Catalyst for preparing higher alcohol from synthesis gas as well as preparation method and application of catalyst

By adjusting the proportion of metal active components and introducing alkali metals, a catalyst with efficient synergistic catalytic action was prepared, which solved the problem of low catalyst stability and selectivity in high carbon alcohols for syngas, and achieved high CO conversion and high carbon Alcohol selective, suitable for industrial applications.

CN118988330APending Publication Date: 2024-11-22YANKUANG ENERGY R&D CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411100664.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing synthetic gas high-carbon alcohol catalysts have problems such as poor catalyst stability, low alcohol selectivity, many by-products, low high-carbon alcohol content and limited ASF distribution, which is difficult to meet the needs of industrial applications.

Method used

By adjusting different proportions of metal active components, a catalyst including Fe, Cu, Zn, M and N is prepared, and a uniform distribution of active components is formed by co-precipitation, aging, washing, drying and calcining, and alkali metal is introduced to Regulate the acid-base distribution on the catalyst surface, improve CO conversion and high carbon alcohol selectivity.

Benefits of technology

The CO conversion rate is ≥75%, the total alcohol selectivity is ≥15%, the CH4 selectivity is ≤10%, and the spatiotemporal yield of C2+ alcohol reaches 80mg.gcat-1.h, which improves the stability of the catalyst and the high carbon alcohol. Selective, suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004989280690000111
    Figure BDA0004989280690000111
  • Figure BDA0004989280690000121
    Figure BDA0004989280690000121
Patent Text Reader

Abstract

The invention discloses a catalyst for preparing high alcohol from synthesis gas and a preparation method and application thereof, active components of the catalyst comprise Fe, Cu, Zn, M and N, M comprises at least one of Mn, Zr, La, Al and Sr, and N comprises one or more of K, Na and Cs; the molar ratio of Fe to Cu to Zn to M in the active components is (0.01-1): 2: 1: (0.01-0.1), and the mass ratio of N is 0.1-2%. The high-efficiency synergistic effect among the components is realized by adjusting the proportion of different active components, the preparation process is simple, the raw materials are cheap and easy to obtain, the CO conversion rate is more than or equal to 75%, the total alcohol selectivity is more than or equal to 15%, the CH4 selectivity is less than or equal to 10% and the C2 + alcohol STY reaches 80mg. Gcat-1. H in the process of preparing the high alcohol by catalyzing the synthesis gas, and the reaction activity and the high alcohol selectivity of the product can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparing higher carbon alcohols from synthesis gas, and in particular to a catalyst for preparing higher carbon alcohols from synthesis gas, and a preparation method and application thereof. Background Art

[0002] Syngas-to-alcohol not only broadens the supply of process raw materials for alcohol products and reduces production costs, but also provides opportunities and possibilities for downstream coal and natural gas chemical industries to enrich the product chain. The expected demand for alcohol products as fuels, fuel additives, chemical raw materials, and medical raw materials will increase significantly; while the research on syngas-to-mixed alcohols and high-carbon alcohols is still in the laboratory research stage, and there are still many problems that need to be solved in order to break through the thermodynamic limit of syngas-to-alcohol conversion and improve the activity and product selectivity of the catalyst.

[0003] Currently used to prepare C 2+ The catalytic systems for alcohols above OH mainly include Mo-based, Rh-based, modified methanol synthesis, and modified Fischer-Tropsch synthesis catalysts. The alcohol products on modified methanol catalysts and Mo-based catalysts are mainly C 1~5 OH, Mo-based catalysts use MoS2 as the main active component, and have strong resistance to poisoning and carbon deposition. Rh-based catalysts have high activity, but weak carbon chain growth ability, so the product generated is mainly ethanol, and the high price limits its industrial application. In contrast, the modified Fischer-Tropsch synthesis catalyst uses the ability of active components Co or Fe to dissociate and activate CO and promote carbon chain growth, regulates the active phase to improve the selectivity of alcohols, and is conducive to obtaining straight-chain primary alcohols with higher carbon numbers. The currently reported catalysts that can obtain C 6+ The catalyst for OH production mainly comes from the modified Fischer-Tropsch synthesis system.

