Iron-based catalyst for low-temperature Fischer-Tropsch synthesis as well as preparation method and application thereof
Through PVP assisting Mg-modified iron-based catalyst, the MgFe2O4 spinel phase is formed, which solves the problems of low activity of traditional catalysts and high by-products, and achieves medium-to-high activity and good selectivity of low-temperature Fischer Tropsch synthesis, simplifies the preparation process, and is suitable for industrialization Production.
Patent Information
- Application Number
- CN202410963464.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional iron-based catalysts have problems such as low activity, high by-products and complex preparation process in Fischer-Tropsch synthesis, which limits their application, and existing improved methods have failed to effectively pay attention to the stability of the catalyst and the feasibility of industrial production.
The iron-based catalyst was synthesized by PVP-assisted Mg modification of low-temperature Fischer Tropsch. By adding magnesium salt and PVP to the metal salt solution, the formation of the MgFe2O4 spinel phase was promoted, the activity and stability of the catalyst was improved, and the preparation process was simplified.
The activity of the catalyst and product selectivity are significantly improved under low temperature conditions, the preparation process is simplified, the production cost is reduced, and the production efficiency of Fischer-Tropsch synthesis is improved.
Smart Images

Figure BDA0004951007330000121
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of Fischer-Tropsch synthesis, and in particular to an iron-based catalyst for low-temperature Fischer-Tropsch synthesis and a preparation method and application thereof. Background Art
[0002] As an important chemical reaction, Fischer-Tropsch synthesis is one of the main methods for synthesizing hydrocarbon compounds in industry. Through this reaction, carbon monoxide and hydrogen are converted into various hydrocarbons, especially hydrocarbon products such as methane, ethane and long-chain hydrocarbons in the presence of a suitable catalyst. These products are widely used in the chemical industry in the fields of lubricants, fuels and chemical raw materials. In the Fischer-Tropsch synthesis process, the performance of the catalyst is crucial to the reaction efficiency. As one of the main catalysts for Fischer-Tropsch synthesis, iron-based catalysts have the advantages of abundant resources and low cost, and have been widely used in industrial production. However, traditional iron-based catalysts have problems such as complex preparation process, low activity and poor stability, which limit their application in Fischer-Tropsch synthesis. Therefore, it is of great industrial significance to find a method that can improve the activity and stability of iron-based catalysts.
[0003] At present, low-temperature Fischer-Tropsch iron-based catalysts are mainly prepared by precipitation method. The crystals of the catalysts are small. In addition, Fischer-Tropsch synthesis is a highly exothermic reaction, and there are violent exothermic hot spots at the active sites. The active particles of the catalysts are often prone to sintering or breaking, which reduces the activity of the catalyst. Typical commercial Fe-based catalysts generally add a certain amount of electronic additive K, reduction additive Cu, carrier SiO2, and some other transition metal additives. The method of adding K additives is mostly to add potassium source compounds to the precipitated filter cake after washing and filtration. The role is to inhibit CH4 and improve the selectivity of heavy hydrocarbons and olefins. The Cu additive can promote the reduction of iron oxides. The main purpose of adding SiO2 is to increase the specific surface area and wear resistance of the catalyst. At present, almost all Fischer-Tropsch synthesis iron-based catalysts need to introduce SiO2 to improve the mechanical strength of the catalyst particles. In order to further improve the activity and stability of the catalyst, researchers have improved the mechanical strength of the catalyst by adding one or more structural additives. For example, in Chinese patents CN107913714B, CN1245255C, CN101293206A, CN101298046A and CN105478128B, one or more rare earth metals, alkaline earth metals and other transition metal additives are added to improve the activity and wear resistance of the catalyst by utilizing the synergistic effect between the additives. Although it shows a high conversion rate and maintains low CO2 selectivity and CH4 selectivity, the patents do not pay attention to the stability of the catalyst. In addition, due to the complex catalyst composition and cumbersome preparation process, it also increases time and cost, which is not conducive to industrial production. Summary of the invention
[0004] In order to solve the problems of low activity, high by-products and complex preparation process of traditional iron-based catalysts, the present invention provides an iron-based catalyst for low-temperature Fischer-Tropsch synthesis and a preparation method and application thereof, and utilizes PVP to assist Mg in modifying the low-temperature Fischer-Tropsch synthesis iron-based catalyst so that it has significant catalytic activity and good product selectivity under low temperature conditions; and the preparation process of the catalyst is simple and efficient, and can be mass-produced; applying it to the low-temperature Fischer-Tropsch synthesis process can significantly improve production efficiency and reduce production costs, and has very important economic and social value.
