Printing stencil and preparation method thereof

By forming an upwardly raised arc metal mesh structure in the ink-transmissive area of ​​the printing template, the problem of uneven ink transmission in the prior art is solved, the flatness and straightness of the printing lines are improved, and more efficient is achieved silver paste used.

CN118906632APending Publication Date: 2024-11-08ZHEJIANG SHUOKE SCI & TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411280965.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The ink-permeable zone structure design of the existing printing templates leads to uneven ink transmission, affecting the flatness and straightness of the printing lines. Especially when the electrode lines are refined, the silver paste consumption is difficult to reduce.

Method used

Design a printing template, including mesh frame, edge yarn, metal mesh and shielding film layer. The metal mesh forms an upwardly protruding arc structure at the ink-permeable area, increasing the effective thickness of the shielding film layer and ensuring ink flowability Consistently, plastically deformed metal mesh is formed by molding or rolling, and printed patterns are prepared thereon.

Benefits of technology

It improves the flatness and straightness of the printing lines, increases the height of the printing graphics, reduces the ups and downs, ensures sufficient flow space for the ink at the position of the printing graphics, and achieves more efficient use of silver paste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906632A_ABST
    Figure CN118906632A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of printing stencils, in particular to a printing stencil which comprises a screen frame, an edge yarn, a metal gauze and a shielding film layer, a printing pattern is arranged on the shielding film layer, the shielding film layer covers the metal gauze, an upward-protruding structure is formed on the metal gauze at the position corresponding to an ink penetrating area of the printing pattern of the shielding film layer, and the shielding film layer covers the metal gauze. And the lower surface of the metal gauze in the range of the upward convex structure is higher than the lower surface of the metal gauze corresponding to the non-ink-permeable area. Meanwhile, the invention further discloses a preparation method of the printing stencil. The arc-shaped structure is pressed at the position, corresponding to the ink penetrating area of the printed pattern, of the metal gauze, so that the effective thickness of the shielding film layer at the printed pattern position is increased, sufficient flowing space is provided for ink in the printed pattern position, the thickness of an oil film in the printed pattern position is more consistent, and the printing quality is improved. The height of a printed pattern is increased, the flatness is improved, and fluctuation is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printing templates, in particular to a printing template and a preparation method thereof. Background Art

[0002] With the development of the photovoltaic industry, in order to achieve higher battery conversion efficiency and minimize the consumption of silver paste, the electrode lines required to be prepared are thin and flat. At present, the preparation of electrode lines is mainly based on screen printing, which is to print silver paste on the surface of the battery through a printing template to form an electrode. The width, height and flatness of the electrode line depend on the structural design of the ink-permeable area of ​​the printing template.

[0003] At present, there are mainly two ways to design the structure of the ink-permeable area:

[0004] Method 1: It is composed of woven wire mesh + shielding film layer, such as Figure 1 , Figure 2 ; Based on the woven structure of the screen, the wires are interwoven up and down, and the wires in the ink-permeable area are arranged horizontally as follows Figure 1 As shown, there is a height difference between the left and right sides, and the longitudinal distribution is as follows Figure 2 As shown, it is also a high-low staggered method. The irregular arrangement of the mesh in the ink-permeable area will affect the uniformity of the printing ink penetration, thereby affecting the flatness and straightness of the printed lines.

[0005] Method 2: Electroformed mesh / etched mesh / laser cut mesh + shielding film layer, such as Figure 3 , Figure 4 The screen has a flat structure, and there is no height difference between the mesh wires. However, the mesh wires will occupy the space of the film layer, reducing the effective height of the film layer. As the printing line width decreases, the shielding film thickness will become thinner and thinner. The low effective height of the film layer will restrict the flow of ink at the mesh position, affecting the flatness and straightness of the printed lines. Summary of the invention

[0006] In order to solve the above technical deficiencies, the present invention provides a printing template and a preparation method thereof, which can effectively increase the effective thickness of the shielding film layer, improve the ink fluidity in the ink-permeable area, so as to achieve the consistency of the oil film filling in the ink-permeable area, and improve the straightness and flatness of the printed lines.

[0007] The present invention discloses a printing template, comprising a screen frame, a border yarn, a metal mesh yarn and a shielding film layer, wherein a printed pattern is arranged on the shielding film layer, and the shielding film layer is covered on the metal mesh yarn. The metal mesh yarn at a position corresponding to an ink-permeable area of ​​the printed pattern of the shielding film layer forms an upwardly protruding structure, and the lower surface of the metal mesh yarn within the upwardly protruding structure range should be higher than the lower surface of the metal mesh yarn corresponding to the non-ink-permeable area.