[0004] Patent CN 118002187 A discloses a copper-based catalyst and its preparation method and application. The catalyst comprises an active component and a carrier, wherein the active component is Cu, the carrier is a modified all-silicon molecular sieve, and the active component is loaded on the surface and pores of the carrier, so that the catalyst has excellent activity, selectivity and stability, and can also ensure high catalytic activity when used at high temperatures. CN102319575B discloses a supported Cu-Fe-based catalyst obtained by impregnating SiO2 and Al2O3 for the synthesis of high-carbon alcohols from synthesis gas. European patent EP1017657B1 reports CuCoMn and CuCoMg catalysts for the synthesis of mixed alcohols. The catalyst is prepared by coprecipitation method, and the conversion rate of CO is only 14%.

[0005] After more than 40 years of development, modified Fischer-Tropsch catalysts for synthesis gas to produce mixed alcohols have made great progress in catalyst formulation development, reaction mechanism understanding, and catalyst synthesis methods. However, in order to meet the needs of industrial applications, further improving the selectivity of high-carbon alcohols, enhancing catalyst stability, and optimizing the reaction process all need systematic research. Summary of the invention

[0006] In order to overcome the problems of poor catalyst stability, low alcohol selectivity, high by-product content, low content of high alcohol, limited ASF distribution, wide distribution, etc. in the current synthesis gas to high alcohol catalyst, the present invention provides a synthesis gas to high alcohol catalyst and its preparation method and application, by adjusting different proportions of metal active components to achieve efficient synergistic catalytic effect between active components; the catalyst of the present invention achieves CO conversion rate ≥75%, total alcohol selectivity ≥15%, CH4 selectivity ≤10%, C 2+ The STY of alcohol reached 80mg.g cat -1 .h. The catalyst is used in the reaction of preparing high-carbon alcohols from synthesis gas, which can improve the conversion rate of CO, reduce the selectivity of CH4, and improve the selectivity of high-carbon alcohols.

[0007] According to a first aspect of the present invention, a catalyst for preparing higher alcohols from synthesis gas is provided, wherein the active components of the catalyst include Fe, Cu, Zn, M and N, wherein M includes at least one of Mn, Zr, La, Al and Sr, and N includes one or more of K, Na and Cs;

[0008] The molar ratio of Fe, Cu, Zn and M in the active component is (0.01-1):2:1:(0.01-0.1), and the mass proportion of N is 0.1-2%.

[0009] As a preferred embodiment, the M is one or two of Mn and Zr; the N is one or two of K and Na; the molar ratio of Fe, Cu, Zn and M in the active component is 0.05:2:1:0.04, and the mass proportion of N is 1%.

[0010] According to a second aspect of the present invention, there is further provided a method for preparing a catalyst for preparing higher alcohols from synthesis gas, comprising the following steps:

[0011] S1. According to the composition ratio of the catalyst, a metal salt containing Fe, Cu, Zn and M is weighed to prepare a mixed salt solution, and a precipitant is weighed to prepare a precipitant solution;

[0012] S2. adding the mixed salt solution and the precipitant solution to a container in parallel for coprecipitation reaction to obtain a reaction mixture, and aging the reaction mixture;

[0013] S3. The reaction mixture after aging is filtered, washed, dried and calcined to obtain a catalyst;

[0014] S4. Weigh the calcined catalyst, add alkali metal solution dropwise and perform ultrasonic treatment, and obtain an alkali metal modified catalyst after stirring, drying and calcining.

[0015] As a preferred embodiment, the metal salt is selected from one or more of nitrates, hydrochlorides, carbonates and sulfates;

[0016] The precipitant is selected from one or a mixture of sodium hydroxide, sodium carbonate, potassium carbonate and ammonium carbonate.

[0017] As a preferred embodiment, in step S2, the reaction temperature of the coprecipitation reaction is 30-80°C; the pH value of the reaction mixture is 6.0-9.0; the aging temperature is 30-80°C, and the time is 0.5-4h;

[0018] And / or, in step S3 and step S4, the drying temperature is 110°C and the time is 12 hours; the calcination temperature is 350-450°C and the time is 3-6 hours;

[0019] And / or, in step S4, the ultrasonic time is 30 minutes and the stirring time is 3 to 24 hours.

