Long-circulation graphite negative electrode material as well as preparation method and application thereof
Through multi-layer gradient temperature-retardant coking process and pulverized graphitization technology, artificial graphite negative electrode materials with high particle size shrinkage were prepared, which solved the problem of insufficient cycle times in the existing technology, and achieved high-performance long cycle characteristics and high capacity Retention rate to meet the needs of the new energy industry.
Patent Information
- Application Number
- CN202411125589.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The artificial graphite negative electrode material that is difficult to achieve long cycle characteristics in lithium-ion batteries has a cycle time of less than 15,000 weeks, and lacks customized and personalized R&D and back-end product design, making it difficult to meet the demand for high performance in the new energy industry. .
The delayed coking process with multi-layer gradient heating is used to prepare needle-shaped coke with high volatile components and high Hastello grinding index. Through crushing and rapid graphitization, a higher particle size shrinkage is achieved, and artificial graphite negative electrode with long cycle characteristics is obtained. Material. Specific steps include filtration, delayed coking, pulverization and graphitization, with a graphitization temperature of 2900-3000°C and a time of 48h-54h to obtain a long-circulated graphite negative electrode material with a particle size shrinkage of 67%.
The capacity retention rate of the buckle battery at 5000 weeks is achieved by achieving a capacity retention rate of more than 87.6%, with cycles of more than 15,000+, and up to 18,000+, meeting the new energy industry's demand for high-performance artificial graphite anode materials.
Smart Images

Figure CN118908199A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a long-cycle graphite negative electrode material and a preparation method and application thereof, belonging to the field of artificial graphite negative electrode materials for lithium ion batteries, and in particular to a preparation process of artificial graphite with higher particle size shrinkage. Background Art
[0002] Needle coke is the most mainstream raw material for the preparation of artificial graphite negative electrode materials. Its physical and electrochemical properties are closely related to the comprehensive performance of artificial graphite negative electrode materials. With the rapid development of the new energy industry, the market has higher and higher performance requirements for artificial graphite, and there are more and more demands for customization or personalization. At present, there are clear different performance requirements in the market, such as long cycle, high capacity, high compaction, high rate, easy processing and other characteristics. With the advancement of CTP battery replacement and V2G operation modes, the demand for long cycle is particularly urgent in the recent market and is widely used in energy storage system batteries and power system batteries. From a macro perspective, the key factors affecting cycle performance are divided into raw materials, that is, needle coke properties, and back-end product design.
[0003] At present, in terms of the direction of improving the cycle performance of artificial graphite, the disclosed patents and literatures all improve from a single perspective, such as conducting product research and design from the direction of the back-end design of needle coke or from the product application end such as the battery cell end. The trend value of cycle performance is difficult to exceed 15,000 cycles, and the number of cycles above 18,000 cycles is even rarer. There are almost no cases or products based on the customized / personalized research and development of needle coke for artificial graphite as a negative electrode material, and the process design of artificial graphite at the back end, the research and development of personalized products with long cycles, and artificial graphite negative electrode materials for lithium-ion batteries. Therefore, it is an inevitable trend to improve the performance of needle coke, the raw material of artificial graphite, while matching the back-end product design.
[0004] This article invents an artificial graphite negative electrode material, which first prepares needle coke with high volatile matter and high Hastelloy grindability index through a multi-level gradient temperature delayed coking process; then uses this as the raw material, crushes it, and rapidly graphitizes it to achieve a high particle size shrinkage, and finally obtains an artificial graphite negative electrode material with long cycle characteristics. Summary of the invention The specific technical solution of the present invention to solve the above technical problems is: a method for preparing a long-cycle graphite negative electrode material, characterized in that: using FCC slurry as a raw material, filtering, delayed coking, crushing and grading, and graphitizing to obtain an artificial graphite negative electrode material, comprising the following steps; Step 1: Filter the FCC slurry through a filter to remove solid impurities. Step 2: The filtered oil slurry is subjected to delayed coking treatment, cooled to room temperature and then directly decoked to obtain needle coke. Step 3: crush the needle coke to a particle size of DQ = Dv50 = 15.0 ± 0.5 μm. Step 4: The crushed needle coke is graphitized at a graphitization temperature of 2900-3000°C and a graphitization time of 48h-54h to obtain a long-cycle graphite negative electrode material. The particle size after graphitization is DH=Dv50=10.0±0.5μm.
