Activated carbon loaded porous silicon dioxide material as well as preparation method and application thereof
Through activated carbon-loaded porous silica material with in-situ loading and porous treatment on activated carbon, the problem of difficulty in removing impurities in polycrystalline silicon is solved, the adsorption efficiency and product quality are improved, the preparation process is simplified, and the trichlorodichlorodioxide is realized Efficient removal of phosphorus impurities in the middle.
Patent Information
- Application Number
- CN202411033715.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, impurities and impurities of trichlorosilicon during the polycrystalline silicon production process are difficult to effectively remove, especially phosphorus elements, which leads to the impact of product quality. In addition, the surface functional groups of existing adsorbent materials such as activated carbon are weak, the adsorption selectivity is poor, and silica is loaded. The process is complicated and the binding force is not strong, resulting in a single adsorption effect.
The preparation method of activated carbon-loaded porous silica material is adopted. The silane precursor is hydrolyzed and condensed on the surface of activated carbon to form silica, and is loaded in situ on the activated carbon, combined with pore-generating treatment, and the adsorption capacity is improved.
It significantly improves the adsorption efficiency and capacity, enhances the adsorption effect, and is particularly suitable for removing phosphorus impurities in trichlorosilicon, improves the quality of polycrystalline silicon products, simplifies the preparation process, and enhances the binding force between silica and activated carbon.
Smart Images

Figure CN118988248A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an activated carbon-loaded porous silicon dioxide material and a preparation method and application thereof. Background Art
[0002] In the synthesis step of trichlorosilane, the intermediate product of polysilicon production process, the raw silicon powder contains various metal and non-metal impurities, and the raw hydrogen chloride is not a high-purity gas, which contains some impurity gases. Therefore, the product trichlorosilane also contains many impurities caused by side reactions, such as: AlCl3, ZnCl2, CrCl3, TiCl4, PbCl2, AgCl, BCl3, CCl4, CaCl2, CuCl2, PCl3, etc. If it is not purified or not purified deeply, these impurities will also exist in polysilicon. Among them, phosphorus is an important impurity that affects the quality of polysilicon products, so its content must be very low.
[0003] To achieve this goal, researchers have widely adopted adsorption methods with high separation efficiency and low equipment investment. Among them, activated carbon, as a key adsorption material, still has problems such as weak surface functional groups and poor adsorption selectivity. Silica is another adsorbent with excellent performance, which has the characteristics of high specific surface area, high mechanical strength, and high temperature resistance. Therefore, the preparation of activated carbon-loaded silica materials is an important way to develop new adsorbents.
[0004] However, the silica loaded in the products of existing preparation methods are mostly solid spheres, which only have secondary pores formed by the aggregation of activated carbon and silica. They have no adsorption effect on smaller molecular impurities and have a single effect. In addition, silica is usually synthesized first and then loaded on activated carbon. There are many steps and a complicated process. In addition, the solid sphere silica has a weak bonding force with the activated carbon carrier, which can easily lead to the collapse of the secondary pores, causing the silica to fall off, affecting the adsorption performance, and even contaminating the adsorption sample. Porous silica is even more difficult to load. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide an activated carbon-loaded porous silica material and a preparation method and application thereof in view of the above-mentioned deficiencies in the prior art. The material has three or more levels of pores, which can greatly increase the size range of adsorbable molecules, has a good adsorption effect, and has a simple preparation process. The silica and activated carbon carrier have a stronger binding force. The material is particularly suitable for occasions such as chlorosilane adsorption and phosphorus removal, can effectively improve the quality of polysilicon products, and has great application prospects.