[0020] According to the third aspect of the present invention, there is further provided an application of a catalyst for preparing high-carbon alcohols from synthesis gas, wherein the reaction conditions for preparing high-carbon alcohols from synthesis gas are controlled as follows: the molar ratio of the reaction atmosphere is H2:CO:Ar=(3-8):(1-5):1, the reaction gas flow rate is 100-500 mL / min, the reaction temperature is 240-300°C, and the reaction space velocity is 1200-6000 mL / g cat / h.

[0021] As a preferred solution, it also includes a pre-reduction process of the catalyst, and the pre-reduced catalyst is used for preparing high-carbon alcohols from synthesis gas.

[0022] As a preferred embodiment, the reduction pressure of the pre-reduction process is 0.5 MPa, the reduction temperature is 250-400°C, the reduction time is 6-12h, the heating rate is 2°C / min, the reducing gas is H2, CO or a mixture of the two, and the reducing gas flow rate is 100 mL / min.

[0023] The present invention adopts the above technical solution to have at least the following beneficial effects:

[0024] 1. The present invention provides a catalyst for preparing high-carbon alcohols from synthesis gas, wherein the active components of the catalyst include Fe, Cu and Zn, and the catalyst preparation is controlled to achieve a phase composition of Cu-modified spinel metal oxides, such as ZnFe2O4, ZrZn2O4, MnFe2O4, etc. In the Cu-modified spinel metal oxide, Cu can replace part of Fe ions and enter the tetrahedral structure to form more oxygen vacancies, thereby promoting the adsorption and non-dissociative desorption of CO, which is beneficial to CO * Direct insertion of the intermediate, although not active in CC coupling, generates a large amount of CH x * monomer, but CH x * The intermediates can react with CO adsorbed on neighboring species. * The species react to promote the formation of alcohols; at the same time, the electron-donating property of Cu will also promote the electron transfer in the spinel oxide, improve the CO adsorption and insertion capacity and hydrogenation performance, and increase CH * 、CH2 * 、CH3 * In addition, the addition of zirconium oxide promoter, due to its amorphous and highly defective nature, will also promote the increase of catalyst surface area, the formation of metal carbides, the activation of H2 and the adsorption of CO, and also contribute to the stability of the structure;

[0025] 2. The present invention provides a catalyst for preparing high-carbon alcohols from synthesis gas, and also introduces an alkali metal. The addition of the alkali metal can, on the one hand, regulate the acid-base distribution on the catalyst surface, promote the adsorption and dissociation of CO, promote the reaction by enhancing linear CO adsorption and weakening bridging CO adsorption, and regulate the ratio of undissociated CO to dissociated CO, thereby providing sufficient * CH x and * CO Species Involved * CH x - * CO coupling reaction. K can also inhibit H2 activation, thereby inhibiting the alkylation reaction; K can affect the catalyst surface by regulating CO activation and H2 activation * CH x , * CO and * The balance of H species is adjusted to regulate the generation of alcohols. By adjusting the different proportions of metal active components to achieve efficient synergistic catalysis between active components, alkali metals are introduced to reduce CH4 selectivity and increase C 2+On the other hand, the addition of alkali metals, due to their electron-donating properties, can regulate the electronic environment on the Cu-modified spinel oxide, stabilize the generated formate intermediates, and then promote the formation of alcohol products and inhibit the formation of methane and CO2 in the products; finally, the medium and strong alkaline sites on the catalyst surface are increased at the same time, which accelerates the formation of formate and adsorbed CO to C2 intermediates and improves the selectivity of alcohols.

[0026] 3. The present invention provides a method for preparing a catalyst for preparing higher alcohols from synthesis gas, comprising steps of coprecipitation, aging, washing, drying and calcination, which help to form a uniform distribution of active components, improve the mechanical strength and thermal stability of the catalyst, and thus achieve long-term stable operation;

[0027] 4. The present invention provides an application of a catalyst for preparing high-carbon alcohols from synthesis gas. The catalyst has the characteristics of uniform composition, cheap and readily available raw materials, simple preparation method, and short preparation cycle, and is easy to be industrially produced on a large scale. When used in the catalytic reaction of preparing high-carbon alcohols from synthesis gas, the CO conversion rate is ≥75%, the total alcohol selectivity is ≥15%, the CH4 selectivity is ≤10%, and the C 2+ The STY of alcohol reached 80mg.g cat -1 .h. The catalyst is used in the reaction of preparing high-carbon alcohols from synthesis gas, which can improve the conversion rate of CO, reduce the selectivity of CH4, and improve the selectivity of high-carbon alcohols. DETAILED DESCRIPTION

[0028] The following is a detailed description of an embodiment of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiment.