[0005] As an alkaline earth metal, Mg plays many roles in iron-based low-temperature Fischer-Tropsch synthesis catalysts, including promoting the growth and stability of MgFe2O4 spinel crystals, regulating active sites, improving redox performance, preventing crystal aggregation and accumulation, and regulating surface acidity and alkalinity. These effects jointly affect the activity, selectivity and stability of the catalyst, thereby affecting the efficiency and product selectivity of the Fischer-Tropsch synthesis reaction. In catalyst synthesis, the addition of PVP is conducive to the formation of nano-metal oxide precursor particles, which can improve the dispersibility, activity and stability of the active components of the catalyst, thereby improving the performance of the catalyst; however, excessive or insufficient addition of PVP may lead to a decrease in catalyst performance. Therefore, when designing and optimizing iron-based catalysts, it is necessary to comprehensively consider the addition amount of Mg and PVP and the pretreatment conditions to achieve the best catalytic effect.
[0006] According to one aspect of the present invention, there is provided a method for preparing an iron-based catalyst, comprising the following steps:
[0007] S1. Add the required amount of iron salt, copper salt, magnesium salt and PVP to an appropriate amount of deionized water, stir to fully dissolve, and obtain solution A; fully mix the required amount of precipitant and silicon source aqueous solution to obtain solution B; and keep the remaining required amount of silicon source for standby use, i.e., solution C;
[0008] S2, adding solution A to solution C at a certain pump speed to perform a coprecipitation reaction, and then performing solid-liquid separation and washing to obtain a filter cake M1;
[0009] S3, adding deionized water to the filter cake M1 obtained above to re-slurry, then adding the C solution, continuing the slurry treatment, adjusting the pH value and temperature of the slurry, and then filtering to obtain the filter cake M2;
[0010] S4, drying and calcining the filter cake M2 to obtain the iron-based catalyst;
[0011] The above-mentioned magnesium salt and PVP can also be added in the following manner: first, the filter cake M2 obtained in S3 is re-slurried by adding an appropriate amount of deionized water, and then the required amount of one or both of the magnesium salt solution and PVP are added to the above-mentioned slurry; the slurry does not need to be filtered, but is directly dried and calcined to obtain the iron-based catalyst.
[0012] As a preferred embodiment, the iron salt, copper salt and magnesium salt are selected from nitrate, chloride, bicarbonate, ammonium salt, sulfate, organic salt, hydroxide or any mixture thereof; and / or,
[0013] The specification of the PVP is one or more of K15, K30, and K60, preferably K30; and / or,
[0014] The precipitant is selected from one or more of sodium carbonate, potassium carbonate, sodium hydroxide, ammonia water, ammonium carbonate, ammonium bicarbonate, and potassium hydroxide; and / or,
[0015] The silicon source is selected from one or more of potassium silicate solution, sodium silicate solution, acidic or alkaline silica sol solution.
[0016] As a preferred embodiment, the concentration of the precipitant is 1M-2M, and the concentration of the iron salt is 1-2M.
[0017] As a preferred solution, the required amount of silicon source can be added in whole or in part to the precipitant solution to obtain solution B; or it can be used in whole or in part as a backup silicon source, i.e., solution C. The silicon sources mentioned above can be the same or different silicon sources. For example, the silicon source used in solution B can be silica sol (acidic silica sol or alkaline silica sol), or any one or more of potassium silicate or sodium silicate. The remaining silicon source in solution C is added to the mixed slurry M1, and the silicon source can be any one or more of silica sol, potassium silicate, and sodium silicate.
[0018] The silicon source added in steps S2 and S3 is calculated based on the total mass of SiO2 introduced into the catalyst. For example, if the mass of SiO2 in the silicon source added in step S2 accounts for 20% of the total mass of SiO2 in the catalyst, then the silicon source corresponding to the remaining 80% of SiO2 is added to the mixed slurry M1 in step S3, and so on.