[0006] The technical solution of the present invention to solve the above technical problems is:
[0007] According to a first aspect of the present invention, there is provided a method for preparing an activated carbon-supported porous silica material, comprising:
[0008] (1) mixing ethanol and water evenly, adding an appropriate amount of silane precursor, and mixing again evenly to prepare a silane precursor solution;
[0009] (2) adding an appropriate amount of activated carbon to the silane precursor solution, mixing evenly, then adding an initiator, stirring for a period of time under certain stirring conditions, so that the silane precursor undergoes a hydrolysis and condensation reaction to generate silicon dioxide and in-situ loads the silicon dioxide on the activated carbon, thereby obtaining activated carbon-loaded silicon dioxide;
[0010] (3) Dispersing the activated carbon-loaded silica into water, adding a protective agent, boiling and refluxing for a period of time and then cooling, then adding an appropriate amount of a porogen, stirring and etching for a period of time, washing, drying, and calcining to obtain an activated carbon-loaded porous silica material.
[0011] Optionally, the volume ratio of ethanol to water is 1 to 3:1.
[0012] Optionally, the volume ratio of the amount of the silane precursor to the total amount of ethanol and water is 1:1-24.
[0013] Optionally, the silane precursor is one or a combination of ethyl orthosilicate, methyl orthosilicate, polysiloxane, methyltrimethoxysilane, methyltriethoxysilane, and 3-(aminopropyl)triethoxysilane.
[0014] Optionally, the activated carbon is one or a combination of coal-based activated carbon, fruit shell activated carbon, wood-based activated carbon, and petroleum-based activated carbon.
[0015] Optionally, the initiator is aqueous ammonia, and the volume ratio of aqueous ammonia to the silane precursor is 1 to 4:1.
[0016] Optionally, in step (2), the stirring speed is ≥500 rpm / min, and the stirring time is 2 to 10 h.
[0017] Optionally, the protective agent is polyvinyl pyrrolidone, and the mass ratio of polyvinyl pyrrolidone to ammonia water is 1:1-3.
[0018] Optionally, the boiling reflux time is 2 to 5 hours.
[0019] Optionally, the porogen is a sodium hydroxide solution, the concentration of the sodium hydroxide solution is 1 to 3 mol / L, the volume ratio of the sodium hydroxide solution to ammonia water is 1 to 8:1, and the stirring etching time is 1 to 3 hours.
[0020] According to a second aspect of the present invention, there is provided an activated carbon-loaded porous silica material, which is prepared by the preparation method described above, and the activated carbon-loaded porous silica material comprises at least three levels of pores, namely, a first pore located on the activated carbon, a second pore located between silica and the activated carbon and between silica and silica, and a third pore located on the silica.
[0021] According to a third aspect of the present invention, there is provided an application of an activated carbon-loaded porous silica material, wherein the activated carbon-loaded porous silica material is used for adsorbing and removing phosphorus impurities in trichlorosilane.
[0022] Compared with the prior art, the activated carbon-loaded porous silica material and the preparation method and application thereof of the present invention have the following beneficial effects:
[0023] (1) The material prepared by this method combines the macroporous structure of activated carbon and loads porous silica, so that the material has three levels of pores (the first pores of the activated carbon itself, the second pores formed by the aggregation of silica, and the third pores formed by the pores of silica) or even more pores, which further increases the specific surface area and the number of active sites of the material, and can greatly increase the size range of adsorbable molecules, especially the adsorption capacity of small molecules, thereby improving the adsorption efficiency and adsorption capacity of the material and enhancing the adsorption effect.
[0024] (2) This method utilizes the hydrolysis and condensation of silane precursors on the surface and in the pores of activated carbon to generate solid silica spheres. The prepared silica can be directly loaded on the surface of activated carbon in situ while preparing the silica. This method has fewer steps and a simpler process. In addition, the silica has a stronger binding force with the activated carbon carrier, which can prevent the silica from falling off and form a stable secondary pore.
