Manganese zinc ferrite with low stress sensitivity and sintering method thereof

Through the multi-stage sintering process, the manganese zeolite material is gradually heated up and cooled down, which solves the problem of stress sensitivity of manganese zeolite in the sintering process, and significantly improves its inductance stability and performance, especially in large-scale products The influence of stress on inductor is effectively reduced.

CN118908709AActive Publication Date: 2024-11-08HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411157075.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing high permeability manganese-zeb ferrite materials are susceptible to stress in the sintering process, resulting in a decrease in inductance. Especially large-sized products are more significantly affected by stress, which fails to effectively solve the problem of performance degradation of magnetic cores under stress.

Method used

The multi-stage sintering method of primary, secondary, tertiary and quadratic sintering with increasing temperature gradient is adopted. By gradually increasing the temperature and cooling, moisture is eliminated, PVA is evaporated, acid ions are eliminated, grain growth is promoted, and grain growth is reduced. The volatility of zinc oxide increases density and prepares low-stress-sensitive manganese-zeb ferrite.

Benefits of technology

Under the same stress, compared with traditional manganese-zeb ferrite, the prepared material has a smaller inductance drop ratio, has wide frequency, high impedance, and high conductivity, and has superior performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005305550000101
    Figure BDA0005005305550000101
Patent Text Reader

Abstract

The invention provides a low-stress sensitive manganese zinc ferrite and a sintering method thereof. The sintering method comprises the following steps: (1) carrying out compression molding on manganese zinc ferrite powder to obtain a blank to be sintered; and (2) carrying out multi-stage sintering on the blank to be sintered, and then cooling to obtain the low-stress sensitive manganese zinc ferrite, wherein the multi-stage sintering process consists of first-stage sintering, second-stage sintering, third-stage sintering and fourth-stage sintering of which the temperatures are increased in a gradient manner. The manganese-zinc ferrite with low stress sensitivity, wide frequency, high impedance and high conductivity is prepared by adopting a multi-stage sintering mode of first-stage sintering, second-stage sintering, third-stage sintering and fourth-stage sintering with the temperature increased in a gradient manner, and the inductance drop proportion of the manganese-zinc ferrite is smaller than that of the traditional manganese-zinc ferrite under the condition that the manganese-zinc ferrite is subjected to the same stress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic materials, and in particular relates to a low stress-sensitive manganese-zinc ferrite and a sintering method thereof. Background Art

[0002] In recent years, with the beginning of the third industrial revolution and the development of science and technology, mankind has gradually entered the electronic information age, and electronic products have become indispensable for human work, office, leisure, entertainment, study, video conferencing, etc. While electronic products bring convenience to humans, they also bring certain environmental pollution-electromagnetic interference. High magnetic permeability manganese zinc ferrite is widely used in signal transmission and anti-electromagnetic interference technology. It has been favored by customers for its high magnetic permeability, low price, and product miniaturization. However, due to the low resistivity of high-conductivity manganese zinc ferrite materials, it is difficult to meet the withstand voltage requirements. Spraying treatment, as well as assembly and winding treatment by downstream customers are required. The subsequent operations of the above cores will produce certain stress on the cores, resulting in a decrease in the inductance of the cores, especially large-size products are more significantly affected by stress.

[0003] At present, patent CN101870578A discloses a high magnetic permeability 12000μi wide temperature manganese-zinc ferrite material, which achieves high magnetic permeability and wide temperature performance of manganese-zinc ferrite material with magnetic permeability μi=12000 by limiting the content of iron oxide to 53-58mol%, the content of zinc oxide to 20-28mol%, and the rest to manganese oxide; patent CN103011791A discloses a high magnetic permeability manganese-zinc ferrite material, which achieves high magnetic permeability and wide temperature performance of manganese-zinc ferrite material with magnetic permeability μi=12000 by limiting the content of iron oxide to 51-5 4mol%, the content of zinc oxide is limited to 23-27mol%, and the rest is manganese oxide, so as to achieve high magnetic permeability of manganese-zinc ferrite material; CN105541316A discloses a manganese-zinc ferrite material for anti-EMI and its preparation method, which limits the content of iron oxide to 50.5-52.5mol%, the content of zinc oxide to 18.5-20.5mol%, and the rest is manganese oxide, so as to achieve the preparation of manganese-zinc ferrite material for anti-EMI with magnetic permeability>12000. However, the above-mentioned prior art does not explore the influence of sintering process on stress sensitivity of magnetic core.