[0019] As a preferred embodiment, in step S2, solution A is added to solution B for co-precipitation reaction, the pump speed is calculated according to the volume of the solution and the feeding time, the feeding time is controlled to be 5 to 30 minutes, the temperature of the co-precipitation reaction is 50 to 90°C, the pH value is 5.5 to 9.5 at the end of the reaction, and aging is continued for 0 to 2 hours after the feeding is completed.
[0020] As a preferred embodiment, in step S2, during the solid-liquid separation and washing to obtain the filter cake M1, the conductivity of the filtrate is controlled to be 300 to 3000 μs / cm.
[0021] As a preferred solution, in step S3, the filter cake M1 is re-slurried with deionized water, the slurry concentration of the slurry treatment is 7-25%, the slurrying time is 0.5-2h, and the slurrying temperature is 10-50°C.
[0022] As a preferred solution, in step S3, solution C is then added and beating treatment is continued, and the beating time is controlled within 0.5 to 2 hours.
[0023] As a preferred solution, in step S3, the pH value of the slurry is adjusted to about 5 to 9 with dilute nitric acid, and then the temperature of the slurry is raised to 50 to 90° C., and then filtered to obtain a filter cake M2; the concentration of the dilute nitric acid is 5 to 25%, preferably 10 to 20%.
[0024] As a preferred embodiment, in step S4, the drying process is air oven drying or vacuum oven drying, the air oven drying temperature is 80-150°C, preferably 90-120°C; the vacuum oven drying temperature is 20-80°C, preferably 40-60°C; the drying time is 1-30h, preferably 12-28h.
[0025] As a preferred solution, in step S4, the calcination temperature is 300-600°C, the heating rate is 0.5-2°C / min, and the calcination time is 4-10h. The calcined catalyst is sieved with 80-100 mesh.
[0026] According to another aspect of the present invention, an iron-based catalyst prepared by the above-mentioned preparation method is further provided, wherein the mass ratio of the components in the iron-based catalyst is: Fe:Cu:Mg:K:Na:SiO2=100:(0~5):(0.2~10):(0.5~8):(0.5~3):(10~30); preferably Fe:Cu:Mg:K:Na:SiO2=100:(0~5):(0.2~5):(0.5~8):(0.5~1.5):(10~30).
[0027] As a preferred embodiment, the mass percentage of PVP during the synthesis of the iron-based catalyst is Fe:PVP=100:(1-40), preferably Fe:PVP=100:(1-20).
[0028] According to yet another aspect of the present invention, there is further provided application of the above iron-based catalyst in low-temperature Fischer-Tropsch synthesis.
[0029] The present invention adopts the above technical solution to have at least the following beneficial effects:
[0030] 1. The iron-based catalyst for low-temperature Fischer-Tropsch synthesis provided by the present invention, as well as its preparation method and application, utilizes PVP (polyvinyl pyrrolidone) to assist Mg in modifying the iron-based catalyst for low-temperature Fischer-Tropsch synthesis, adds magnesium salt and PVP dispersant to the metal salt solution, and reacts under appropriate conditions. In this method, the interaction between magnesium and iron is promoted, and the MgFe2O4 spinel phase is easily formed. This structure has a high active site density and surface oxygen activity, can promote the adsorption and dissociation of CO, improve the catalytic reaction activity, and can effectively inhibit the peroxidation reaction of CO, reduce the generation of CO2, and thus reduce the selectivity of CO2; and the introduction of PVP can promote the dispersion and mutual contact of metal ions, improve the synthesis efficiency of MgFe2O4 spinel, help to obtain spinel materials with excellent catalytic performance, and ensure the uniformity and stability of the reaction; it can also form complexes with metal ions or coat the surface of particles during the synthesis process, thereby regulating the morphology and size distribution of the product, which is conducive to obtaining MgFe2O4 spinel with good morphology and dispersibility; in addition, the structure of PVP can act as a template, which is conducive to the formation of a spinel phase with a certain pore structure, and helps to maintain the crystal structure and stability of the catalyst; the catalyst provided by the present invention has significant catalytic activity and good product selectivity under low temperature conditions, can effectively improve the yield of the target product, and reduce the generation of by-products;
[0031] 2. The iron-based catalyst for low-temperature Fischer-Tropsch synthesis provided by the present invention and its preparation method and application have a simple preparation process, mild and easy-to-control conditions, and good industrial application prospects;
[0032] 3. The iron-based catalyst for low-temperature Fischer-Tropsch synthesis provided by the present invention, as well as its preparation method and application, is easy to manufacture, has excellent catalytic performance and good heat resistance, and is not easily deactivated after long-term use. Therefore, its application can significantly improve the production efficiency of the Fischer-Tropsch synthesis process and reduce production costs, and has very important economic and social value. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the present application. The various commonly used reagents used in the examples are all commercially available products.