[0006] Furthermore, the delayed coking treatment adopts a uniform gradient temperature increase, and the temperature curve is 445±5°C→50±5h→475±5°C.
[0007] Furthermore, the FCC slurry oil has an aromatic content of 60±5%, a residual carbon content of 10±2%, and a total content of aromatic hydrocarbons with less than 2 rings and cycloalkanes with less than 2 rings of 25±5%.
[0008] Furthermore, the volatile matter of the decoked needle coke is 10%±3%, and the Hastelloy grindability index is 110±10.
[0009] A long-circulation graphite negative electrode material is characterized in that it is prepared by the preparation method of the long-circulation graphite negative electrode material, and the particle size shrinkage Ds50 of the long-circulation graphite negative electrode material is the ratio of Dv50 after graphitization to Dv50 before graphitization, Ds50=DH / DQ=67±5%, and the Dv50 refers to the particle size corresponding to 50% in the volume distribution, and the particle size is DH=Dv50=10.0±0.5μm.
[0010] The purpose of long-cycle graphite negative electrode material is to use long-cycle graphite negative electrode material to prepare button batteries.
[0011] Furthermore, the capacity retention rate of the button battery at 5000 cycles is greater than 87.6%.
[0012] Furthermore, the button battery has a cycle number trend value of more than 15000.
[0013] Furthermore, the trend value of the button battery cycle number is above 18000+.
[0014] The beneficial effects of the present invention are: The present invention provides a long-cycle graphite negative electrode material and a preparation method thereof. The long-cycle graphite negative electrode material prepared by the preparation method of the long-cycle graphite negative electrode material within the protection scope of the present invention can ensure that when Ds50=DH / DQ=67±5%, the capacity retention rate of the button battery at 5000 cycles is greater than 87.6%, under the premise that the Dv50 particle size DH after graphitization is 10.0±0.5μm. The button-type battery prepared using this long-cycle graphite negative electrode material has a cycle life of more than 15,000 cycles at 25°C and a charge and discharge rate of 1C / 1C, with a capacity retention rate of 80% as the evaluation limit. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Attached Figure 1 This is a SEM image of the graphitized product of Example 1 of the present invention; Attached Figure 2 This is a schematic diagram of the relationship between the feeding time and the cycle performance of the present invention; Attached Figure 3 is the Dv50 particle size spectrum of the pulverized needle coke in Example 1 of the present invention; Attached Figure 4 This is the Dv50 particle size spectrum of the long-cycle graphite negative electrode material after graphitization in Example 1 of the present invention; Attached Figure 5 It is a cycle performance test and cycle trend prediction diagram of the present invention. DETAILED DESCRIPTION
[0016] In the description of the present invention, specific details are only for a full understanding of the embodiments of the present invention, but those skilled in the art should know that the implementation of the present invention is not limited to these details. In addition, well-known structures and functions are not described or shown in detail to avoid blurring the key points of the embodiments of the present invention. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0017] Specific implementation of the present invention: Example
[0018] Using FCC slurry oil as raw material, the aromatic content of FCC slurry oil is 60±5%, the residual carbon content is 10±2%, and the total content of aromatic hydrocarbons with less than 2 rings and cycloalkanes with less than 2 rings is 25±5%; The artificial graphite negative electrode material is obtained by filtering, delayed coking, crushing and grading, and graphitization, including the following steps: Step 1: Filter the FCC slurry through a filter to remove solid impurities. The second step: subjecting the filtered oil slurry to delayed coking treatment, wherein the delayed coking treatment adopts a uniform gradient temperature increase, and the temperature curve is 445±5℃→50±5h→475±5℃; after water cooling to room temperature, the oil slurry is directly decoked to obtain needle coke. Step 3: crushing the needle coke, and the particle size of the needle coke after crushing is DQ=Dv50=15.0±0.5μm; Step 4: Graphitize the crushed needle coke at a graphitization temperature of 2900-3000°C and a graphitization time of 48h-54h to obtain a long-cycle graphite negative electrode material.