[0029] Example 1

[0030] This embodiment provides a catalyst for preparing higher alcohols from synthesis gas, wherein the active components of the catalyst include Fe, Cu, Zn, M and N, wherein M includes at least one of Mn, Zr, La, Al and Sr, and N includes one or more of K, Na and Cs;

[0031] Specifically, the molar ratio of Fe, Cu, Zn and M is Fe:Cu:Zn:M=(0.01-1):2:1:(0.01-0.1), and the mass proportion of alkali metal in the catalyst is 0.1-2%.

[0032] Example 2

[0033] Based on Example 1, this example further provides a method for preparing the above catalyst, and the specific steps are as follows:

[0034] S1. According to the composition ratio of the catalyst, a metal salt containing Fe, Cu, Zn and M is weighed to prepare a mixed salt solution, and a precipitant is weighed to prepare a precipitant solution;

[0035] S2. The mixed salt solution and the precipitant solution are added to the container in parallel for coprecipitation reaction to obtain a reaction mixture, and the reaction mixture is aged;

[0036] S3. The reaction mixture after aging is filtered, washed, dried and calcined to obtain a catalyst;

[0037] S4. Weigh the calcined catalyst, add alkali metal solution dropwise and perform ultrasonic treatment, and obtain an alkali metal modified catalyst after stirring, drying and calcining.

[0038] In step 1, the metal salt containing Fe, Cu and Zn is iron nitrate, copper nitrate and zinc nitrate; the metal salt containing M is one of manganese nitrate, strontium nitrate, aluminum nitrate, zirconium nitrate and lanthanum nitrate; and the alkali metal salt containing N is one of cesium nitrate, potassium nitrate and sodium nitrate.

[0039] The above-mentioned Fe, Cu and Zn metal salt solutions can be respectively prepared into 1M metal salt solutions, and the amount of the metal salt solutions containing Fe, Cu and Zn can be calculated according to the molar ratio of the active components of the catalyst, and then the above-mentioned metal salt solutions are measured and evenly mixed to form a mixed salt solution. The mass of the metal salt M is calculated in proportion and dissolved in the mixed salt solution.

[0040] The above precipitant is potassium carbonate.

[0041] In step 2, the flow rates of the mixed salt solution and the precipitant solution are controlled by a peristaltic pump, and the mixed salt solution and the precipitant solution are added into a three-necked flask with a stirrer for co-precipitation reaction to obtain a reaction mixture. The preferred reaction temperature is 70° C., and the pH value of the reaction mixture is maintained at 7.0. After the mixed salt solution and the precipitant solution are added dropwise, the mixture is stirred at 70° C. for aging for 2 hours.

[0042] In step 3, after aging, the reaction mixture is naturally cooled to 20°C and then filtered and washed with deionized water. The reaction mixture is placed in an oven at 110°C for 12 hours for drying and then calcined in a muffle furnace at 450°C for 5 hours to obtain the catalyst.

[0043] In step 4, the ultrasonic immersion time is 30 minutes, the stirring time is continued for 12 hours, the drying temperature is 110° C., the time is 12 hours, and then calcined at 450° C. in a muffle furnace for 5 hours.

[0044] Example 3

[0045] In this embodiment, the application of the catalyst provided by the present invention in the reaction of hydrogenating synthesis gas to produce higher alcohols is described. First, the catalyst is pre-reduced, and the preferred pre-reduction conditions are: the reducing gas is H2, the flow rate of the reducing gas is 100 mL / min, the reducing pressure is 0.5 MPa, the reducing temperature is 300°C, the reducing time is 10 h, and the heating rate is 2°C / min.

[0046] The pre-reduced catalyst was then used in the synthesis gas to produce high-carbon alcohol reaction process. The catalytic reaction conditions were: H2 / CO / Ar in the reaction atmosphere = 6 / 3 / 1, the reaction gas flow rate was 300 mL / min, the reaction temperature was 260°C, and the reaction space velocity was 3600 mL / g cat / h.

[0047] The reactor for the process of preparing high-carbon alcohols from synthesis gas catalyzed by the catalyst is a fixed bed reactor, a fluidized bed reactor or a slurry bed reactor, and its specific structure and form are not specifically limited in this embodiment.