[0025] (3) The loading of silica on the surface and pores of activated carbon is achieved through the hydrolysis and condensation of silane precursors. Compared with the commonly used method of using sodium silicate as a silicon source and then calcining by the sol-gel method, the conditions are milder and simpler. In addition, when the silica generated by hydrolysis and condensation is loaded on the surface or pores of activated carbon, it can also form pores between particles due to aggregation, thereby increasing the specific surface area of the material, and then increasing the material's adsorption active sites, greatly enhancing the material's adsorption effect.
[0026] (4) The material prepared by this method is particularly suitable for use in chlorosilane adsorption and phosphorus removal, and can more thoroughly remove phosphorus impurities in trichlorosilane, effectively improving the quality of polysilicon products, but is not limited to this, and has great application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The present invention is a flowchart of a method for preparing an activated carbon-loaded porous silica material according to an embodiment of the present invention. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings in the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the protection scope of the present invention.
[0029] In view of the problems of single effect and complicated process in the prior art, the present invention discloses a method for preparing an activated carbon-loaded porous silica material, comprising:
[0030] (1) mixing ethanol and water evenly, adding an appropriate amount of silane precursor, and mixing again evenly to prepare a silane precursor solution;
[0031] (2) adding an appropriate amount of activated carbon to the silane precursor solution, mixing evenly, then adding an initiator, stirring for a period of time under certain stirring conditions, so that the silane precursor undergoes a hydrolysis and condensation reaction to generate silicon dioxide and in-situ loads the silicon dioxide on the activated carbon, thereby obtaining activated carbon-loaded silicon dioxide;
[0032] (3) Dispersing the activated carbon-loaded silica into water, adding a protective agent, boiling and refluxing for a period of time and then cooling, then adding an appropriate amount of a porogen, stirring and etching for a period of time, washing, drying, and calcining to obtain an activated carbon-loaded porous silica material.
[0033] Correspondingly, the present invention also discloses activated carbon-loaded porous silica materials prepared by more than one method and applications thereof.
[0034] Example 1
[0035] like Figure 1 As shown, this embodiment discloses a method for preparing an activated carbon-supported porous silica material, comprising:
[0036] (1) Preparation of silane precursor solution: ethanol and water are mixed evenly, an appropriate amount of silane precursor is added, and the mixture is mixed evenly again to prepare a silane precursor solution;
[0037] (2) Preparation of activated carbon-supported silica: Add an appropriate amount of activated carbon to the silane precursor solution obtained in step S1, mix well, then add a small amount of initiator, and stir for a period of time under certain stirring conditions to allow the silane precursor to undergo hydrolysis and condensation reaction to generate silica and load it in situ on the activated carbon to obtain activated carbon-supported silica. Compared with the prior art in which silica is first prepared and then loaded on activated carbon, the present method directly hydrolyzes and condenses the silane precursor on the surface of activated carbon to form solid silica spheres. In other words, while preparing silica, the prepared silica is directly loaded on the surface of activated carbon, and the process is simpler.
[0038] (3) Etching pores of silica: Activated carbon-loaded silica is dispersed in water, and a protective agent is added. After boiling and refluxing for a period of time, the protective agent is allowed to adhere to the surface of the silica solid spheres to ensure that the silica after pores are formed can maintain a spherical shape. Then, an appropriate amount of pore-forming agent is added, and the solid silica is etched to form pores. After washing, drying, and calcining, an activated carbon-loaded porous silica material is obtained.
[0039] In some embodiments, the volume ratio of ethanol to water is 1 to 3:1, so as not to affect the particle size and morphology of silica, thereby affecting the adsorption performance of the product.
[0040] In some embodiments, the volume ratio of the amount of silane precursor to the total amount of ethanol and water is 1:1-24, so as not to affect the particle size and morphology of silica, thereby affecting the adsorption performance of the product.
[0041] In some embodiments, the silane precursor is one or more of tetraethyl orthosilicate (TEOS), methyl orthosilicate (TMOS), polysiloxane (PEDS), methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), 3-(aminopropyl)triethoxysilane (APTES), but is not limited thereto, and may also be other silicon-containing organic matter that can undergo hydrolysis and condensation reactions. Compared with the commonly used method of using sodium silicate as a silicon source and then calcining by a sol-gel method in the prior art, the conditions are mild and more convenient.