[0004] Therefore, developing a sintering method for manganese-zinc ferrite with low stress sensitivity so that the inductance drop of the magnetic core is smaller than that of traditional manganese-zinc ferrite under the same stress is a technical problem that needs to be solved urgently. Summary of the invention

[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a low stress-sensitive manganese-zinc ferrite and a sintering method thereof. The present invention adopts a multi-stage sintering method of primary sintering, secondary sintering, tertiary sintering and quadruple sintering with a temperature gradient increase to prepare a low stress-sensitive, broadband high-impedance and high-conductivity manganese-zinc ferrite, which has a smaller inductance drop ratio than traditional manganese-zinc ferrite under the same stress, high impedance and good performance.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a sintering method of a low stress-sensitive manganese-zinc ferrite, the sintering method comprising the following steps:

[0008] (1) pressing the manganese zinc ferrite powder into a shape to obtain a sintered blank;

[0009] (2) performing multi-stage sintering on the blank to be sintered, and then cooling the blank to obtain the low stress-sensitive manganese-zinc ferrite;

[0010] The multi-stage sintering process includes primary sintering, secondary sintering, tertiary sintering and quaternary sintering with the temperature increasing in a gradient.

[0011] The present invention adopts a multi-stage sintering method of primary sintering, secondary sintering, tertiary sintering and quadruple sintering with a temperature gradient increase to prepare a manganese-zinc ferrite with low stress sensitivity, wide-band high impedance and high conductivity. The inductance drop ratio of the manganese-zinc ferrite is smaller than that of the traditional manganese-zinc ferrite under the same stress.

[0012] As a preferred technical solution of the present invention, the initial magnetic permeability of the manganese-zinc ferrite powder in step (1) is ≥10000, for example, it can be 10000, 12000 or 15000.

[0013] Preferably, the blank to be sintered is a standard sample ring blank with a size of 50 mm×20 mm×25 mm.

[0014] It should be noted that large-sized manganese-zinc ferrite is more susceptible to stress, but the technical solution provided by the present invention can effectively avoid this problem and obtain a wide-band, high-impedance and high-conductivity manganese-zinc ferrite material.

[0015] As a preferred technical solution of the present invention, the temperature of the primary sintering is 120-220°C, for example, it can be 120°C, 140°C, 160°C, 180°C, 200°C or 220°C.

[0016] Preferably, the primary sintering time is 3-5 h, for example, 3 h, 3.5 h, 4 h, 4.5 h or 5 h.

[0017] The present invention performs primary sintering at 120-220° C. for 3-5 hours, which can fully remove moisture from the blank.

[0018] Preferably, during the primary sintering process, an oxygen-containing gas is introduced, and the flow rate of the oxygen-containing gas is 20-40 m 3 / h, for example, it can be 20m 3 / h、25m 3 / h、30m 3 / h、35m 3 / h or 40m 3 / h, etc. Exemplarily, the oxygen-containing gas may be air.

[0019] As a preferred technical solution of the present invention, the temperature of the secondary sintering is 500-700°C, for example, it can be 500°C, 550°C, 600°C, 650°C or 700°C.

[0020] Preferably, the secondary sintering time is 2-3 h, for example, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h or 3 h.

[0021] The present invention performs secondary sintering at 500-700° C. for 2-3 hours, which is helpful to realize the volatilization of PVA (polyvinyl alcohol) at a low melting point position.

[0022] Preferably, during the secondary sintering process, an oxygen-containing gas is introduced, and the flow rate of the oxygen-containing gas is 30-40 m / s. 3 / h, for example, 30m 3 / h、32m 3 / h、34m 3 / h、36m 3 / h、38m 3 / h or 40m 3 / h, etc. Exemplarily, the oxygen-containing gas may be air.

[0023] As a preferred technical solution of the present invention, the temperature of the three-stage sintering is 900-1200°C, for example, it can be 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C or 1200°C, preferably 1050-1150°C.

[0024] Preferably, the three-stage sintering time is 3-5 hours, for example, it can be 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours.

[0025] The present invention performs three-stage sintering at 900-1200° C. for 3-5 hours, which helps to remove acid ions (such as sulfate ions) in the blank.

[0026] Preferably, during the three-stage sintering process, an oxygen-containing gas is introduced, and the flow rate of the oxygen-containing gas is 30-35m 3 / h, for example, 30m 3 / h、31m 3 / h、32m 3 / h、33m 3 / h、34m 3 / h or 35m 3 / h, etc. Exemplarily, the oxygen-containing gas may be air.

