Low-damage welding method and system for semi-coherent magnesium alloy and computer equipment
Through laser welding technology and auxiliary thermal management, a uniformly distributed precipitation phase structure is formed, which solves the problem of thermal cycling failure interface of magnesium alloy welding, and significantly improves the mechanical properties and welding quality of magnesium alloy welds.
Patent Information
- Application Number
- CN202411011025.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The thermal cycle of welding magnesium alloys is prone to destroy the semi-common interface, resulting in a decrease in the strength and plasticity of magnesium alloys. It is difficult for existing welding technologies to effectively solve this problem.
Using low-damage welding method, through the combined use of the laser welding machine's cyclic intermittent working mode and auxiliary infrared lamps and semiconductor refrigeration sheets, directional heat transfer is realized, forming a uniformly distributed micro- and sub-micron-level precipitation phase structure, maintaining semi-concentration lattice interface to reduce the size of the welding heat affected zone.
The mechanical properties of the magnesium alloy welds are significantly improved, high-quality welding connections are obtained, the size of the welding heat-affected zone is reduced, the interface relationship between the specific precipitation phase in the alloy and the magnesium matrix is maintained, and the overall performance of welding is improved.
Smart Images

Figure CN118905433A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of magnesium alloy welding, and in particular to a low-damage welding method, system and computer equipment for semi-coherent magnesium alloy. Background Art
[0002] As the lightest structural material, magnesium alloy has unparalleled advantages in various industries such as lightweight automobiles, aerospace and consumer electronics. In particular, the modification of magnesium alloys by rare earth elements further refines the grains and forms thermally stable rare earth precipitation phases in the alloy, thereby enhancing the specific properties of the alloy and expanding its application range. The processing and manufacturing of complex magnesium alloy parts inevitably requires welding. The effects of welding thermal cycles on the precipitation and distribution of intermetallic compounds in the alloy are usually irreversible, especially for precipitation phases with poor thermal stability. Due to the changes in the microstructure of these intermetallic compounds, the mechanical properties of magnesium alloy welded joints are easily compromised.
[0003] The addition of rare earth yttrium can form a semi-coherent interface in magnesium alloys, thereby significantly improving the strength and plasticity of the alloy. This is the latest strengthening technology for magnesium alloys. However, it should be pointed out that welding thermal cycles will destroy this semi-coherent interface strengthening structure, thereby reducing the strength and plasticity of magnesium alloys. Obviously, the development of welding technology for semi-coherent magnesium alloys is particularly urgent and important. Summary of the invention
[0004] The present invention aims to improve at least one of the technical problems existing in the prior art. To this end, the present invention provides a low-damage welding method, system and computer equipment for semi-coherent magnesium alloy.
[0005] A low-damage welding method for semi-coherent magnesium alloy according to an embodiment of the first aspect of the present invention comprises: Step S1, building a low-damage welding scene for a semi-coherent magnesium alloy, wherein the low-damage welding scene includes a welding workbench and a laser welder, and cleaning and polishing a semi-coherent magnesium alloy plate; Step S2, fixing and clamping the cleaned and polished semi-coherent magnesium alloy plate on the surface of a welding workbench in the scene; Step S3, pasting a semiconductor cooling sheet on a surface away from the joint of the semi-coherent magnesium alloy sheet; Step S4, installing an infrared lamp, placing an infrared lamp on the upper surface of the butt joint of the semi-coherent magnesium alloy plate to preheat the semi-coherent magnesium alloy plate; Step S5, adjusting the working mode of the laser welder, starting the laser welder, setting the laser oscillation frequency to the laser welder, and making the laser welder enter a cyclic intermittent working mode.
[0006] Step S6, parameter input, inputting welding machine parameters and laser vibration trajectory into the laser welding machine; Step S7, parameter judgment, judging whether the input welding machine parameters meet the first preset conditions and whether the laser vibration trajectory meets the second preset conditions. If both meet, it prompts that the welding preparation is complete; Step S8, welding heat directional transmission control, within a first threshold time before welding starts, the infrared lamp and the semiconductor cooling sheet are turned on at the same time to achieve directional heat transmission from the upper surface to the lower surface of the joint; Step S9, performing laser welding of magnesium alloy to output a weld with low damage and good formation.