[0042] In some embodiments, the amount of activated carbon used is 20-40 g for every 250-300 mL of silane precursor solution.
[0043] In some embodiments, the activated carbon is one or a combination of coal-based activated carbon, fruit shell (core) activated carbon, wood-based activated carbon, and petroleum-based activated carbon.
[0044] In some embodiments, the initiator is aqueous ammonia, which has an ammonia content of 25% to 27% at room temperature, but is not limited thereto, and may also be a sodium hydroxide solution or the like; the volume ratio of aqueous ammonia to silane precursor is 1 to 4:1 to control the pH of the solution within an appropriate range to avoid affecting the particle size and morphology of silica.
[0045] In some embodiments, in step (2), the stirring speed is ≥500 rpm / min and the stirring time is 2 to 10 h to control the morphology, particle size and dispersibility of the silica.
[0046] In some embodiments, the protective agent is polyvinyl pyrrolidone, and the mass ratio of polyvinyl pyrrolidone to ammonia water is 1:1-3.
[0047] In some embodiments, the boiling reflux time is 2 to 5 hours.
[0048] In some embodiments, the porogen is a sodium hydroxide solution, the concentration of the sodium hydroxide solution is 1 to 3 mol / L, but not limited thereto. The volume ratio of the sodium hydroxide solution to ammonia water is 1 to 8:1, and the stirring etching time is 1 to 3 hours.
[0049] In the method of this embodiment, during the preparation process, the specific surface area of activated carbon-supported silica can be controlled (up to 1100 m2 / g or more) by combining the type of activated carbon matrix and silane precursor, the amount added, the treatment conditions (temperature, time, etc.), and the stirring method (mechanical stirring, magnetic stirring, etc.), thereby achieving the purpose of adjusting the phosphorus removal adsorption effect. At the same time, by adjusting the concentration of sodium hydroxide and the treatment time, the number of active sites of the activated carbon-supported silica material is increased, and the selective adsorption of activated carbon to phosphorus impurities is increased, thereby effectively improving the adsorption effect of the adsorbent.
[0050] Compared with the prior art, the method for preparing the activated carbon-supported porous silica material of this embodiment has at least the following effects:
[0051] (1) The material prepared by this method combines the macroporous structure of activated carbon and loads porous silica, so that the material has three levels of pores (the first pores of the activated carbon itself, the second pores formed by the aggregation of silica, and the third pores formed by the pores of silica) or even more pores, which further increases the specific surface area and the number of active sites of the material, and can greatly increase the size range of adsorbable molecules, especially the adsorption capacity of small molecules, thereby improving the adsorption efficiency and adsorption capacity of the material and enhancing the adsorption effect.
[0052] (2) This method utilizes the hydrolysis and condensation of silane precursors on the surface and in the pores of activated carbon to generate solid silica spheres. The prepared silica can be directly loaded on the surface of activated carbon in situ while preparing the silica. This method has fewer steps and a simpler process. In addition, the silica has a stronger binding force with the activated carbon carrier, which can prevent the silica from falling off and form a stable secondary pore.
[0053] (3) The loading of silica on the surface and pores of activated carbon is achieved through the hydrolysis and condensation of silane precursors. Compared with the commonly used method of using sodium silicate as a silicon source and then calcining by the sol-gel method, the conditions are milder and simpler. In addition, when the silica generated by hydrolysis and condensation is loaded on the surface or pores of activated carbon, it can also form pores between particles due to aggregation, thereby increasing the specific surface area of the material, and then increasing the material's adsorption active sites, greatly enhancing the material's adsorption effect.