[0019] According to the above method, FCC slurry is obtained by purchasing. The model characteristics of FCC slurry are as follows: the content of aromatic components (one of the four components, the other three are saturated components, colloids, and asphaltene) in FCC slurry is 60±5%, the residual carbon content is 10±2%, the total content of aromatic hydrocarbons with less than 2 rings and cycloalkanes with less than 2 rings is 25±5%, and the total amount of metals (calcium, vanadium, manganese, iron, nickel, copper, lead, titanium, chromium) after filtration is less than 10ppm. The same batch of FCC slurry is used as raw material, and parallel examples are implemented for different delayed coking processes and relevant indicators are tested. In order to more intuitively demonstrate the process advantages of the present invention, the preparation method of the long-cycle graphite negative electrode material of the present invention is compared with the method of equivalent replacement using the same process. Comparative Examples 1-8: The preparation method is the same as that of the embodiment, except that: in the preparation process of this comparative example, parallel comparative examples are carried out for different delayed coking treatments. The same batch of FCC slurry oil was used as raw material, and the graphite negative electrode material was prepared through filtration, delayed coking, crushing and classification, and graphitization. The process and effect parameters of Examples 1-6 and Comparative Examples 1-6 are shown in Table 1.
[0020] The evaluation of cycle performance is expressed by the number of cycles until the full battery room temperature cycle test reaches 80% capacity retention. The full battery is designed as a 1Ah soft pack battery, in which the preparation of the negative electrode sheet is to dissolve polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) solvent, add a conductive agent (SP), stir evenly, and then add a modified artificial graphite negative electrode material (among which, the modified artificial graphite negative electrode material: PVDF: NMP: SP = 95.0: 1.5: 1.5: 2.0), stir evenly again to complete the slurry, and then coat (single-sided surface density is 7g / cm3), preheat and dry, roll press, dry, roll press twice, die cut, cut pieces, and assemble to obtain a button battery; the electrolyte uses 1M LiPF6, EC: DEC: DMC = 1: 1: 1 (volume ratio), the counter electrode is lithium cobalt oxide, the charge and discharge cut-off voltage is 3.0V-4.3V, the charge and discharge rate is 1C / 1C, and the test temperature is 25°C. It should be noted that since the cycle performance test period of long cycle characteristics is too long (generally ≥10 years), the industry-recognized evaluation method is to predict the final cycle performance through the trend of the cycle capacity retention rate curve after a period of testing (≥2000 cycles). The cycle performance test and cycle trend prediction chart are shown in the figure below. Figure 5 shown.
[0021] Ds50 is the particle size shrinkage of long-cycle graphite negative electrode materials, which is the ratio of Dv50 after graphitization to Dv50 before graphitization. This indicator affects the capacity retention rate and cycle number at 5000 cycles; Among them, Dv50 after graphitization is DH=10.0±0.5μm; Dv50 before graphitization is DQ=15.0±0.5μm; Dv50 refers to the particle size corresponding to 50% in the volume distribution. The particle size was measured by laser diffraction using a Malvern 3000 laser particle size analyzer; specific test data are shown in Table 1:
[0022] According to the data analysis in Table 1: (1) Examples 1-6, the long-cycle graphite negative electrode materials prepared by the preparation method of the long-cycle graphite negative electrode materials within the protection scope of the present invention, can ensure that when Ds50=DH / DQ=67±5%, the capacity retention rate of the button battery at 5000 cycles is greater than 87.6%, and the trend value of the battery cycle number is more than 15000+, and can reach up to 18000+; (2) Example 1 is compared with Comparative Examples 5-6: the same uniform gradient heating rate as the present invention is adopted, that is, 0.5°C / h, the difference is that the temperature range is different, that is, the initial temperature and the end temperature are both beyond the range specified by the present invention, but the uniform gradient heating rate is the same as the present invention; According to the experimental results, the Ds50=DH / DQ of comparative examples 5-6 is 99% and 50%, the capacity retention rate of button batteries at 5000 cycles is 11.0% and 27.4%, and the trend value of battery cycle times is 2000+ and 5000+; Therefore, under the same uniform gradient heating rate as the present invention, that is, the temperature curve is 445±5℃→50±5h→475±5℃, it is proved that the temperature range affects Ds50 and has an impact on the capacity retention rate and battery cycle number trend value of the button battery at 5000 cycles; (3) The