[0008] The position of the lower surface of the metal mesh within the upwardly protruding structural range is higher than the position of the upper surface of the shielding film layer on both sides of the ink-permeable area.

[0009] The upwardly protruding structure formed on the metal mesh is an arc-shaped structure.

[0010] The metal mesh is a woven mesh, an electroformed mesh, an etched mesh or a laser cut mesh.

[0011] The metal mesh yarn within the arc structure is locally drawn, and the number of drawn wires is 1-6.

[0012] A method for preparing a printing template,

[0013] Step 1:

[0014] (1) Cut the metal mesh according to the needs;

[0015] (2) Pressing an upwardly protruding arc structure on the metal mesh by molding or rolling to form a plastically deformed metal mesh;

[0016] Step 2:

[0017] (1) Fixing the plastically deformed metal mesh on the edge mesh on the mesh frame;

[0018] (2) preparing a shielding film layer on the metal mesh, coating the metal mesh with a photosensitive adhesive, or laminating a polymer film or a metal film on the metal mesh;

[0019] (3) Preparing printed patterns by exposure and development, or preparing printed patterns by laser lithography or micro-etching.

[0020] Before preparing the printed pattern, the position of the arc structure on the metal mesh is determined by surveying and scanning equipment, and coordinate positioning is performed so that the prepared printed pattern corresponds to the arc structure.

[0021] The metal mesh of the above-mentioned printing template forms a raised arc structure in the opposite direction of the shielding film layer at the corresponding position of the ink-permeable area, and the thickness of the metal mesh remains unchanged. In this way, the up and down deviation of the metal mesh in the shielding film layer can be eliminated at the raised arc position, thereby increasing the effective thickness of the shielding film layer at the metal mesh arc structure, so as to ensure that the printing ink has high consistency in the ink filling of the ink-permeable area at the graphic position of the printing template, and has sufficient flow space to achieve good printing effects.

[0022] A printing template and a preparation method thereof obtained by the present invention press an arc structure on the metal mesh at a position corresponding to the ink-permeable area of ​​the printed graphic, thereby increasing the effective thickness of the shielding film layer at the position of the printed graphic, providing the ink with sufficient flow space at the position of the printed graphic, making the thickness of the oil film at the position of the printed graphic more consistent, and achieving an increase in the height of the printed graphic, an improvement in flatness, and a reduction in undulation.

[0023] The definition of knot-free structure is: there are only single-directional meshes in the printed graphic area, without interwoven knots. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the horizontal structural state of the woven wire mesh and the shielding film layer in the prior art;

[0025] Figure 2 It is a schematic diagram of the longitudinal structural state of the woven wire mesh and the shielding film layer in the prior art;

[0026] Figure 3 It is a schematic diagram of the horizontal structural state of the plane screen and the shielding film layer in the prior art;

[0027] Figure 4 It is a schematic diagram of the longitudinal structural state of the plane screen and the shielding film layer in the prior art;

[0028] Figure 5 It is a structural schematic diagram of the printing template of the present invention;

[0029] Figure 6 It is a schematic front view cross-sectional view of the woven wire mesh and the shielding film layer at A of the present invention;

[0030] Figure 7 It is a schematic cross-sectional view of the woven wire mesh and the shielding film layer at A of the present invention;

[0031] Figure 8 It is a schematic front view cross-sectional view of the plane screen and the shielding film layer of the present invention at point A;

[0032] Fig. 9 It is a schematic cross-sectional view of the plane screen and the shielding film layer of the present invention at A;

[0033] Fig.10 This is a printing morphology diagram of Example 1 of the present invention;

[0034] Fig.11 This is an enlarged view of the printing morphology of Example 1 of the present invention;

[0035] Fig.12 This is the printing morphology of Comparative Example 1;

[0036] Fig.13 This is an enlarged view of the printing morphology of Comparative Example 1. DETAILED DESCRIPTION

[0037] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation mode, structure, characteristics and effects of the present invention are described in detail below in combination with the accompanying drawings and preferred embodiments.

[0038] Embodiment 1:

[0039] like Figure 5 As shown, the present invention discloses a printing template, including a screen frame 1, a border yarn 2, a metal mesh 3 and a shielding film layer 5, a printed pattern is arranged on the shielding film layer 5, the shielding film layer 5 is covered on the metal mesh 3, and an upwardly protruding structure is formed on the metal mesh 3 corresponding to the ink-permeable area 4 of the printed pattern of the shielding film layer 5, and the lower surface of the metal mesh 3 within the range of the upwardly protruding structure should be higher than the lower surface of the metal mesh 3 corresponding to the non-ink-permeable area.