[0054] (4) The material prepared by this method is particularly suitable for use in chlorosilane adsorption and phosphorus removal, and can more thoroughly remove phosphorus impurities in trichlorosilane, effectively improving the quality of polysilicon products, but is not limited to this, and has great application prospects.
[0055] Example 2
[0056] This embodiment discloses an activated carbon-loaded porous silica material, which is prepared by the preparation method described above. The activated carbon-loaded porous silica material includes at least three levels of pores, namely, a first pore located on the activated carbon, a second pore located between silica and the activated carbon and between silica and silica, and a third pore located on the silica.
[0057] Compared with the prior art in which the loaded silica is mostly solid spheres, resulting in only secondary pores formed by the aggregation of activated carbon and silica, the silica loaded on the activated carbon-loaded porous silica material in this embodiment is porous silica, having three or more pores (the first pore of the activated carbon itself, the second pore formed by the aggregation of silica, and the third pore formed by the pores of silica) and above, a large specific surface area, a large number of active sites, which can greatly increase the size range of adsorbable molecules, have a good adsorption effect, and a simple preparation process. The silica and activated carbon carrier have a stronger binding force, which can prevent the silica from falling off and form a stable secondary pore. The material is particularly suitable for use in chlorosilane adsorption and phosphorus removal and other occasions, and can effectively improve the quality of polysilicon products, but is not limited to this, and has great application prospects.
[0058] Example 3
[0059] This embodiment discloses an application of the above-mentioned activated carbon-loaded porous silica material, wherein the activated carbon-loaded porous silica material is used for phosphorus removal by adsorption of chlorosilane, more specifically, for adsorption and removal of phosphorus impurities in trichlorosilane, but is not limited thereto and can also be used in other fields.
[0060] Compared with the prior art, the above-mentioned activated carbon-loaded porous silica material is used to adsorb and remove phosphorus impurities in trichlorosilane, and the adsorption effect is better. The phosphorus impurity removal rate can reach more than 75%, which can effectively improve the quality of polysilicon products. In addition, the material preparation process is simple and has great application prospects.
[0061] Example 4
[0062] This embodiment discloses an activated carbon-loaded porous silica material, comprising the following steps:
[0063] (1) Preparation of silane precursor solution: In a beaker, weigh 210 mL of anhydrous ethanol and 70 mL of deionized water, mix them evenly, add 50 mL of TEOS, and mix them evenly again to prepare a silane precursor solution;
[0064] (2) Preparation of activated carbon-supported silica: Weigh 30 g of coconut shell activated carbon and add it to the above-mentioned silane precursor solution, mix well, then add 50 mL of ammonia water with an ammonia content of 25% to 27% at room temperature, and stir at a stirring speed of 500 rpm / min for 2 h to allow the silane precursor to hydrolyze and condense to generate silica and load it in situ on the activated carbon to obtain activated carbon-supported silica. The product was repeatedly washed with deionized water and ethanol for 3 times.
[0065] (3) Preparation of activated carbon-supported porous silica: The product of step (2) was dispersed in 300 mL of deionized water, 20 g of polyvinyl pyrrolidone was added, and the mixture was boiled and refluxed for 3 h, then cooled. Then 100 mL of 2 mol / L sodium hydroxide solution was added, and the mixture was stirred and etched for 3 h. The etched product was washed with water, dried at 105 °C for 2 h, and calcined in a muffle furnace at 550 °C for 4 h to obtain an activated carbon-supported porous silica material, which was recorded as product 1.
[0066] Example 5
[0067] This embodiment discloses an activated carbon-loaded porous silica material, comprising the following steps:
[0068] (1) Preparation of silane precursor solution: In a beaker, weigh 210 mL of anhydrous ethanol and 70 mL of deionized water, mix them evenly, add 20 mL of TEOS and 30 mL of MTMS, and mix them evenly again to prepare a silane precursor solution;
[0069] (2) Preparation of activated carbon-supported silica: Weigh 30 g of activated carbon and add it to the above-mentioned silane precursor solution, mix well, then add 50 mL of ammonia water with an ammonia content of 25% to 27% at room temperature, and stir at a stirring speed of 500 rpm / min for 2 h to allow the silane precursor to hydrolyze and condense to generate silica and load it in situ on the activated carbon to obtain activated carbon-supported silica. The product was repeatedly washed with deionized water and ethanol for 3 times.
