Manufacturing method of large-piece-weight 321 stainless steel extra-thick plate
By using steel ingots made of three continuous casting billets, combined with the slow heating and gradually increasing rolling and pressing process, the problems of low material yield and long production cycle of large single-weight special thick plates are solved, and efficient production is achieved and performance improvement.
Patent Information
- Application Number
- CN202410976781.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
It is difficult to produce large single-weight and extra-thick 321 stainless steel plates, with low material yield and long production cycle, resulting in the performance of the steel plates not meeting the standards.
Three 180~200mm thick 321 continuous casting billet stacks are made into 600mm thick steel ingots. Through slow heating and slow rolling technology, the temperature of the steel ingot surface and core part is controlled to be consistent. A small pressure is used during initial rolling. Then gradually increase until the target thickness is reached.
The production of 321 thick plates with a maximum single weight of more than 30 tons and a thickness of 150mm has been achieved, with a material yield of more than 80%, and the performance of the steel plate has been significantly improved, and all indicators meet the standard requirements.
Smart Images

Figure CN118904944A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of material manufacturing, and in particular to a method for manufacturing a heavy unit weight 321 stainless steel extra-thick plate. Background Art
[0002] With the development of large-scale chemical equipment, the requirements for material size have also increased, and the demand for large unit weight and unconventional size steel plates has increased. The thickness of 321 continuous casting billet is 200mm, the maximum width is 2050mm, and the maximum length allowed by the heating furnace is 4000mm. The unit weight of the produced steel plate cannot exceed 10 tons, or when producing steel plates thicker than 80mm, the performance of the steel plate does not meet the standards due to the low rolling compression ratio. Before this invention, the domestic 321 stainless steel plate was at most 90mm thick and had a maximum unit weight of 10 tons. It was produced using die casting, electroslag, forging, and rolling processes. The steel plate yield rate was 50% and the manufacturing cycle was three months.
[0003] The present invention adopts 3 layers of 200mm thick continuous casting billets to stack to form 600mm thick steel ingots. The maximum unit weight of the produced steel plate exceeds 30 tons, the thickest can be up to 150mm, and the steel plate yield rate is over 80%, which solves the problem of low yield rate and long production cycle of thick steel plates produced by die casting and billet rolling. Summary of the invention
[0004] The purpose of the present invention is to provide a method for manufacturing heavy and thick plates in order to solve the above problems.
[0005] The object of the present invention is achieved as follows: A method for manufacturing a heavy unit weight 321 stainless steel extra thick plate comprises the following steps: Step 1: Controlling the composition of smelted molten steel: C: 0.03-0.035%, Ti: 0.25-0.30%; Step 2: Determining the size of the billet: Heating and rolling a 540-600 mm thick steel ingot made by stacking three 180-200 mm thick stainless steel continuous casting billets; Step 3: Heating the steel ingot: Cold loading the steel ingot into the steel ingot furnace Heating is carried out, the furnace temperature in the preheating stage is 500±10℃, and after keeping warm for 3~4 hours, the temperature is increased at a rate of ≤50℃ / h. The second stage insulation temperature is 1000±10℃, and after keeping warm for 4~5 hours, the temperature is increased at a rate of ≤50℃ / h. The third stage insulation temperature is 1150±10℃, and after keeping warm for 4~5 hours, the temperature is increased to 1180±10℃ at a rate of ≤50℃ / h. Step 4: Ingot rolling: The ingot is rolled after being heated.
[0006] In step 4, the first three rolling passes are rolled with a reduction of 25-30 mm per pass, and from the fourth pass onwards, the rolling is carried out at a reduction of 50-55 mm per pass until the required thickness is reached.
[0007] The beneficial effects of the present invention are as follows: the present invention adopts three 200mm thick 321 continuous casting billets to stack for rolling, heats the billets slowly, fully keeps the target temperature warm, initially rolls with a small reduction, and after the billets are completely fused, adopts the extreme reduction for rolling, and produces large unit weight 321 thick plates, with a maximum unit weight of over 30 tons and a maximum thickness of 150mm, which are exclusively produced in China. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] The present invention will be further described below in conjunction with the accompanying drawings.
[0009] Figure 1 : Surface grain size diagram of 130mm thick 321 steel plate.