[0007] The low-damage welding method of semi-coherent magnesium alloy according to the embodiment of the present invention has the following innovative advantages compared with the prior art: (1) The present invention can form a dispersed precipitation phase structure in the alloy. The present invention uses a preset laser oscillation to break the original precipitation phase in the alloy to form a uniformly distributed micron-level and submicron-level precipitation phase structure. (2) Significantly reduce the size of the welding heat affected zone The present invention uses specific laser oscillation to maintain the microstructure of the heat-affected zone, especially the semi-coherent interface, thereby significantly reducing the size of the welding heat-affected zone, thereby obtaining a high-quality weld.
[0008] (3) Maintaining the semi-coherent interface relationship between the specific precipitate phase and the magnesium matrix The present invention maintains a semi-coherent interface relationship between a specific precipitated phase in the alloy and the magnesium matrix by finely regulating welding heat input and assisting in forced heat dissipation.
[0009] (4) Achieving high-quality connection of magnesium alloys The present invention forms a weld zone strengthened by micron and submicron precipitation phases, reduces the size of the welding heat affected zone, can significantly improve the mechanical properties of the weld, and obtain a high-quality magnesium alloy weld.
[0010] In a possible implementation of the first aspect, in step S5, the cyclic intermittent working mode of the laser welder includes the laser welder outputting for 0.05 s to 0.1s and then pausing for 0.01 s to 0.02s, which is conducive to the temperature controllable operation of the welding pool.
[0011] In a possible implementation of the first aspect, in step S6, the welding machine parameters include welding speed, welding power, laser defocus amount, and welding shielding gas selection.
[0012] In a possible implementation of the first aspect, in step S7, the standard for determining whether the input welding machine parameter meets the first preset condition is specifically that the following conditions need to be met at the same time: Condition 1: The input threshold range of the welding speed is 10 mm / s to 50 mm / s; Condition 2: The input threshold range of the welding power is 500 W to 3000 W; Condition three: the input threshold range of the laser defocus amount is -5 to +5 mm; Condition 4: the welding shielding gas is selected to be argon or helium.
[0013] In a possible implementation manner of the first aspect, in step S7, the criterion for determining whether the laser vibration trajectory meets the second preset condition is specifically: The laser vibration trajectory is any one of an "8" shape, a "Z" shape, an "S" shape or a "spiral shape" or a combination thereof.
[0014] In a possible implementation of the first aspect, step S4 specifically includes placing an infrared lamp on the upper surface of the magnesium alloy weld, and heating the semi-coherent magnesium alloy to 80-120° C., preferably 100° C., by the infrared lamp.
[0015] In a possible implementation manner of the first aspect, the operating temperature range of the semiconductor refrigeration chip is -20°C to 0°C, and the measurement position is the surface of the semiconductor refrigeration chip.
[0016] In a possible implementation manner of the first aspect, the welding form is butt joint or overlap joint.
[0017] The low-damage welding system for semi-coherent magnesium alloy according to the second embodiment of the present invention comprises a welding workbench and a laser welder, and further comprises: Pretreatment module, used for cleaning and grinding semi-coherent magnesium alloy plates; A clamping module is used to fix and clamp the cleaned and polished semi-coherent magnesium alloy plate on the surface of the welding workbench in the scene, and fix the semi-coherent magnesium alloy plate on the surface of the welding workbench through a clamp; A front installation module is used for pasting a semiconductor cooling sheet and an infrared lamp for installation, wherein the semiconductor cooling sheet is pasted on a surface away from the butt joint of the semi-coherent magnesium alloy sheet, wherein the semiconductor cooling sheet covers the butt joint to be welded; an infrared lamp is placed on the upper surface of the butt joint of the semi-coherent magnesium alloy sheet to preheat the semi-coherent magnesium alloy sheet; The regulating module is used to adjust the working mode of the laser welder, start the laser welder, set the laser oscillation frequency to the laser welder, and make the laser welder enter a cyclic intermittent working mode.