[0070] (3) Preparation of activated carbon-supported porous silica: The product of step (2) was dispersed in 300 mL of deionized water, 20 g of polyvinyl pyrrolidone was added, and the mixture was boiled and refluxed for 3 h, then cooled. Then 100 mL of 2 mol / L sodium hydroxide solution was added, and the mixture was stirred and etched for 3 h. The etched product was washed with water, dried at 105 °C for 2 h, and calcined in a muffle furnace at 550 °C for 4 h to obtain an activated carbon-supported porous silica material, which was recorded as product 2.
[0071] Example 6
[0072] This embodiment discloses an activated carbon-supported porous silica material, comprising the following steps:
[0073] (1) Preparation of silane precursor solution: In a beaker, weigh 210 mL of anhydrous ethanol and 70 mL of deionized water, mix them evenly, add 50 mL of MTMS, and mix them evenly again to prepare a silane precursor solution;
[0074] (2) Preparation of activated carbon-supported silica: Weigh 30 g of activated carbon and add it to the above-mentioned silane precursor solution, mix well, then add 50 mL of ammonia water with an ammonia content of 25% to 27% at room temperature, and stir at a stirring speed of 500 rpm / min for 2 h to allow the silane precursor to hydrolyze and condense to generate silica and load it in situ on the activated carbon to obtain activated carbon-supported silica. The product was repeatedly washed with deionized water and ethanol for 3 times.
[0075] (3) Preparation of activated carbon-supported porous silica: The product of step (2) was dispersed in 300 mL of deionized water, 20 g of polyvinyl pyrrolidone was added, and the mixture was boiled and refluxed for 3 h, then cooled. Then 100 mL of 2 mol / L sodium hydroxide solution was added, and the mixture was etched with stirring for 3 h. The etched product was washed with water, dried at 105 °C for 2 h, and calcined in a muffle furnace at 550 °C for 4 h to obtain an activated carbon-supported porous silica material, which was recorded as product 3.
[0076] Comparative Example 1
[0077] This comparative example discloses an activated carbon-loaded silica material, comprising the following steps:
[0078] (1) Preparation of silane precursor solution: In a beaker, weigh 210 mL of anhydrous ethanol and 70 mL of deionized water, mix them evenly, add 50 mL of TEOS, and mix them evenly again to prepare a silane precursor solution;
[0079] (2) Preparation of activated carbon-supported silica: Weigh 30 g of activated carbon and add it to the above-mentioned silane precursor solution, mix well, then add 50 mL of ammonia water with an ammonia content of 25% to 27% at room temperature, and stir at a stirring speed of 500 rpm / min for 2 h to allow the silane precursor to hydrolyze and condense to generate silica and load it in situ on the activated carbon to obtain activated carbon-supported silica. The product was repeatedly washed with deionized water and ethanol for 3 times.
[0080] (3) Dry the product of step (2) at 105°C for 2 h to obtain product 5.
[0081] Comparative Example 2
[0082] This comparative example uses coconut shell activated carbon, which is recorded as product 6.
[0083] Comparative Example 3
[0084] This comparative example discloses a silicon dioxide material, comprising the following steps:
[0085] (1) Preparation of silane precursor solution: In a beaker, weigh 210 mL of anhydrous ethanol and 70 mL of deionized water, mix them evenly, add 50 mL of TEOS, and mix them evenly again to prepare a silane precursor solution;
[0086] (2) Preparation of silicon dioxide: 50 mL of aqueous ammonia with an ammonia content of 25% to 27% at room temperature was added to the above silane precursor solution, and the mixture was stirred at 500 rpm / min for 2 h. The product was washed repeatedly with deionized water and ethanol for 3 times.