[0034] The test conditions of the catalyst involved in the present invention include placing 15g of catalyst and 500mL of liquid paraffin in a 1L stirred reactor, and reacting the catalyst in a synthesis gas containing CO and H2 after the catalyst is first subjected to reduction and carburization steps. The Fischer-Tropsch synthesis reaction conditions include: reaction temperature 210-275°C, reaction pressure 0.1-4MPa, a molar ratio of H2 to CO in the synthesis gas of (1.0-3.0):1, and a reaction space velocity of 8000-2000h -1 .
[0035] The reduction step of the catalyst of the present invention can be carried out by conventional methods in the art, such as using CO, H2 or a mixture of H2 and CO in any proportion as a reducing agent. The reduction conditions include: a reduction temperature of 200 to 275°C, a reduction pressure of 0.1 to 2 MPa, and a reduction space velocity of 8000 to 15000 h -1 The reduction time is 8 to 48 hours.
[0036] In the carburizing step of the catalyst of the present invention, CO or a H2 / CO mixed gas in any proportion is used as a reducing agent. The carburizing conditions include: a temperature of 200-275°C, a pressure of 0.1-2 MPa, and a space velocity of 8000-15000 h -1 , time is 12 to 60 hours.
[0037] The CO conversion rate and CO2 and CH4 selectivity were calculated by measuring and analyzing the CO molar number at the feed inlet of the Fischer-Tropsch synthesis reactor and measuring and analyzing the CO, CO2 and CH4 molar numbers at the discharge port.
[0038] CO conversion rate % = [(CO moles at the feed port - CO moles at the discharge port) ÷ CO moles at the feed port] × 100%;
[0039] CO+H2 conversion rate % = [(CO moles at feed inlet - CO moles at discharge outlet + H2 moles at inlet - H2 moles at outlet) ÷ (CO moles at feed inlet + H2 moles at inlet)] × 100%;
[0040] CO2 selectivity % = [CO2 mole number at the outlet ÷ (CO mole number at the feed inlet - CO mole number at the outlet)] × 100%;
[0041] CH4 selectivity % = [CH4 mole number at the outlet ÷ (CO mole number at the feed inlet - CO mole number at the outlet)] × 100%;
[0042] C 5+ Selectivity % = [discharge port C 5+ mole number ÷ (mole number of CO at the feed port - mole number of CO at the discharge port)] × 100%;
[0043] The percentages used in the embodiments of the present invention are all by mass unless otherwise specified.
[0044] Example 1
[0045] 404g of Fe(NO3)3·9H2O, 10.62g of Cu(NO3)2·3H2O, 17.76g of Mg(NO3)2·6H2O and 16.75g of PVP(K30) were added to deionized water and slurried to dissolve, and a 1L solution was prepared, and stirred to fully dissolve to obtain solution A. 10.86g of potassium silicate with a SiO2 content of 25.72% was added to 1.7L of a 1mol / L Na2CO3 solution and stirred to obtain solution B.
[0046] Solution A was added to solution B for coprecipitation reaction, the precipitation reaction temperature was 80°C, the feeding time was controlled to be 20min, and finally the pH value of the slurry was adjusted to about 7 with 20wt% dilute nitric acid. The precipitated filter cake was not aged and was directly filtered. Subsequently, it was washed with deionized water for multiple times, and the final filtrate conductivity was controlled to be below 500μs / cm. The filter cake M1 obtained above was re-slurried with deionized water until it was uniform, and then 43.3g of potassium silicate with a SiO2 content of 25.72% was added for slurry treatment. The slurrying time was controlled to be 1h, and then the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid, and then the slurry was heated to 80°C and filtered to obtain filter cake M2. The filter cake obtained above was dried in a 120°C oven for 24h, and then calcined in a muffle furnace at 400°C for 6h to obtain catalyst 1.