[0048] In order to better understand and apply the above scheme and effectively demonstrate the corresponding benefits, the catalyst for preparing higher carbon alcohols from synthesis gas provided by the present invention, its preparation method and application are further described below in combination with specific embodiments.

[0049] Example 4

[0050] First, copper nitrate, iron nitrate, zinc nitrate and potassium carbonate (precipitant) were dissolved in deionized water to prepare a 1M solution. 100 mL of 1M copper nitrate solution, 50 mL of 1M iron nitrate solution, 50 mL of 1M zinc nitrate solution and 0.86 g of zirconium nitrate were measured and evenly mixed in a 500 mL beaker to prepare a mixed salt solution. 600 mL of 1M potassium carbonate solution was measured in a 500 mL measuring cylinder.

[0051] The mixed salt solution and potassium carbonate solution were added dropwise in parallel into a three-necked flask with a stirrer for coprecipitation reaction to obtain a reaction mixture, the reaction temperature was maintained at 70°C, the dropping speed of the potassium carbonate solution was adjusted by a peristaltic pump, the pH value was controlled to be 7.0, and after the dropping was completed, the temperature was maintained at 70°C and stirring was continued for 2 hours of aging;

[0052] After the aging reaction, the reaction mixture was naturally cooled to 20°C, filtered and washed with deionized water, dried at 110°C for 12 hours, and then calcined in a muffle furnace at 450°C for 5 hours to obtain Fe1Cu2Zn1Zr 0.04 catalyst.

[0053] Take 5g Fe1Cu2Zn1Zr 0.04Catalyst, add 0.13g potassium nitrate and 20mL deionized water, immerse in ultrasound for 30min, continue stirring for 12h, dry at 110℃ for 12h, then calcine at 450℃ in a muffle furnace for 5h.

[0054] K1Fe1Cu2Zn1Zr 0.04 Catalyst activity test:

[0055] First, the catalyst was pre-reduced, and the pre-reduction conditions were: reducing gas was H2, the reducing gas flow rate was 100 mL / min, the reducing pressure was 0.5 MPa, the reducing temperature was 300°C, the reducing time was 10 h, and the heating rate was 2°C / min.

[0056] The pre-reduced catalyst was then used in the synthesis gas to produce high-carbon alcohol reaction process. The catalytic reaction conditions were: H2 / CO / Ar in the reaction atmosphere = 6 / 3 / 1, the reaction gas flow rate was 300 mL / min, the reaction temperature was 260°C, and the reaction space velocity was 3600 mL / g cat / h, the catalytic performance results are shown in Table 1.

[0057] Example 5

[0058] Referring to Example 4, the difference is that the 0.86g zirconium nitrate in Example 4 is replaced with 0.72g 50% manganese nitrate solution, and the other preparation conditions are the same as those in Example 4 to obtain K1Fe1Cu2Zn1Mn 0.04 catalyst.

[0059] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0060] Example 6

[0061] Referring to Example 4, the difference is that the 0.86g zirconium nitrate in Example 4 is replaced by 0.75g aluminum nitrate nonahydrate, and the other preparation conditions are the same as those in Example 4 to obtain K1Fe1Cu2Zn1Al 0.04 catalyst.

[0062] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0063] Example 7

[0064] Referring to Example 4, the difference is that the 0.86g zirconium nitrate in Example 4 is changed to 0.65g lanthanum nitrate, and the other preparation conditions are the same as those in Example 4 to obtain K1Fe1Cu2Zn1La 0.04 catalyst.

[0065] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0066] Example 8

[0067] Refer to Example 4, except that 0.86g of zirconium nitrate in Example 4 is replaced by 0.42g of strontium nitrate, and the other preparation conditions are the same as those in Example 4 to obtain K1Fe1Cu2Zn1Sr 0.04 catalyst.

[0068] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0069] Example 9

[0070] Referring to Example 4, the difference is that 0.13g potassium nitrate in Example 4 is replaced by 0.19g sodium nitrate, and the other preparation conditions are the same as those in Example 4 to obtain Na1Fe1Cu2Zn1Zr 0.04 catalyst.

[0071] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0072] Example 10

[0073] Referring to Example 4, the difference is that 0.13g potassium nitrate in Example 4 is replaced by 0.12g cesium nitrate, and the other preparation conditions are the same as those in Example 4 to obtain Cs1Fe1Cu2Zn1Zr 0.04 catalyst.