difference between the embodiment and comparative examples 1-4 is that the temperature range and the heating rate are different. Although comparative examples 1-4 have the same starting temperature or ending temperature as the present invention, the heating rates are different. According to the experimental results, Ds50=DH / DQ of comparative examples 1-4 is 80%, 55%, 55% and 90%, the capacity retention rate of button batteries at 5000 cycles is 43.8%, 49.3%, 60.2% and 21.9%, and the trend values of battery cycle times are 8000+, 9000+, 11000+ and 4000+, which are much lower than 18000+ of the present invention; there is a certain correlation between Ds50 and the capacity retention rate of button batteries at 5000 cycles and the trend value of battery cycle times. It can be seen that different temperature ranges and different heating rates also affect Ds50, and Ds50 has an impact on the capacity retention rate of button batteries at 5000 cycles and the trend value of battery cycle times; In addition, compared with Comparative Examples 1-4, although Comparative Examples 5-6 have the same uniform gradient heating rate as the present invention, the effect is lower than Comparative Examples 1-4; therefore, the temperature range is different, that is, the initial temperature and the end temperature are beyond the range defined by the present invention, which has a greater impact on Ds50, the capacity retention rate of the button battery at 5000 cycles and the trend value of the battery cycle number, but excludes a simple linear relationship; The uniform gradient heating rate of the temperature curve of 445±5℃→50±5h→475±5℃ has no significant effect on Ds50, the capacity retention rate of button batteries at 5000 cycles and the trend value of battery cycle times.
[0023] (4) Comparison between Comparative Example 3 and Comparative Example 7: The difference is that the uniform gradient heating rate is different. According to Table 4, Ds50=DH / DQ of Comparative Examples 1, 7 and 8 are: 80%, 80% and 55%, the capacity retention rate of button batteries at 5000 cycles is: 43.8%, 32.8% and 54.8%, and the trend value of battery cycle times is 8000+, 6000+ and 10000+; It can be seen that under the same temperature range as the present invention, that is, the temperature curve is 445±5℃→475±5℃, it is proved that the different uniform gradient heating rates will also affect Ds50 and the capacity retention rate and battery cycle number trend value of the button battery at 5000 cycles; (5) Compared with Example 1 and Comparative Example 7: The difference is that the particle size DH of Dv50 after graphitization is different, while the particle size DH of Dv50 after graphitization is different under the same delayed coking treatment conditions, and DH depends on Dv50 before graphitization as DQ; According to Table 4, Example 1 and Comparative Example 7 have the same delayed coking treatment conditions and the same Ds50, that is, Ds50=DH / DQ of Example 1 and Example 7 are both 67%, and the capacity retention rates of the button batteries at 5000 cycles are 98.6% and 66.7%, respectively. The trend values of the battery cycle times are 18000+ and 12000+.
[0024] This shows that: when Ds50=DH / DQ=67±5%, the capacity retention rate of the button battery at 5000 cycles is greater than 87.6%, and the trend values of the battery cycle times are all above 15000+. The prerequisite for reaching 18000+ is that the Dv50 particle size DH after graphitization is 10.0±0.5μm. Otherwise, even if Ds50=DH / DQ=67±5%, the capacity retention rate of the button battery at 5000 cycles is greater than 87.6%, and the trend values of the battery cycle times are all above 15000+.
[0025] In order to more intuitively demonstrate the process advantages of the present invention, the equivalent replacement method is used for comparison, and the effect of the heating rate of the delayed coking process on the product performance is studied. The preparation methods of Comparative Examples 1-7, Comparative Examples 1-8, Comparative Examples 1-9 and Comparative Examples 1-10 are the same as those of the embodiment, except that the heating rates of delayed coking treatment in Comparative Examples 1-7, Comparative Examples 1-8, Comparative Examples 1-9 and Comparative Examples 1-10 are different; and parallel comparisons are performed, as shown in Table 2:
[0026] From the data analysis in Table 2, we can see that: Compared with Comparative Examples 1-7, 1-8, 1-9 and 1-10, the delayed coking treatment in Example 1 has a different heating rate; as the feeding time increases, the heating rate decreases, and under the premise of the same DQ, the change trend of Ds50 does not show a linear relationship, but presents a curve that first increases and then decreases. Therefore, under the premise of the same DQ, the different heating rates of the delayed coking treatment are not positively correlated with Ds50, and further, are not positively correlated with the capacity retention rate of the button battery at 5000 weeks and the trend value of the number of battery cycles.