[0047] Example 2
[0048] 404g of Fe(NO3)3·9H2O, 10.62g of Cu(NO3)2·3H2O, 8.88g of Mg(NO3)2·6H2O and 11.17g of PVP(K30) were added to deionized water and slurried to dissolve, and a 1L solution was prepared, and stirred to fully dissolve to obtain solution A. 10.86g of potassium silicate with a SiO2 content of 25.72% was added to 1.7L of a 1mol / L Na2CO3 solution and stirred to obtain solution B.
[0049] Solution A was added to solution B for coprecipitation reaction, the precipitation reaction temperature was 80°C, the feeding time was controlled to be 20min, and finally the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid. The precipitated filter cake was not aged and was directly filtered. Subsequently, it was washed with deionized water for multiple times, and the final filtrate conductivity was controlled to be about 1000μs / cm. The filter cake M1 obtained above was re-slurried with deionized water until it was uniform, and then 43.3g of potassium silicate with a SiO2 content of 25.72% was added for slurry treatment. The slurrying time was controlled to be 1h, and then the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid, and then the slurry was heated to 80°C and filtered to obtain filter cake M2. The filter cake obtained above was dried in a 120°C oven for 24h, and then calcined in a muffle furnace at 400°C for 6h to obtain catalyst 2.
[0050] Example 3
[0051] 404g of Fe(NO3)3·9H2O, 5.31g of Cu(NO3)2·3H2O and 17.76g of Mg(NO3)2·6H2O were added to deionized water and slurried to dissolve, and 1L of solution was prepared and stirred to fully dissolve to obtain solution A. 10.86g of potassium silicate with a SiO2 content of 25.72% was added to 1.7L of a 1mol / L Na2CO3 solution and stirred to obtain solution B.
[0052] Solution A was added to solution B for coprecipitation reaction, the precipitation reaction temperature was 85°C, the feeding time was controlled to be 20min, and finally the pH value of the slurry was adjusted to about 6.5 with 20wt% dilute nitric acid. The precipitated filter cake was not aged and was directly filtered. Subsequently, it was washed with deionized water for multiple times, and the final filtrate conductivity was controlled to be about 1000μs / cm. The filter cake M1 obtained above was re-slurried with deionized water until it was uniform, and then 43.3g of potassium silicate with a SiO2 content of 25.72% was added for slurry treatment, and the slurrying time was controlled to be 1h, and then the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid, and then the slurry was heated to 85°C, and the filter cake M2 was obtained by suction filtration. First, 22.34g PVP (K30) was dissolved in 100ml water, and then the above solution was added to M2 for re-slurrying, and the slurrying time was 1h. The slurry obtained above was then dried in an oven at 120°C for 24 h, and then calcined in a muffle furnace at 400°C for 6 h to obtain catalyst 3.
[0053] Example 4
[0054] 404g Fe(NO3)3·9H2O, 1.06g Cu(NO3)2·3H2O, 17.76g Mg(NO3)2·6H2O and 22.34g PVP(K30) were added to deionized water and slurried to dissolve, and 1L solution was prepared, and stirred to fully dissolve to obtain solution A. 10.86g potassium silicate with SiO2 content of 25.72% was added to 1.7L Na2CO3 solution with a concentration of 1mol / L and stirred to obtain solution B.
[0055] Solution A was added to solution B by the reverse addition method for coprecipitation reaction. The precipitation reaction temperature was 85°C, and the feeding time was controlled to be 20min. Finally, the pH value of the slurry was adjusted to about 6.5 with 20wt% dilute nitric acid. The precipitated filter cake was not aged and was directly filtered. Subsequently, it was washed with deionized water for multiple times to control the final filtrate conductivity to be about 2000μs / cm. The filter cake M1 obtained above was re-slurried with deionized water until it was uniform, and then 43.3g of potassium silicate with a SiO2 content of 25.72% was added for slurry treatment. The slurrying time was controlled to be 1h, and then the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid. The slurry was heated to 85°C and filtered to obtain filter cake M2. The filter cake obtained above was dried in a 120°C oven for 24h, and then calcined in a muffle furnace at 400°C for 6h to obtain catalyst 4.