[0040] like Figure 6-Figure 9 As shown, an upwardly protruding structure is pressed on the metal mesh 3, so that the metal mesh 3 corresponding to the ink-permeable area 4 is arched upward, so that the space of the ink-permeable area 4 of the shielding film layer 5 is increased, and the effective film layer of the ink-permeable area 4 is a whole film, so the fluidity of the ink in the ink-permeable area 4 is increased, and the printing effect is also increased accordingly.

[0041] The lower surface of the metal mesh 3 within the upwardly protruding structural range is higher than the upper surface of the shielding film layer 5 on both sides of the ink permeable area 4. This structure ensures that when the ink flows and falls from the ink permeable area 4, the top metal mesh 3 does not contact the ink and does not generate adsorption force, so the ink in each part of the ink permeable area 4 falls more evenly and stably, and the printed lines formed have good flatness and straightness.

[0042] The upwardly protruding structure formed on the metal mesh 3 is an arc-shaped structure 6. Of course, the upwardly protruding structure formed on the metal mesh 3 can be in the shape of a step, as long as it can increase the ink flow space for the ink permeable area 4. Preferably, the arc-shaped structure 6 is used, which can be pressed by molding or rolling. The arc-shaped structure 6 has a small deformation amplitude on the metal mesh 3, and the metal mesh 3 has high stability, thereby ensuring the performance of the metal mesh 3 during the printing process.

[0043] The metal mesh 3 is a woven mesh, an electroformed mesh, an etched mesh or a laser cut mesh. There is no specific requirement for the form of the metal mesh 3. The metal mesh 3 in the above form can be used to increase the space of the ink permeable area 4 after pressing the arc structure 6, and the ink fluidity is better.

[0044] The metal mesh 3 within the range of the arc structure 6 is locally drawn, and the number of drawn wires is 1-6. The specific number of drawn wires is determined according to the actual situation, and 2-4 wires are preferably drawn, such as 2 wires, 3 wires, or 4 wires. In this embodiment, 2 wires are drawn, which means that 2 wires are drawn within the range of each arc structure 6 to achieve no net knots within the range of the arc structure 6. The metal mesh 3 that can be drawn is generally a woven mesh. The wire drawing can be performed on the metal mesh 3 corresponding to the ink permeable area 4 to reduce the number of metal wires in the ink permeable area 4 and achieve no net knots. Under the condition of ensuring the connection strength and integrity of the metal mesh 3, the space of the ink permeable area 4 can be further increased, the ink fluidity can be increased, and finally the flatness and straightness of the printed lines can be improved.

[0045] A method for preparing a printing template,

[0046] Step 1:

[0047] (1) Cut the metal mesh 3 as needed, and cut the sheet mesh of appropriate size as needed. The metal mesh 3 can be a woven mesh, an electroformed mesh, an etched mesh, or a laser cut mesh, and the selection is made according to actual needs;

[0048] (2) pressing the upwardly protruding arc structure 6 on the metal mesh 3 by molding or rolling to form a plastically deformed metal mesh 3;

[0049] According to the shape, spacing and number of the printed graphics, a corresponding mold plate or roller is made, and the metal mesh 3 is pressed by the mold plate or roller to form an upwardly protruding arc structure 6. Under normal circumstances, the arc structure 6 of the pressed metal mesh 3 protrudes from the upper surface of other areas of the metal mesh 3 by 1-50μm, preferably 2-10μm; the specific protruding height can be selected according to actual needs, such as 3μm, 5μm, 6μm, 8μm, 9μm, etc.

[0050] Step 2:

[0051] (1) Fixing the plastically deformed metal mesh 3 on the edge yarn 2 on the mesh frame 1;

[0052] (2) preparing a shielding film layer 5 on the metal mesh 3, coating a photosensitive adhesive on the metal mesh 3, or pasting a polymer film or a metal film on the metal mesh 3;

[0053] The photosensitive adhesive can be a positive adhesive or a negative adhesive, which can be selected according to actual needs. The polymer film can be a polymer material such as PI, PET, PA, etc. The metal film can be nickel foil, nickel alloy foil, copper foil, etc.

[0054] (3) Preparing printed patterns by exposure and development, or preparing printed patterns by laser lithography or micro-etching.

[0055] Before preparing the printed pattern, the position of the arc structure 6 on the metal mesh 3 is determined by surveying and scanning equipment, and coordinate positioning is performed so that the prepared printed pattern corresponds to the arc structure 6.

[0056] In the actual preparation process, the metal mesh 3 can be first pressed out with an arc-shaped protrusion by molding or rolling and then fixed on the mesh frame 1 through the edge yarn 2; or the metal mesh 3 can be first fixed to the mesh frame 1 through the edge yarn 2 and then pressed out with an arc-shaped protrusion by molding or rolling.