[0018] An input module, used for parameter input, inputting welding machine parameters and laser vibration trajectory into the laser welding machine; A judgment module, used to judge whether the input welding machine parameters meet the first preset conditions and whether the laser vibration trajectory meets the second preset conditions, and if both meet, prompting that welding preparation is complete; A directional transmission control module is used for directional transmission control of welding heat. Within a first threshold time before welding starts, the infrared lamp and the semiconductor cooling sheet are turned on at the same time to achieve directional transmission of heat from the upper surface to the lower surface of the joint. The execution module is used to perform laser welding of magnesium alloys and output low-damage, well-formed welds.
[0019] According to a computer device of an embodiment of the third aspect of the present invention, the computer storage medium stores instructions, and when the instructions are executed on the computer, the computer executes the above-mentioned low-damage welding method for semi-coherent magnesium alloy.
[0020] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 is a flow chart of a low-damage welding method for a semi-coherent magnesium alloy according to an embodiment of the present invention; Figure 2 is a schematic diagram of low damage welding of a semi-coherent magnesium alloy according to an embodiment of the present invention; Figure 3 is a schematic diagram of dispersedly distributed micron and submicron precipitate phases in an embodiment of the present invention; Figure 4 Schematic diagram of an extremely narrow welding heat-affected zone according to an embodiment of the present invention; Figure 5 Schematic diagram of the semi-coherent interface between the precipitate phase and the magnesium matrix in an embodiment of the present invention; Figure 6 Schematic diagram of a high-quality magnesium alloy weld according to an embodiment of the present invention. DETAILED DESCRIPTION
[0023] The embodiments of the present invention are described in detail below. The embodiments described with reference to the accompanying drawings are exemplary. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0024] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0026] The terms "first", "second", "third", etc. in the specification and claims of the present application and the drawings are used to distinguish different objects rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a series of steps or units are included, or optionally, steps or units not listed are included, or optionally, other steps or units inherent to these processes, methods, products or devices are included.
[0027] Only the part relevant to the present application is shown in the accompanying drawings, but not all of the content. Before discussing the exemplary embodiments in more detail, it should be mentioned that some exemplary embodiments are described as processing or methods depicted as flow charts. Although the flow chart describes each operation (or step) as a sequential process, many of the operations therein can be implemented in parallel, concurrently or simultaneously. In addition, the order of each operation can be rearranged. When its operation is completed, the process can be terminated, but it can also have additional steps not included in the accompanying drawings. The process can correspond to a method, function, procedure, subroutine, subprogram, etc.
[0028] The terms "component", "module", "system", "unit", etc. used in this specification are used to represent computer-related entities, hardware, firmware, a combination of hardware and software, software, or software in execution. For example, a unit can be, but is not limited to, a process running on a processor, a processor, an object, an executable file, an execution thread, a program, and / or distributed between two or more computers. In addition, these units can be executed from various computer-readable media having various data structures stored thereon. Units can communicate through local and / or remote processes, for example, based on signals having one or more data packets (e.g., data from a second unit interacting with another unit in a local system, a distributed system, and / or a network. For example, the Internet interacts with other systems via signals).
[0029] As the lightest structural material, magnesium alloy has unparalleled advantages in various industries such as lightweight automobiles, aerospace and consumer electronics. In particular, the modification of magnesium alloys by rare earth elements further refines the grains and forms thermally stable rare earth precipitation phases in the alloy, thereby enhancing the specific properties of the alloy and expanding its application range. The processing and manufacturing of complex magnesium alloy parts inevitably requires welding. The effects of welding thermal cycles on the precipitation and distribution of intermetallic compounds in the alloy are usually irreversible, especially for precipitation phases with poor thermal stability. Due to the changes in the microstructure of these intermetallic compounds, the mechanical properties of magnesium alloy welded joints are easily compromised.
[0030] The addition of rare earth yttrium can form a semi-coherent interface in magnesium alloys, thereby significantly improving the strength and plasticity of the alloy. This is the latest strengthening technology for magnesium alloys. However, it should be pointed out that welding thermal cycles will destroy this semi-coherent interface strengthening structure, thereby reducing the strength and plasticity of magnesium alloys. Obviously, the development of welding technology for semi-coherent magnesium alloys is particularly urgent and important.