[0056] Example 5
[0057] 404g of Fe(NO3)3·9H2O, 10.62g of Cu(NO3)2·3H2O, 28.42g of Mg(NO3)2·6H2O and 11.17g of PVP(K30) were added to deionized water and slurried to dissolve, and a 1L solution was prepared, and stirred to fully dissolve to obtain solution A. 10.86g of potassium silicate with a SiO2 content of 25.72% was added to 1.7L of a 1mol / L Na2CO3 solution and stirred to obtain solution B.
[0058] Solution A was added to solution B by the reverse addition method for coprecipitation reaction. The precipitation reaction temperature was 85°C, and the feeding time was controlled to be 18 minutes. Finally, the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid. The precipitated filter cake was not aged and was directly filtered. Subsequently, it was washed with deionized water for multiple times, and the final filtrate conductivity was controlled to be about 1000μs / cm. The filter cake M1 obtained above was re-slurried with deionized water until it was uniform, and then 43.3g of potassium silicate with a SiO2 content of 25.72% was added for slurry treatment. The slurrying time was controlled to be 1h, and then the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid. The slurry was heated to 85°C and filtered to obtain filter cake M2. The filter cake obtained above was dried in a 120°C oven for 24h, and then calcined in a muffle furnace at 400°C for 6h to obtain catalyst 5.
[0059] Example 6
[0060] 404g Fe(NO3)3·9H2O, 10.62g Cu(NO3)2·3H2O, 35.53g Mg(NO3)2·6H2O and 11.17g PVP(K30) were added to deionized water and slurried to dissolve, and 1L solution was prepared and stirred to fully dissolve to obtain solution A. 21.71g potassium silicate with SiO2 content of 25.72% was added to 1.7L Na2CO3 solution with a concentration of 1mol / L and stirred to obtain solution B.
[0061] Solution A was added to solution B by the reverse addition method for coprecipitation reaction. The precipitation reaction temperature was 85°C, and the feeding time was controlled to be 18 minutes. Finally, the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid. The precipitated filter cake was not aged and was directly filtered. Subsequently, it was washed with deionized water for multiple times to control the final filtrate conductivity to be about 1000μs / cm. The filter cake M1 obtained above was re-slurried with deionized water until it was uniform, and then 32.47g of potassium silicate with a SiO2 content of 25.72% was added for slurry treatment. The slurrying time was controlled to be 1 hour, and then the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid. The slurry was heated to 85°C and filtered to obtain filter cake M2. The filter cake obtained above was dried in a 120°C oven for 24 hours, and then calcined in a muffle furnace at 400°C for 6 hours to obtain catalyst 6.
[0062] Example 7
[0063] 404g Fe(NO3)3·9H2O, 10.62g Cu(NO3)2·3H2O, 1.78g Mg(NO3)2·6H2O and 11.17g PVP(K30) were added to deionized water and slurried to dissolve, and 1L solution was prepared, and stirred to fully dissolve to obtain solution A. 10.86g potassium silicate with SiO2 content of 25.72% was added to 1.7L Na2CO3 solution with a concentration of 1mol / L and stirred to obtain solution B.
[0064] Solution A was added to solution B for coprecipitation reaction. The precipitation reaction temperature was 85°C. The feeding time was controlled to be 15 minutes. The pH value of the final slurry was about 6.8. The precipitated filter cake was not aged and was directly filtered. It was then washed with deionized water for multiple times to control the final filtrate conductivity to be about 1000 μs / cm. The filter cake M1 obtained above was re-slurried with deionized water until it was uniform. Then 42.3 g of potassium silicate with a SiO2 content of 25.72% was added for slurry treatment. The slurrying time was controlled to be 1 hour. Then, the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid. The slurry was heated to 85°C and filtered to obtain filter cake M2. The filter cake obtained above was dried in a 120°C oven for 24 hours, and then calcined in a muffle furnace at 400°C for 6 hours to obtain catalyst 7.
[0065] Comparative Example 1
[0066] 404g Fe(NO3)3·9H2O, 10.62g Cu(NO3)2·3H2O, 65.829g Mg(NO3)2·6H2O and 11.17g PVP(K30) were added to deionized water and slurried to dissolve, and 1L solution was prepared, and stirred to fully dissolve to obtain solution A. 10.86g potassium silicate with SiO2 content of 25.72% was added to 1.7L Na2CO3 solution with a concentration of 1mol / L and stirred to obtain solution B.