[0010] Figure 2 : Grain size diagram of the core of 130mm thick 321 steel plate. DETAILED DESCRIPTION
[0011] With the large-scale development of various chemical equipment, the requirements for material size are also increasing. There is an increasing demand for large unit weight and unconventional size steel plates. In response to the above needs, the present invention opens up the process route of continuous casting billet rolling of ultra-large unit weight 321 extra-thick plates and realizes mass production. The maximum unit weight of the steel plate is more than 30 tons and the thickest is 150mm. The various performances of the steel plate at each thickness position are far higher than the standard requirements.
[0012] The technical idea of the present invention: 1. Composition design idea: The standard requires that the C content of 321 stainless steel is ≤0.08%, and there is no requirement for the lower limit. The C content is crucial to the yield strength of the steel plate. The thicker the steel plate, the more difficult it is to meet the requirements. As the C content increases, the corrosion resistance of the material decreases significantly. A higher content of Ti is required to improve the corrosion resistance of the material. The Ti element easily forms TiN inclusions with the N element during the smelting process. The TiN inclusions react with the continuous casting protection slag, which deteriorates the physical properties of the protection slag. The surface of the continuous casting billet is prone to form slag rolls and longitudinal cracks. Incomplete grinding leads to scrapping of the steel plate. Comprehensive consideration, under the premise of ensuring the performance of the steel plate, the C content control range is set at 0.03~0.035%, and the corresponding Ti content control range is set at 0.25~0.30%. The surface of the continuous casting billet is defect-free, and the qualified rate of the steel plate is 100%.
[0013] 2. Determination of billet size: The billet is designed according to the weight of the steel plate required by the customer. The customer requires a single steel plate weight of 25 tons and a yield rate of 80%. The required billet weight is 31 tons. According to the weight and size conversion, three 321 continuous casting billets must be used for billet making. A 600mm thick steel ingot made by stacking three 200mm thick 321 stainless steel continuous casting billets is used for rolling.
[0014] 3. Ingot heating process: Since the thickness of the ingot is 600mm, the surface and core temperatures of the ingot should be as consistent as possible before rolling, so it is required to heat up slowly, and the holding time should be long enough after reaching the target temperature. The ingot is cold loaded into the ingot furnace for heating. The furnace temperature in the preheating stage is 500±10℃, and the temperature is increased at a rate of ≤50℃ / h after 3 hours of holding. The second stage holding temperature is 1000±10℃, and the temperature is increased at a rate of ≤50℃ / h after 4 hours of holding. The third stage holding temperature is 1150±10℃, and the temperature is increased to 1180℃ at a rate of ≤50℃ / h after 4 hours of holding.
[0015] 4. Ingot rolling process: Since the ingot is made of three 200mm thick continuous casting billets, a small reduction should be used during the initial rolling to ensure that the three billets do not crack during the rolling process. As the rolling progresses, after the billets are completely fused, a large reduction is conducive to the crushing of the continuous casting billet structure and promotes the occurrence of recrystallization during the rolling process. The more complete the recrystallization, the more uniform the structure of the steel plate after rolling, and the better the performance. After the ingot is out of the furnace, the reduction is 30mm for each of the first three passes of rolling. Starting from the fourth pass, the rolling force is gradually increased according to the rolling force of the rolling mill until the required thickness is rolled.
[0016] The specific implementation manner of the present invention is described in detail below in conjunction with the embodiments, but the specific implementation manner of the present invention is not limited to the following embodiments. Embodiment 1
[0017] (1) 321 stainless steel continuous casting billets were produced by electric furnace + AOD + LF + continuous casting process. The composition of the continuous casting billets is as follows: C: 0.033, Si: 0.61, Mn: 0.90, P: 0.0028, S: 0.001, Cr: 17.13, Ni: 9.05, N: 0.01, Ti: 0.28. The continuous casting billet thickness is 200 mm and the width is 1535 mm.
[0018] (2) Three continuous casting billets with a length of 4000 mm were stacked to form billets. The final ingot specifications were thickness × width × length (mm): 600 × 1535 × 4000, and the total weight was 28.7 tons.
[0019] (3) The steel ingot is placed in the steel ingot furnace for heating and insulation. The furnace temperature in the preheating stage is 500°C. After 3 hours of insulation, the temperature is increased at a rate of 30°C / h. The second stage insulation temperature is 1000°C. After 4 hours of insulation, the temperature is increased at a rate of ≤30°C / h. The third stage insulation temperature is 1150°C. After 4 hours of insulation, the temperature is increased to 1180°C at a rate of ≤30°C / h.