[0031] Laser welding is distinguished by its high energy density, rapid heating rate, and low and precise heat input. During laser welding of magnesium alloys, the magnesium alloy is only briefly exposed to the heat of welding, thereby reducing the size of the heat-affected zone and reducing the impact of the welding thermal cycle on the microstructure of the magnesium alloy. It should be noted that there are no research cases and related process literature on laser welding of semi-coherent magnesium alloys. The regulation of microstructural evolution of the semi-coherent interface during the welding thermal cycle and the study of changes in mechanical properties before and after the evolution of the semi-coherent interface are both in a blank stage. Obviously, the present invention is unique and original in terms of research objects and research methods.
[0032] By forming a precipitate phase with a semi-coherent interface with the magnesium matrix in the magnesium alloy, a strong bonding interface is introduced into the magnesium alloy, thereby achieving the reinforcement and plasticization of the magnesium alloy. However, the precipitate phase with a semi-coherent interface with the magnesium matrix is consistent with other precipitates, and is easily affected by the welding thermal cycle and undergoes microstructural evolution, resulting in the disappearance of the original semi-coherent interface in the alloy, thereby seriously reducing the strength and plasticity of the magnesium alloy. These characteristics make the welding of semi-coherent magnesium alloys extremely difficult, and semi-coherent interface strengthening is the latest magnesium alloy strengthening technology. At present, there is no relevant literature reporting the welding process of this type of magnesium alloy. Obviously, the development of welding technology for semi-coherent magnesium alloys is of great practical significance.
[0033] Existing magnesium alloys are mainly strengthened and plasticized by fine grain strengthening, precipitation phase strengthening, and second phase strengthening. Strengthening and plasticizing magnesium alloys through semi-coherent interfaces is at the forefront of research in this field. However, there is no literature report on the welding of semi-coherent magnesium alloys. Existing magnesium alloy welding methods mainly include: (1) Fusion welding: TIG (Tungsten Inert Gas Welding): It uses a non-consumable tungsten electrode to generate an arc for welding, and is often used to weld thin-walled magnesium alloy materials. However, the heat-affected zone of TIG welding is large, and the microstructure of the weld zone and the heat-affected zone, especially the precipitated phase structure, will change significantly, resulting in typical softening of the heat-affected zone.
[0034] MIG (Metal Inert Gas Welding): uses consumable electrodes for welding and is suitable for welding thicker magnesium alloy workpieces. However, the heat input of MIG welding is much greater than that of TIG welding, the size of the heat-affected zone is larger, and the microstructure of the weld is more difficult to control, especially the microstructure of the precisely designed magnesium alloy is very easy to change.
[0035] Laser welding: With high energy density, fast heating rate and precise heat input, it is suitable for high-precision welding of magnesium alloy thin plates.
[0036] (2) Solid-state welding: Friction stir welding (FSW): The friction between the rotating tool and the workpiece surface generates heat, heats the workpiece to a plastic state and stirs it to achieve welding. This method is suitable for welding magnesium alloy thick plates and dissimilar materials. However, magnesium alloys are HCP structures with inherently poor properties, and stir friction welding can easily cause cracking and microcracks in magnesium alloys.
[0037] Obviously, during the welding process, the original carefully designed and precisely distributed precipitation phase structure in the magnesium alloy is affected by the welding thermal cycle, and most of them melt or dissolve, and the structure is destroyed, resulting in a decrease in the number of fine precipitation phases and a weakening of the original precipitation strengthening or second phase strengthening effect of the alloy. Therefore, conventional magnesium alloy welding is prone to typical heat-affected zone softening. The above phenomenon seriously limits the application of magnesium alloy parts, and how to achieve high-quality welding of magnesium alloys has become one of the frontiers of magnesium alloy research.