[0067] Solution A was added to solution B for coprecipitation reaction, the precipitation reaction temperature was 85°C, the feeding time was controlled to be 20min, the pH value of the final slurry was about 6.8, the filter was filtered and washed with water, and the conductivity of the final filtrate was controlled to be about 1000μs / cm, the filter cake M1 obtained above was re-slurried with deionized water until it was uniform, and then 42.3g of potassium silicate with a SiO2 content of 25.72% was added for slurry treatment, the slurrying time was controlled to be 1h, and then the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid, and then the slurry was heated to 85°C and filtered to obtain filter cake M2. The filter cake obtained above was dried in a 120°C oven for 24h, and then calcined in a muffle furnace at 400°C for 6h to obtain control catalyst 1.
[0068] Comparative Example 2
[0069] 404g Fe(NO3)3·9H2O, 10.62g Cu(NO3)2·3H2O, 17.76g Mg(NO3)2·6H2O and 28g PVP(K30) were added to deionized water and slurried to dissolve, and 1L solution was prepared, and stirred to fully dissolve to obtain solution A. 10.86g potassium silicate with SiO2 content of 25.72% was added to 1.7L Na2CO3 solution with a concentration of 1mol / L and stirred to obtain solution B.
[0070] Solution A was added to solution B for coprecipitation reaction, the precipitation reaction temperature was 85°C, the feeding time was controlled to be 20min, the pH value of the final slurry was about 6.8, the filter was filtered and washed with water, and the conductivity of the final filtrate was controlled to be about 1000μs / cm, the filter cake M1 obtained above was re-slurried with deionized water until it was uniform, and then 42.3g of potassium silicate with a SiO2 content of 25.72% was added for slurry treatment, the slurrying time was controlled to be 1h, and then the pH value of the slurry was adjusted to about 6.8 with 20wt% dilute nitric acid, and then the slurry was heated to 85°C and filtered to obtain filter cake M2. The filter cake obtained above was dried in a 120°C oven for 24h, and then calcined in a muffle furnace at 400°C for 6h to obtain control catalyst 1.
[0071] The reaction performance results of the catalysts prepared in the examples and comparative examples are shown in Table 1.
[0072] Table 1 Reaction performance of catalysts
[0073]
[0074] Implementation effect:
[0075] The above experiments prove that the PVP-assisted Mg-modified catalyst is more conducive to the formation of MgFe2O4 spinel phase, promotes CO adsorption and dissociation, improves catalytic activity, and makes the catalyst show higher activity in the Fischer-Tropsch synthesis reaction, significantly improves catalytic efficiency, and can reduce the oxidation of the iron carbide active phase to generate Fe3O4 (water-gas shift reaction active phase) in the reaction, and reduce the selectivity of CO2. It has a significant implementation effect: the low-temperature Fischer-Tropsch synthesis catalyst can obtain a higher CO conversion rate, a lower CO2 selectivity, and a lower CH4 selectivity. In addition, the preparation method proposed in the present invention is simple and easy, the process conditions are mild, and no complicated equipment and operation are required, which is suitable for industrial production. At the same time, the required raw materials are easy to obtain and the cost is low, which has high economic efficiency. The successful implementation of the present invention provides new ideas and solutions for the technological progress in the field of Fischer-Tropsch synthesis, and lays a foundation for realizing a low-cost, high-efficiency, and high-selectivity Fischer-Tropsch synthesis reaction.
[0076] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing an iron-based catalyst, characterized in that: The following steps are involved: S1. Add the required amount of iron salt, copper salt, magnesium salt and PVP to an appropriate amount of deionized water, stir to fully dissolve, and obtain solution A; fully mix the required amount of precipitant and silicon source aqueous solution to obtain solution B; and keep the remaining required amount of silicon source for standby use, i.e., solution C; S2, mixing the above-mentioned solution A and solution B for coprecipitation reaction, and then performing solid-liquid separation and washing to obtain a filter cake M1; S3, adding deionized water to the filter cake M1 obtained above to re-slurry, then adding the C solution, continuing the slurry treatment, adjusting the pH value and temperature of the slurry, and then filtering to obtain the filter cake M2; S4, drying and calcining the filter cake M2 to obtain the iron-based catalyst; The above-mentioned magnesium salt and PVP can also be added in the following manner: first, the filter cake M2 obtained in S3 is re-slurried by adding an appropriate amount of deionized water, and then the required amount of one or both of the magnesium salt solution and PVP are added to the above-mentioned slurry; the slurry does not need to be filtered, but is directly dried and calcined to obtain the iron-based catalyst.