[0027] In summary: the present invention provides a long-cycle graphite negative electrode material and a preparation method thereof. The long-cycle graphite negative electrode material prepared by the preparation method of the long-cycle graphite negative electrode material within the protection scope of the present invention can ensure that when Ds50=DH / DQ=67±5%, the capacity retention rate of the button battery at 5000 cycles is greater than 87.6%, under the premise that the Dv50 particle size DH after graphitization is 10.0±0.5μm. The button-type battery prepared using this long-cycle graphite negative electrode material has a cycle life of more than 15,000 cycles at 25°C and a charge and discharge rate of 1C / 1C, with a capacity retention rate of 80% as the evaluation limit.
Claims
1. A method for preparing a long-cycle graphite negative electrode material, characterized in that: Using FCC oil slurry as raw material, filtering, delayed coking, crushing and grading, and graphitizing to obtain artificial graphite negative electrode material, including the following steps; Step 1: Filter the FCC slurry through a filter to remove solid impurities. The second step: the filtered oil slurry is subjected to delayed coking treatment, and then directly decoked after being cooled to room temperature to obtain needle coke. Step 3: crushing the needle coke, and the particle size of the needle coke after crushing is DQ=15.0±0.5μm; Step 4: Graphitize the crushed needle coke at a graphitization temperature of 2900-3000°C and a graphitization time of 48h-54h to obtain a long-cycle graphite negative electrode material.
2. The method for preparing a long-cycle graphite negative electrode material according to claim 1, characterized in that The delayed coking treatment adopts uniform gradient temperature increase, and the temperature curve is 445±5°C→50±5h→475±5°C.
3. The method for preparing a long-cycle graphite negative electrode material according to claim 1 or 2, characterized in that The FCC oil slurry has an aromatic content of 60±5%, a residual carbon content of 10±2%, and a total content of aromatic hydrocarbons with less than 2 rings and cycloalkanes with less than 2 rings of 25±5%.
4. The method for preparing a long-cycle graphite negative electrode material according to claim 1 or 2, characterized in that The volatile matter of the needle coke after decoking is 10%±3%, and the Hastelloy grindability index is 110±10.
5. A long-cycle graphite negative electrode material characterized by The long-cycle graphite negative electrode material is prepared by the preparation method of any one of claims 1-2, wherein the particle size shrinkage Ds50 of the long-cycle graphite negative electrode material is the ratio of Dv50 after graphitization to Dv50 before graphitization, Ds50=DH / DQ=67±5%, and the Dv50 refers to the particle size corresponding to 50% in the volume distribution, and the particle size after graphitization DH=10.0±0.5μm.
6. Use of long-cycle graphite negative electrode material, characterized in that The long-cycle graphite negative electrode material of claim 5 is used to prepare button batteries.
7. The use of the long-cycle graphite negative electrode material according to claim 6, characterized in that The capacity retention rate of the button battery at 5000 cycles is greater than 87.6%.
8. The use of the long-cycle graphite negative electrode material according to claim 7, characterized in that The button battery has a cycle number trend value of more than 15000.
9. The use of the long-cycle graphite negative electrode material according to claim 8, characterized in that The trend value of the button battery cycle number is above 18000+.
Citation Information
Patent Citations
Graphite material and preparation method thereof, negative electrode and lithium ion battery
CN109768217A
Synthetic graphite material, synthetic graphite material production method, negative electrode for lithium ion secondary battery, and lithium ion secondary battery
CN113365942A
Artificial graphite material for negative electrode of lithium ion secondary battery and method for producing same
CN115699369A
Electrode material for secondary battery
JP1998241679A
Process for producing coke
US20030098260A1