluoroethylene, hexafluoropropylene, silane coupling agent with perfluoropolyether (PFPE-5), acrylic polymer containing (perfluoroalkyl) ethyl methacrylate, butyl methacrylate-co-perfluoroalkyl acrylate, semi-fluorinated fluorocarbon diblock copolymer poly (butyl methacrylate-co-perfluoroalkyl acrylate), n-perfluorononane, perfluoropropylene oxide (perfluoropropyleneoxyde), polytetrafluoroethylene, poly (tetrafluoroethylene-co-hexafluoropropylene), perfluorobutyl (PFB), perfluoromethyl, perfluoroethyl or a combination thereof. All of the above wetting agents can be used alone or in any combination.
[0096] The wetting agent, fluoropolymer or fluorosurfactant may be used in a concentration of about 5 ppm (parts per million) to about 5000 ppm.
[0097] The use of a wetting agent in the electrolyte allows for a uniform distribution of the electrolyte 4 in the electrochemical cells 2a, 2b. The use of a wetting agent can significantly reduce the filling time and enable the manufacture of large lithium-ion batteries within an acceptable time frame suitable for mass production.
[0098] Figure 4 A sealed battery pack 1 is shown, wherein after filling the battery pack 1 with electrolyte 4 the opening 6 of the pouch 5 has been closed.
[0099] It is obvious to the person skilled in the art that there are other possible ways of packaging the electrochemical cells 2a, 2b than the pouch 5. For example, a battery casing made of known plastic materials may be used.
[0100] It is obvious to those skilled in the art that a plurality of battery packs 1 can be combined to increase the capacity and / or voltage of the battery.
[0101] at last, Figure 5 The charge / discharge (1C / 1C) cycle stability comparison of water-based binder electrodes G / NMC622 (blue) and G / NMCA (88% Ni, red) is shown. Figure 5 As can be seen from the figure in , the G / NMCA battery cell according to the present invention shows similar cycling stability to the G / NMC622 battery cell with significantly less Ni content.
[0102] The above description of the preferred embodiment of the present invention is for the purpose of illustration and description only. It is not intended to be exhaustive or limit the present invention to the precise form disclosed, and modifications and variations are possible according to the above teachings, or can be obtained from the practice of the present invention. The embodiment is selected and described to explain the principles of the present invention and its practical application, so that those skilled in the art can utilize the present invention in various embodiments suitable for the intended specific use. The scope of the present invention is limited by the appended claims and their equivalents.
Claims
1. A slurry for making an electrode for a lithium-ion battery cell, wherein the slurry is a water-based binder system comprising an electrochemically active compound having a Li metal oxide comprising Ni, wherein the metal (LiMeO 2 ) has a Ni content of at least 80 wt %, and wherein the pH of the slurry is adjusted to 9 to 10.
5.
2. The slurry according to claim 1, wherein the electrochemically activatable compound is selected from lithium nickel manganese cobalt oxide type, lithium nickel cobalt aluminum oxide type, lithium nickel cobalt aluminum oxide type, high voltage Li-NMO (LiNi 0.5 Mn 1.5 O 4 ) and high voltage Li-NMA (LiNi 1-x-y Mn x Al y O 2 )type.
3. The slurry according to claim 1 or 2, wherein the PVdF content of the water-based binder system is selected between 0 wt% and 2 wt%.
4. The slurry according to claim 3, wherein the PVdF content of the water-based binder system is 0 wt%.
5. The slurry according to claim 3, wherein the PVdF content of the water-based binder system is between 0.5 wt% and 1 wt%.
6. The slurry of claim 3, wherein the PVdF content of the water-based binder system is between 1 wt% and 2 wt%.
7. The slurry according to any one of the preceding claims, wherein the water-based binder system comprises carboxymethyl cellulose (CMC).
8. The slurry according to any one of the preceding claims, wherein the water-based binder system comprises styrene butadiene rubber (SBR).
9. The slurry according to any one of the preceding claims, wherein the water-based binder system comprises an acrylic-based binder.
10. The slurry according to any one of the preceding claims, wherein the solids content in the slurry is 60% to 85%.
11. The slurry according to claim 10, wherein the solid content in the slurry is 75% to 85%.
12. The slurry according to any one of the preceding claims, wherein for adjusting the pH value of the binder solution, acrylates such as polyacrylic acid (PAA) or polyethylene-co-acrylic acid (PEAA), phosphoric acid, citric acid, LiH 2 SO 4 , LiH 2 PO 4 or ammonia.
13. An electrode for an electrochemical cell containing lithium ions, produced from the slurry according to any one of claims 1 to 12.
14. An electrochemical cell comprising an electrode according to claim 13.
15. A method for producing an electrode for an electrochemical cell containing lithium ions, the method comprising: The following steps are involved: a. preparing a slurry according to any one of claims 1 to 12, b. coating or laminating the slurry on a current collector, and c. Drying the slurry.