2. The preparation method according to claim 1, characterized in that: The iron salt, copper salt and magnesium salt are selected from nitrate, chloride, bicarbonate, ammonium salt, sulfate, organic salt, hydroxide or any mixture thereof; and / or, The specification of the PVP is one or more of K15, K30, and K60; and / or, The precipitant is selected from one or more of sodium carbonate, potassium carbonate, sodium hydroxide, ammonia water, ammonium carbonate, ammonium bicarbonate, and potassium hydroxide; and / or, The silicon source is selected from one or more of potassium silicate solution, sodium silicate solution, acidic or alkaline silica sol solution.
3. The preparation method according to claim 2, characterized in that: The mass ratio of each component in the iron-based catalyst is: Fe:Cu:Mg:K:Na:SiO2=100:(0-5):(0.2-10):(0.5-8):(0.5-3):(10-30).
4. The preparation method according to claim 2 or 3, characterized in that: The mass percentage of PVP during the synthesis of the iron-based catalyst is Fe:PVP=100:(1-40).
5. The preparation method according to claim 1, characterized in that: In step S1, The required amount of silicon source can be added in whole or in part to the precipitant solution to obtain solution B; or it can be used in whole or in part as a backup silicon source, namely solution C.
6. The preparation method according to claim 1, characterized in that: In step S2, The temperature for the coprecipitation reaction of the mixture of solution A and solution B is 50-90° C., the feeding time is 5-30 min, the pH value is 5.5-9.5 at the end of the reaction, and the aging is continued for 0-2 h after the feeding is completed; and / or, During the solid-liquid separation and washing process to obtain the filter cake M1, the conductivity of the filtrate is controlled at 300 to 3000 μs / cm.
7. The preparation method according to claim 1, characterized in that: Step S3 is specifically as follows: The filter cake M1 obtained above is re-slurried with deionized water, the slurry concentration of the slurry treatment is 7-25%, the slurrying time is 0.5-2h, and the slurrying temperature is 10-50°C; Then add solution C and continue beating, and the beating time is controlled at 0.5 to 2 hours; The pH value of the slurry is adjusted to about 5 to 9, and then the temperature of the slurry is raised to 50 to 90° C., and then filtered to obtain a filter cake M2.
8. The preparation method according to claim 1, characterized in that: In step S4, The drying process is air oven drying or vacuum oven drying. The air oven drying temperature is 80-150°C, preferably 90-120°C; the vacuum oven drying temperature is 20-80°C, preferably 40-60°C; the drying time is 1-30h, preferably 12-28h; And / or, the calcination temperature of the calcination process is 300-600°C, the heating rate is 0.5-2°C / min, and the calcination time is 4-10h; And / or, the calcined iron-based catalyst is sieved through 80-100 meshes.
9. An iron-based catalyst, characterized in that The preparation method is adopted according to any one of claims 1 to 8.
10. Use of the iron-based catalyst according to claim 9 in low-temperature Fischer-Tropsch synthesis, characterized in that: The reaction conditions of Fischer-Tropsch synthesis include: reaction temperature 210-275°C, reaction pressure 0.1-4MPa, molar ratio of H2 to CO in synthesis gas (1.0-3.0):1, reaction space velocity 8000-2000h -1 .
Citation Information
Patent Citations
Iron catalyst containing cobalt auxiliary agent for Fischer-Tropsch synthesis reaction and preparation method thereof
CN101602000A
Precipitated iron catalyst for catalyzing Fischer-Tropsch synthetic reaction and preparation method thereof
CN102688761A
Iron-based Fischer-Tropsch catalyst, and preparation method and application thereof, and Fischer-Tropsch synthetic method
CN105709742A
Preparation and application of carbon modified silicon dioxide carrier loaded iron-based catalyst for Fischer-Tropsch synthesis
CN106000404A
Low-temperature Fischer-Tropsch synthesis catalyst, preparation method and applications thereof
CN108620076A
Cited By
A modified Fe2O3-Al2O3 composite oxide, its preparation, and its application in Fischer-Tropsch synthesis.
CN122828738A