[0038] Example 1 See also Figure 1 and Figure 2 As shown, this embodiment provides a low-damage welding method for semi-coherent magnesium alloy, which includes: Step S1, building a low-damage welding scene for a semi-coherent magnesium alloy, wherein the low-damage welding scene includes a welding workbench and a laser welder, and cleaning and polishing a semi-coherent magnesium alloy plate; Step S2, fixing and clamping the cleaned and polished semi-coherent magnesium alloy plate on the surface of the welding workbench in the scene, and fixing the semi-coherent magnesium alloy plate on the surface of the welding workbench by a clamp; Step S3, pasting a semiconductor cooling sheet on a surface away from the butt joint of the semi-coherent magnesium alloy plate, wherein the semiconductor cooling sheet covers the butt joint to be welded; Step S4, installing an infrared lamp, placing an infrared lamp on the upper surface of the butt joint of the semi-coherent magnesium alloy plate to preheat the semi-coherent magnesium alloy plate; Step S5, adjusting the working mode of the laser welder, starting the laser welder, setting the laser oscillation frequency to the laser welder, and making the laser welder enter a cyclic intermittent working mode.
[0039] Step S6, parameter input, inputting welding machine parameters and laser vibration trajectory into the laser welding machine; Step S7, parameter judgment, judging whether the input welding machine parameters meet the first preset conditions and whether the laser vibration trajectory meets the second preset conditions. If both meet, it prompts that the welding preparation is complete; Step S8, welding heat directional transmission control, within the first threshold time before welding starts, the infrared lamp and the semiconductor cooling sheet are turned on at the same time to achieve directional heat transmission from the upper surface to the lower surface of the joint. In this embodiment, 10 to 30 seconds before welding starts, the upper surface infrared lamp and the lower surface semiconductor cooling sheet work at the same time to achieve directional heat transmission from the upper surface to the lower surface; Step S9, performing laser welding of magnesium alloy, due to the directional heat transmission, the alloy microstructure is effectively protected, and the output is a low-damage, well-formed weld.
[0040] The low-damage welding method of semi-coherent magnesium alloy according to the embodiment of the present invention has the following innovative advantages compared with the prior art: (1) The present invention can form a dispersed precipitation phase structure in the alloy, such as Figure 3 As shown, The present invention breaks up the original precipitation phase in the alloy through preset laser oscillation to form a uniformly distributed micron-level and submicron-level precipitation phase structure.
[0041] (2) Significantly reduce the size of the heat affected zone of welding, such as Figure 4 As shown, The present invention uses specific laser oscillation to maintain the microstructure of the heat-affected zone, especially the semi-coherent interface, thereby significantly reducing the size of the welding heat-affected zone, thereby obtaining a high-quality weld.
[0042] (3) Maintaining a semi-coherent interface relationship between a specific precipitate phase and the magnesium matrix, such as Figure 5 As shown, The present invention maintains a semi-coherent interface relationship between a specific precipitated phase in the alloy and the magnesium matrix by finely regulating welding heat input and assisting in forced heat dissipation.
[0043] (4) Achieve high-quality connection of magnesium alloys, such as Figure 6 As shown, Figure 6 a in the figure is the 3D topography of the weld. Figure 6 b in the figure is the weld height diagram. Figure 6 The c in the figure is the weld macroscopic morphology. Figure 6 d in the figure is a cross-sectional view of the weld. It can be seen that the weld surface morphology obtained by the low-damage welding method of the present application is good, without obvious defects, and the weld height is basically consistent, which also proves the feasibility of the present application.
[0044] The invention forms a weld zone strengthened by micron and submicron precipitation phases, thereby reducing the size of the welding heat affected zone. The invention can significantly improve the mechanical properties of the weld and obtain a high-quality magnesium alloy weld.
[0045] It should be noted that the cyclic intermittent working mode of the laser welder in step S5 includes that the laser welder outputs for 0.05 s to 0.1 s and then pauses for 0.01 s to 0.02 s, which is conducive to the temperature controllable operation of the welding pool. In this embodiment, it is preferred to work for 0.05 s and pause for 0.01 s to make the temperature of the welding pool controllable.
[0046] It should be noted that in step S6, the welding machine parameters include welding speed, welding power, laser defocusing amount, and welding shielding gas selection.
[0047] It should be noted that, in step S7, the standard for judging whether the input welding machine parameters meet the first preset condition is specifically that the following conditions need to be met at the same time: Condition 1: The input threshold range of the welding speed is 10 mm / s to 50 mm / s; Condition 2: The input threshold range of the welding power is 500 W to 3000 W; Condition three: the input threshold range of the laser defocus amount is -5 to +5 mm; Condition 4: the welding shielding gas is selected to be argon or helium.