[0074] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0075] Embodiment 11

[0076] Refer to Example 4, except that 0.13g potassium nitrate in Example 4 is changed to 0.013g potassium nitrate, and other preparation conditions are the same as those in Example 4 to obtain K 0.1 Fe1Cu2Zn1Zr 0.04 catalyst.

[0077] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0078] Example 12

[0079] Referring to Example 4, the difference is that 0.13g potassium nitrate in Example 4 is changed to 0.26g potassium nitrate, and the other preparation conditions are the same as those in Example 4 to obtain K2Fe1Cu2Zn1Zr0.04 catalyst.

[0080] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0081] Example 13

[0082] Refer to Example 4, except that 0.86g of zirconium nitrate in Example 4 is replaced by 0.215g of zirconium nitrate, and other preparation conditions are the same as those in Example 4 to obtain K1Fe1Cu2Zn1Zr 0.01 catalyst.

[0083] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0084] Embodiment 14

[0085] Refer to Example 4, except that 0.86g of zirconium nitrate in Example 4 is replaced by 1.505g of zirconium nitrate, and other preparation conditions are the same as those in Example 4 to obtain K1Fe1Cu2Zn1Zr 0.07 catalyst.

[0086] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0087] Embodiment 15

[0088] Refer to Example 4, except that 0.86g of zirconium nitrate in Example 4 is changed to 2.15g of zirconium nitrate, and other preparation conditions are the same as those in Example 4 to obtain K1Fe1Cu2Zn1Zr 0.1 catalyst.

[0089] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0090] Example 16

[0091] Refer to Example 4, except that 50 mL of 1M ferric nitrate solution in Example 4 was replaced with 25 mL of 1M ferric nitrate solution, and other preparation conditions were the same as those in Example 4 to obtain K1Fe 0.5 Cu2Zn1Zr 0.04 catalyst.

[0092] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0093] Embodiment 17

[0094] Referring to Example 4, the difference is that 50 mL of 1M ferric nitrate solution in Example 4 is changed to 2.5 mL of 1M ferric nitrate solution, and the other preparation conditions are the same as those in Example 4, to obtain

[0095] K1Fe 0.05 Cu2Zn1Zr 0.04 catalyst.

[0096] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0097] Comparative Example 1

[0098] Referring to Example 4, the difference is that M nitrate is not added when preparing the mixed salt solution, and alkali metal is not introduced. Other preparation conditions are the same as those of Example 4 to obtain Fe1Cu2Zn1 catalyst.

[0099] The activity test conditions were the same as those in Example 4. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0100] Table 1. Catalytic performance results of different catalysts in Examples 4 to 17 and Comparative Example 1

[0101]

[0102]

[0103] As shown in Table 1, the catalysts obtained in Examples 4-8 differ from those in Comparative Example 1 in that an active component M is added during the preparation process. Among the several metals introduced, Mn metal has the highest total alcohol selectivity of 35.07%, but the introduction of Mn metal results in a low CO conversion rate of the catalyst. After the introduction of Zr metal, the CO conversion rate is significantly improved to 78.61%, which is much higher than that of the other metals. Although the introduction of Zr does not greatly increase the selectivity of the total alcohol of the product, the space-time yield of ROH reaches about 100 mg / gh.

[0104] The catalysts obtained in Examples 9-12 differ from those in Example 4 in that alkali metals Na and Cs are introduced during the preparation process, and the content of alkali metal K is adjusted. Na, K, and Cs increase the proportion of C2 alcohols and reduce the selectivity of CH4. Therefore, the introduction of alkali metals is beneficial to the C 2+ Alcohol production.

[0105] The catalysts obtained in Examples 13-15 are different from those in Example 4 in that the content of metal Zr is changed during the preparation process. The excessive introduction of Zr cannot improve the reaction performance of the catalyst, but instead reduces the CO conversion rate. This may be because the excess Zr changes the structure of the FeCuZn catalyst, thereby reducing the reaction performance of the catalyst.