[0087] (3) Dry the product of step (2) at 105°C for 2 h to obtain product 7.
[0088] Comparative Example 4
[0089] This comparative example discloses an activated carbon-loaded porous silica material, which differs from Example 4 in that no coconut shell activated carbon is added during the hydrolysis and condensation process in this comparative example, and solid silica spheres are prepared and then loaded onto the activated carbon.
[0090] The specific steps of this comparative example are as follows:
[0091] (1) Preparation of silane precursor solution: In a beaker, weigh 210 mL of anhydrous ethanol and 70 mL of deionized water, mix them evenly, add 50 mL of TEOS, and mix them evenly again to prepare a silane precursor solution;
[0092] (2) Preparation of solid silica spheres: 50 mL of aqueous ammonia with an ammonia content of 25% to 27% at room temperature was added to the above silane precursor solution, and the mixture was stirred at a stirring speed of 500 rpm / min for 2 h to hydrolyze and condense the silane precursor to generate solid silica spheres, which were then washed with anhydrous ethanol and deionized water for three times respectively, and dried in an oven at 80° C. for 48 h to obtain solid silica spheres;
[0093] (3) Preparation of activated carbon-supported silica solid spheres: The silica solid spheres prepared in the above step and 30 g of coconut shell activated carbon were added to a mixed solution of 210 mL of anhydrous ethanol and 70 mL of deionized water, and stirred at a stirring speed of 500 rpm / min for 2 h. The product was repeatedly washed with deionized water and ethanol for 3 times;
[0094] (4) The above product was dried at 105°C for 2 h to obtain product 8.
[0095] The products obtained in the above-mentioned Examples 4-6 and Comparative Examples 1-4 were used as adsorbents and placed in six 50 mL trichlorosilane samples at a temperature of -18°C for adsorption. Before adsorption, the phosphorus impurity content in each trichlorosilane was prepared at 3 ppm. The adsorption time was 6 hours, and then the adsorbent was removed, the phosphorus impurity content in each trichlorosilane was detected, and the phosphorus impurity removal rate was calculated. The specific test results are shown in Table 1.
[0096] Table 1 Test results
[0097] sample Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Phosphorus impurity removal rate (%) 75.35 80.03 78.62 62.87 45.67 50.23 57.34 <![CDATA[Specific surface area (m 2 / g)]]> 1195.71 1238.47 1222.98 1187.41 954.39 987.63 1093.26
[0098] As can be seen from Table 1, the phosphorus impurities in trichlorosilane after adsorption in Examples 4-6 and Comparative Examples 1-4 are all reduced, that is, phosphorus impurities can be adsorbed, and the adsorption effects of Examples 4-6 on phosphorus impurities in trichlorosilane are better than those of Comparative Examples 1-4, indicating that the activated carbon-loaded porous silica prepared by the present method can effectively improve the adsorption performance of the adsorbent, and the adsorption effects are respectively higher than the non-porous activated carbon-loaded silica described in Comparative Example 1, higher than the silica used alone described in Comparative Example 3, and higher than the activated carbon used alone described in Comparative Example 2; and, the material of Example 5 has the best adsorption effect, indicating that the loading effect of silica can be controlled and optimized by adjusting the type and proportion of silane precursors, thereby more effectively increasing the surface active sites of the activated carbon and achieving better adsorption effects.
[0099] In addition, it can be seen from Example 4 and Comparative Example 4 that the present method adds activated carbon during the hydrolysis and condensation process, so that the silane precursor undergoes hydrolysis and condensation reaction to generate silicon dioxide and is in-situ loaded on the activated carbon. The obtained product has a larger specific surface area and a higher phosphorus impurity removal rate.