[0048] It should be noted that, in step S7, the criteria for determining whether the laser vibration trajectory meets the second preset condition are specifically: The laser vibration trajectory is any one of an "8" shape, a "Z" shape, an "S" shape or a "spiral shape" or a combination thereof.
[0049] It should be noted that step S4 specifically includes placing an infrared lamp on the upper surface of the magnesium alloy weld, and heating the semi-coherent magnesium alloy to 80-120° C., preferably 100° C., by the infrared lamp.
[0050] It should be noted that the operating temperature range of the semiconductor refrigeration plate is -20°C to 0°C. In this embodiment, the operating temperature of the semiconductor refrigeration plate is -5°C, and the measurement position is the surface of the semiconductor refrigeration plate.
[0051] It should be noted that the welding form is butt welding or overlap welding, and the butt welding form is selected in this embodiment.
[0052] Example 2 This embodiment provides a low-damage welding system for semi-coherent magnesium alloy, including a welding workbench and a laser welder, and further comprising: Pretreatment module, used for cleaning and grinding semi-coherent magnesium alloy plates; A clamping module is used to fix and clamp the cleaned and polished semi-coherent magnesium alloy plate on the surface of the welding workbench in the scene, and fix the semi-coherent magnesium alloy plate on the surface of the welding workbench through a clamp; A front installation module is used for pasting a semiconductor cooling sheet and an infrared lamp for installation, wherein the semiconductor cooling sheet is pasted on a surface away from the butt joint of the semi-coherent magnesium alloy sheet, wherein the semiconductor cooling sheet covers the butt joint to be welded; an infrared lamp is placed on the upper surface of the butt joint of the semi-coherent magnesium alloy sheet to preheat the semi-coherent magnesium alloy sheet; The regulating module is used to adjust the working mode of the laser welder, start the laser welder, set the laser oscillation frequency to the laser welder, and make the laser welder enter a cyclic intermittent working mode.
[0053] An input module, used for parameter input, inputting welding machine parameters and laser vibration trajectory into the laser welding machine; A judgment module, used to judge whether the input welding machine parameters meet the first preset conditions and whether the laser vibration trajectory meets the second preset conditions, and if both meet, prompting that welding preparation is complete; A directional transmission control module is used for directional transmission control of welding heat. Within a first threshold time before welding starts, the infrared lamp and the semiconductor cooling sheet are turned on at the same time to achieve directional transmission of heat from the upper surface to the lower surface of the joint. The execution module is used to perform laser welding of magnesium alloys. Due to the directional heat transmission, the alloy microstructure is effectively protected and the output is a low-damage, well-formed weld.
[0054] Example 3 This embodiment provides a computer device, wherein the computer storage medium stores instructions, and when the instructions are executed on the computer, the computer executes the above-mentioned low-damage welding method for semi-coherent magnesium alloy.
[0055] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation to the invention.
[0056] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0057] Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. Mentioning "embodiment" in this article means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present embodiment application. The appearance of this phrase in various positions in the specification is not necessarily the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It can be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0058] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. Low damage welding method for semi-coherent magnesium alloy, It is characterized in that include: Step S1, building a low-damage welding scene for a semi-coherent magnesium alloy, wherein the low-damage welding scene includes a welding workbench and a laser welder, and cleaning and polishing a semi-coherent magnesium alloy plate; Step S2, fixing and clamping the cleaned and polished semi-coherent magnesium alloy plate on the surface of a welding workbench in the scene; Step S3, pasting a semiconductor cooling sheet on a surface away from the joint of the semi-coherent magnesium alloy sheet; Step S4, installing an infrared lamp, placing an infrared lamp on the upper surface of the butt joint of the semi-coherent magnesium alloy plate to preheat the semi-coherent magnesium alloy plate; Step S5, adjusting the working mode of the laser welder, starting the laser welder, setting the laser oscillation frequency to the laser welder, and making the laser welder enter a cyclic intermittent working mode; Step S6, parameter input, inputting welding machine parameters and laser vibration trajectory into the laser welding machine; Step S7, parameter judgment, judging whether the input welding machine parameters meet the first preset conditions and whether the laser vibration trajectory meets the second preset conditions. If both meet, it prompts that the welding preparation is complete; Step S8, welding heat directional transmission control, within a first threshold time before welding starts, the infrared lamp and the semiconductor cooling sheet are turned on at the same time to achieve directional heat transmission from the upper surface to the lower surface of the joint; Step S9, performing laser welding of magnesium alloy to output a weld with low damage and good formation.