[0106] The catalysts obtained in Examples 16-17 differ from those in Example 4 in that the proportion of Fe is changed. When the Fe content is controlled to 0.5, the CO conversion rate decreases, the CO2 selectivity increases, and the total alcohol selectivity decreases; when the Fe content is controlled to 0.05, the CO conversion rate further decreases, and the CO2 selectivity is relatively low, but the total alcohol selectivity increases from 12.44% to 30.71%. This indicates that the addition of Fe metal elements affects the catalytic reaction activity and product selectivity, and as the Fe element content gradually decreases, the CO conversion rate gradually decreases, and the selectivity of alcohol products shows a trend of first decreasing and then increasing.

[0107] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea, including the best mode, and also enables any technician in the field to practice the present invention, including the manufacture and use of any device or system, and the implementation of any combined method.

[0108] It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A catalyst for preparing higher alcohols from synthesis gas, characterized in that: The active components of the catalyst include Fe, Cu, Zn, M and N, wherein M includes at least one of Mn, Zr, La, Al and Sr, and N includes one or more of K, Na and Cs; The molar ratio of Fe, Cu, Zn and M in the active component is (0.01-1):2:1:(0.01-0.1), and the mass proportion of N is 0.1%-2%.

2. The catalyst according to claim 1, characterized in that The M is one or two of Mn and Zr; The N is one or both of K and Na; The molar ratio of Fe, Cu, Zn and M in the active component is 0.05:2:1:0.04, and the mass proportion of N is 1%.

3. A method for preparing a catalyst for preparing higher alcohols from synthesis gas, characterized in that: The preparation method is used to prepare the catalyst according to claim 1 or 2, and specifically comprises the following steps: S1. According to the composition ratio of the catalyst, a metal salt containing Fe, Cu, Zn and M is weighed to prepare a mixed salt solution, and a precipitant is weighed to prepare a precipitant solution; S2. adding the mixed salt solution and the precipitant solution to a container in parallel for coprecipitation reaction to obtain a reaction mixture, and aging the reaction mixture; S3. The reaction mixture after aging is filtered, washed, dried and calcined to obtain a catalyst; S4. Weigh the calcined catalyst, add alkali metal solution dropwise and perform ultrasonic treatment, and obtain an alkali metal modified catalyst after stirring, drying and calcining.

4. The preparation method according to claim 3, characterized in that: The metal salt is selected from one or more of nitrates, hydrochlorides, carbonates and sulfates; The precipitant is selected from one or a mixture of sodium hydroxide, sodium carbonate, potassium carbonate and ammonium carbonate.

5. The preparation method according to claim 3, characterized in that: In step S2, the reaction temperature of the coprecipitation reaction is 30-80°C; the pH value of the reaction mixture is 6.0-9.0; the aging temperature is 30-80°C and the time is 0.5-4h; And / or, in step S3 and step S4, the drying temperature is 110°C and the time is 12 hours; the calcination temperature is 350-450°C and the time is 3-6 hours; And / or, in step S4, the ultrasonic time is 30 minutes and the stirring time is 3 to 24 hours.

6. An application of a catalyst for preparing higher alcohols from synthesis gas, characterized in that: The catalyst according to claim 1 or 2, or the catalyst prepared by the preparation method according to any one of claims 3 to 5, is used to catalyze synthesis gas to produce higher carbon alcohols.

7. The use according to claim 6, characterized in that: The reaction conditions for synthesizing high-carbon alcohols from syngas are controlled as follows: the molar ratio of the reaction atmosphere is H2:CO:Ar=6:3:1, the reaction gas flow rate is 100-500mL / min, the reaction temperature is 240-300℃, and the reaction space velocity is 1200-6000mL / g cat / h.

8. The use according to claim 6, characterized in that: The method also includes a pre-reduction process of the catalyst, and the pre-reduced catalyst is used to prepare high-carbon alcohols from synthesis gas.

9. The use according to claim 8, characterized in that: The reduction pressure of the pre-reduction process is 0.5MPa, the reduction temperature is 250-400°C, the reduction time is 6-12h, the heating rate is 2°C / min, the reduction gas is H2, CO or a mixture of the two, and the flow rate of the reduction gas is 100mL / min.

Citation Information

Patent Citations

  • Iron-copper based catalyst for synthesizing low carbon mixed alcohol and production method and use

    CN101327435A

  • A catalyst for the synthesis of C2-C25 higher primary alcohols by CO hydrogenation and its preparation method.

    CN102266778A

  • Hydrogenation catalyst and process for its production

    DE102014004413A1