[0057] The metal mesh 3 can be directly prepared by an electroforming process to make a reverse electroforming master mold according to the number, spacing and shape of the printed patterns.

[0058] The metal mesh 3 can also be made into a casting template according to the number, spacing and shape of the printed graphics, and the preparation is achieved by casting.

[0059] The metal mesh 3 can also be prepared by an etching process of a metal foil.

[0060] Embodiment 1: The metal mesh 3 and the ink permeable area 4 are pressed into an arc structure 6 at the corresponding position, and then a shielding film layer 5 is arranged to prepare a printing template.

[0061] Comparative Example 1: The metal mesh 3 is directly compounded with the shielding film layer 5 to prepare a printing template.

[0062] The difference between Example 1 and Comparative Example 1 is that the metal mesh 3 in Example 1 is pressed into an arc-shaped structure 6, while the metal mesh 3 in Comparative Example 1 is not pressed.

[0063] Example 1 and Comparative Example 1 were compared in an experiment, and the experimental parameters were designed as follows:

[0064]

[0065] The printing results of the printing template of Example 1 and the printing template of Comparative Example 1 are as follows:

[0066] Compared with comparative example 1, the printing morphology fluctuation of example 1 is reduced by 1.69μ, the height is increased by 1.1μ, and the width remains the same.

[0067]

[0068] The printed lines of Example 1 are compared with the printed lines of Comparative Example 1. Fig.10 , Fig.11 The printed morphology image and the enlarged image of the printed lines printed by the printing template of the present embodiment 1;

[0069] Fig.12 , Fig.13The following is a printed morphology diagram and an enlarged diagram of the printed lines printed by the printing template of Comparative Example 1. Figure 10-13 It can be seen from the comparison that the metal mesh 3 will block the flow of silver paste, causing large fluctuations in the printed lines. In the present embodiment 1, the metal mesh 3 of the ink permeable area 4 is pressed into an upwardly convex arc structure 6, which increases the space of the ink permeable area 4 and does not block the flow of silver paste, thereby reducing the fluctuations in the printed lines and making the whole smoother.

[0070] The ink described in this application refers to paste. The paste used in different printing occasions is different. The ink in this embodiment 1 refers to silver paste.

[0071] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simplified modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A printing template, comprising a screen frame, a side yarn, a metal mesh and a shielding film layer, characterized in that: A printed pattern is provided on the shielding film layer, and the shielding film layer is covered on the metal mesh. An upwardly protruding structure is formed on the metal mesh corresponding to the ink-permeable area of ​​the printed pattern of the shielding film layer. The lower surface of the metal mesh within the upwardly protruding structure should be higher than the lower surface of the metal mesh corresponding to the non-ink-permeable area.

2. A printing template according to claim 1, characterized in that: The position of the lower surface of the metal mesh within the upwardly protruding structural range is higher than the position of the upper surface of the shielding film layer on both sides of the ink-permeable area.

3. A printing template according to claim 1 or 2, characterized in that: The upwardly protruding structure formed on the metal mesh is an arc-shaped structure.

4. A printing template according to claim 3, characterized in that: The metal mesh is a woven mesh, an electroformed mesh, an etched mesh or a laser cut mesh.

5. A printing template according to claim 3, characterized in that: The metal mesh yarn within the arc structure is locally drawn, and the number of drawn wires is 1-6.

6. A method for preparing a printing template, characterized in that: Step 1: (1) Cut the metal mesh as needed; (2) Pressing an upwardly protruding arc structure on the metal mesh by molding or rolling to form a plastically deformed metal mesh; Step 2: (1) Fixing the plastically deformed metal mesh on the edge mesh on the mesh frame; (2) preparing a shielding film layer on the metal mesh, coating the metal mesh with a photosensitive adhesive, or laminating a polymer film or a metal film on the metal mesh; (3) Preparing printed patterns by exposure and development, or preparing printed patterns by laser lithography or micro-etching.

7. The method for preparing a printing template according to claim 6, characterized in that: Before preparing the printed pattern, the position of the arc structure on the metal mesh is determined by surveying and scanning equipment, and coordinate positioning is performed so that the prepared printed pattern corresponds to the arc structure.

Citation Information

Patent Citations

  • Knotless screen printing plate and manufacturing process thereof

    CN112937076A

  • Diversified yarn thick screen printing plate and preparation process thereof

    CN117885433A

  • Screen printing plate

    CN220681899U

  • Metal gauze and printing screen

    CN221233262U

  • Stepped opening net-knot-free printing screen