[0020] (4) After the ingot is taken out of the furnace, rolling begins. The first three passes have a reduction of 30 mm each time, and the thickness after rolling is 510 mm. The subsequent reductions are greater than the first three passes. The thickness after each pass is 460 mm, 400 mm, 320 mm, 270 mm, 210 mm, 170 mm, and 130 mm respectively. The final steel plate product specifications are thickness × width × length (mm): 130 × 2700 × 9000, and the total weight is 24.6 tons.
[0021] The yield rate of 321 thick plates produced through the above steps is as high as 85.8%, the grain size of the steel plate is uniform throughout the thickness direction, the Z-axis tensile strength is equivalent to that of a single continuous casting billet rolled steel plate, and there is no crack in the side bending test, as shown in Table 1. Embodiment 2
[0022] (1) 321 stainless steel continuous casting billet was produced by electric furnace + AOD + LF + continuous casting process. The composition of the continuous casting billet is as follows: C: 0.035, Si: 0.57, Mn: 0.91, P: 0.0031, S: 0.001, Cr: 17.08, Ni: 9.12, N: 0.01, Ti: 0.30. The continuous casting billet thickness is 200 mm and the width is 2040 mm.
[0023] (2) Three continuous casting billets with a length of 4000 mm are stacked to form billets. The final ingot specifications are thickness × width × length (mm): 600 × 2040 × 4000, and the total weight is 38.2 tons.
[0024] (3) The steel ingot is placed in the steel ingot furnace for heating and insulation. The furnace temperature in the preheating stage is 500°C. After 3 hours of insulation, the temperature is increased at a rate of 20°C / h. The second stage insulation temperature is 1000°C. After 4 hours of insulation, the temperature is increased at a rate of ≤20°C / h. The third stage insulation temperature is 1150°C. After 4 hours of insulation, the temperature is increased to 1180°C at a rate of ≤20°C / h.
[0025] (4) After the ingot is taken out of the furnace, rolling begins. The first three passes have a reduction of 30 mm each time, and the thickness after rolling is 510 mm. The subsequent reductions are greater than the first three passes. The thickness after each pass is 470 mm, 420 mm, 380 mm, 340 mm, 300 mm, 250 mm, 200 mm, 160 mm, and 120 mm respectively. The final steel plate product specifications are thickness × width × length (mm): 120 × 3000 × 11000, and the total weight is 30.9 tons. The yield rate of 321 thick plates produced through the above steps is 80.8%, and all performance indicators are qualified.
[0026]
[0027] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are included in the patent scope of the present invention.
Claims
1. A method for manufacturing heavy unit weight 321 stainless steel extra thick plate, characterized by: The following steps are involved: Step 1: Control of molten steel composition: C: 0.03-0.035%, Ti: 0.25-0.30%; Step 2: Determine the billet size: Use three 180-200 mm thick stainless steel continuous casting billets to stack and heat and roll a 540-600 mm thick steel ingot; Step 3: Ingot heating: The ingot is cold loaded into the ingot furnace for heating. The furnace temperature in the preheating stage is 500±10℃. After keeping warm for 3~4 hours, the temperature is increased at a rate of ≤50℃ / h. The second stage is kept warm at 1000±10℃. After keeping warm for 4~5 hours, the temperature is increased at a rate of ≤50℃ / h. The third stage is kept warm at 1150±10℃. After keeping warm for 4~5 hours, the temperature is increased to 1180±10℃ at a rate of ≤50℃ / h. Step 4: Ingot rolling: The ingot is heated and then rolled.
2. The method for manufacturing a heavy unit weight 321 stainless steel extra thick plate according to claim 1, characterized in that: In step 4, the first three rolling passes are rolled with a reduction of 25-30 mm per pass, and from the fourth pass onwards, the rolling is carried out at a reduction of 50-55 mm per pass until the required thickness is reached.
Citation Information
Patent Citations
Method and device for producing thick plate and super-thick plate by reducing and roll cladding
CN105107842A
Production method of steel plate used for extra-thick specification equipment in hydrogen atmosphere
CN105710152A
Production method of ultra-thick homogenous composite board
CN108405611A
Ultra-thick alloy steel sheet with excellent low-temperature toughness and preparation method thereof
CN109112423A
Stainless steel extra-thick plate manufacturing method
CN111687234A