2. The low damage welding method for semi-coherent magnesium alloy according to claim 1, It is characterized in that In step S5, the cyclic intermittent working mode of the laser welder includes that the laser welder outputs for 0.05 s to 0.1 s and then pauses for 0.01 s to 0.02 s.
3. The low damage welding method for semi-coherent magnesium alloy according to claim 1, It is characterized in that In step S6, the welding machine parameters include welding speed, welding power, laser defocusing amount, and welding shielding gas selection.
4. The low damage welding method for semi-coherent magnesium alloy according to claim 1, It is characterized in that In step S7, the standard for judging whether the input welding machine parameters meet the first preset condition is specifically that the following conditions need to be met at the same time: Condition 1: The input threshold range of the welding speed is 10 mm / s to 50 mm / s; Condition 2: The input threshold range of the welding power is 500 W to 3000 W; Condition three: the input threshold range of the laser defocus amount is -5 to +5 mm; Condition 4: the welding shielding gas is selected to be argon or helium.
5. The low damage welding method for semi-coherent magnesium alloy according to claim 1, It is characterized in that In step S7, the criteria for judging whether the laser vibration trajectory meets the second preset condition are specifically: The laser vibration trajectory is any one of "8" shape, "Z" shape, "S" shape or "spiral shape" or a combination thereof.
6. The low damage welding method for semi-coherent magnesium alloy according to claim 1, It is characterized in that Step S4 specifically includes placing an infrared lamp on the upper surface of the magnesium alloy weld, and heating the semi-coherent magnesium alloy to 80-120° C. through the infrared lamp.
7. The low damage welding method for semi-coherent magnesium alloy according to claim 1, It is characterized in that The working temperature range of the semiconductor refrigeration sheet is -20°C to 0°C, and the measurement position is the surface of the semiconductor refrigeration sheet.
8. The low damage welding method for semi-coherent magnesium alloy according to claim 1, It is characterized in that The welding form is butt joint or lap joint.
9. A low-damage welding system for semi-coherent magnesium alloy, comprising a welding workbench and a laser welder, It is characterized in that Also includes: Pretreatment module, used for cleaning and grinding semi-coherent magnesium alloy plates; A clamping module, used to fix and clamp the cleaned and polished semi-coherent magnesium alloy plate on the surface of the welding workbench in the scene; A front installation module is used for pasting semiconductor cooling sheets and infrared lamps, pasting semiconductor cooling sheets on the surface away from the butt joint of the semi-coherent magnesium alloy sheet; placing infrared lamps on the upper surface of the butt joint of the semi-coherent magnesium alloy sheet to preheat the semi-coherent magnesium alloy sheet; The regulating module is used to adjust the working mode of the laser welder, start the laser welder, set the laser oscillation frequency to the laser welder, and make the laser welder enter a cyclic intermittent working mode. An input module, used for parameter input, inputting welding machine parameters and laser vibration trajectory into the laser welding machine; A judgment module, used to judge whether the input welding machine parameters meet the first preset conditions and whether the laser vibration trajectory meets the second preset conditions, and if both meet, prompting that welding preparation is complete; A directional transmission control module is used for directional transmission control of welding heat. Within a first threshold time before welding starts, the infrared lamp and the semiconductor cooling sheet are turned on at the same time to achieve directional transmission of heat from the upper surface to the lower surface of the joint. The execution module is used to perform laser welding of magnesium alloys and output low-damage, well-formed welds.
10. A computer device, It is characterized in that The computer storage medium stores instructions, and when the instructions are executed on a computer, the computer is caused to execute the low-damage welding method for a semi-coherent magnesium alloy according to any one of claims 1 to 8.