[0100] In summary, the material prepared by the method of the present invention can adsorb phosphorus impurities in trichlorosilane, thereby improving the adsorption effect on impurities in trichlorosilane.
[0101] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing an activated carbon-supported porous silica material, characterized in that: include: (1) mixing ethanol and water evenly, adding an appropriate amount of silane precursor, and mixing again evenly to prepare a silane precursor solution; (2) adding an appropriate amount of activated carbon to the silane precursor solution, mixing evenly, then adding an initiator, stirring for a period of time under certain stirring conditions, so that the silane precursor undergoes a hydrolysis and condensation reaction to generate silicon dioxide and in-situ loads the silicon dioxide on the activated carbon, thereby obtaining activated carbon-loaded silicon dioxide; (3) Dispersing the activated carbon-loaded silica into water, adding a protective agent, boiling and refluxing for a period of time and then cooling, then adding an appropriate amount of a porogen, stirring and etching for a period of time, washing, drying, and calcining to obtain an activated carbon-loaded porous silica material.
2. The method for preparing the activated carbon-supported porous silica material according to claim 1, characterized in that: The volume ratio of ethanol to water is 1 to 3:
1.
3. The method for preparing the activated carbon-supported porous silica material according to claim 1, characterized in that: The volume ratio of the amount of the silane precursor to the total amount of ethanol and water is 1:1-24.
4. According to the method for preparing activated carbon-supported porous silica material according to claim 1, the silane precursor is one or a combination of ethyl orthosilicate, methyl orthosilicate, polysiloxane, methyltrimethoxysilane, methyltriethoxysilane, and 3-(aminopropyl)triethoxysilane.
5. The method for preparing activated carbon-loaded porous silica material according to claim 1, wherein the activated carbon is one or a combination of coal-based activated carbon, fruit shell activated carbon, wood-based activated carbon, and petroleum-based activated carbon.
6. The method for preparing the activated carbon-supported porous silica material according to claim 1, characterized in that: The initiator is ammonia water, and the volume ratio of ammonia water to silane precursor is 1 to 4:
1.
7. The method for preparing an activated carbon-supported porous silica material according to claim 1, characterized in that: In step (2), the stirring speed is ≥500 rpm / min, and the stirring time is 2 to 10 hours.
8. The method for preparing an activated carbon-supported porous silica material according to claim 1, characterized in that: The protective agent is polyvinyl pyrrolidone, and the mass ratio of polyvinyl pyrrolidone to ammonia water is 1:1-3.
9. The method for preparing an activated carbon-supported porous silica material according to claim 1, wherein the boiling reflux time is 2 to 5 hours.
10. The method for preparing activated carbon-supported porous silica material according to claim 1, wherein the porogen is a sodium hydroxide solution, the concentration of the sodium hydroxide solution is 1 to 3 mol / L, the volume ratio of the sodium hydroxide solution to ammonia water is 1 to 8:1, and the stirring etching time is 1 to 3 hours.
11. An activated carbon-supported porous silica material, characterized in that: The activated carbon-loaded porous silica material is prepared by the preparation method described in any one of claims 1 to 10, and includes at least three levels of pores, namely, a first pore located on the activated carbon, a second pore located between the silica and the activated carbon and between the silica and the silica, and a third pore located on the silica.
12. An application of the activated carbon-supported porous silica material according to claim 11, characterized in that: The activated carbon-loaded porous silica material is used for adsorbing and removing phosphorus impurities in trichlorosilane.
Citation Information
Cited By
Preparation method of graphitized mesoporous carbon carrier
CN119660731A
Preparation Method of Graphitized Mesoporous Carbon Support
CN119660731B
Fluorine removal agent for fluorine-containing mine and preparation method of fluorine removal agent
CN120437989A
Fluorine-containing mine defluorination agent and preparation method thereof
CN120437989B
Preparation method and application of core-shell activated carbon-based hierarchical porous concrete internal curing agent
CN122426958A