[0027] As a preferred technical solution of the present invention, the temperature of the four-stage sintering is 1300-1420°C, for example, it can be 1300°C, 1320°C, 1340°C, 1360°C, 1380°C, 1400°C or 1420°C.

[0028] Preferably, the time of the four-stage sintering is 6-10 hours, for example, it can be 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.

[0029] The present invention performs four-stage sintering at 1300-1420° C. for 6-10 hours, which can promote grain growth and improve density.

[0030] Preferably, the four-stage sintering is performed in a protective atmosphere, and the gas in the protective atmosphere includes nitrogen.

[0031] Preferably, the gas in the protective atmosphere also includes oxygen, and the content of oxygen is ≤21 vol%, for example, it can be 21 vol%, 20 vol%, 15 vol%, 10 vol%, 5 vol% or 1 vol%, etc., preferably 11-20 vol%.

[0032] In the present invention, it is preferred that the green body is subjected to four-stage sintering under the condition that the oxygen content is less than 11-20 vol%, which helps to reduce the volatilization of zinc oxide.

[0033] As a preferred technical solution of the present invention, the cooling process in step (2) is carried out in an atmosphere of balanced oxygen partial pressure.

[0034] Preferably, the cooling rate of step (2) is 0-3°C / min, for example, 0, 1°C / min, 2°C / min or 3°C / min.

[0035] As a preferred technical solution of the present invention, the sintering method comprises the following steps:

[0036] (1) pressing and molding a manganese-zinc ferrite powder with an initial magnetic permeability of ≥10000 to obtain a sintered blank with a size of 50 mm×20 mm×25 mm, wherein the sintered blank is a standard sample ring blank;

[0037] (2) The blank to be sintered is subjected to primary sintering at 120-220° C. for 3-5 hours, and the flow rate during the primary sintering is 20-40 m 3 / h of oxygen-containing gas, and then heated to 500-700°C at a heating rate of 0-2°C / min (for example, 0, 1°C / min or 2°C / min, etc.) for 2-3h secondary sintering, and the flow rate during the secondary sintering is 30-40m 3 / h of oxygen-containing gas, and then heated to 900-1200°C at a heating rate of 1-2°C / min (for example, 1, 1.5°C / min or 2°C / min, etc.) for 3-5h of three-stage sintering, and the flow rate during the three-stage sintering is 30-35m 3 / h of oxygen-containing gas, then heating to 1300-1420°C at a heating rate of 0-2°C / min (for example, 0, 1°C / min or 2°C / min, etc.), and performing four-stage sintering in a protective atmosphere, wherein the four-stage sintering time is 6-10h;

[0038] Wherein, the gas in the protective atmosphere includes nitrogen and oxygen, and the content of oxygen is ≤21 vol%;

[0039] (3) Cooling the sintered blank to 40-60°C (for example, 40°C, 50°C or 60°C, etc.), wherein the cooling is carried out in an atmosphere of balanced oxygen partial pressure, and the cooling rate is 0-3°C / min (for example, 0, 1°C / min, 2°C / min or 3°C / min, etc.), to obtain low stress-sensitive manganese-zinc ferrite.

[0040] In a second aspect, the present invention provides a low stress-sensitive manganese-zinc ferrite prepared by the sintering method described in the first aspect.

[0041] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The present invention adopts a multi-stage sintering method of primary sintering, secondary sintering, tertiary sintering and quadruple sintering with a temperature gradient increase to prepare a manganese-zinc ferrite with low stress sensitivity, wide-band high impedance and high conductivity. The inductance drop ratio of the manganese-zinc ferrite is smaller than that of the traditional manganese-zinc ferrite under the same stress. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0045] Example 1

[0046] This embodiment provides a sintering method for low stress-sensitive manganese-zinc ferrite, the sintering method comprising the following steps:

[0047] (1) pressing a manganese-zinc ferrite powder having an initial magnetic permeability of 10,000 to obtain a sintered blank having a size of 50 mm×20 mm×25 mm, wherein the sintered blank is a standard sample ring blank;

[0048] (2) The blank to be sintered is subjected to primary sintering at 210° C. for 3 h, and the flow rate during the primary sintering is 30 m 3 / h of air, the exhaust frequency is 35Hz, and then the temperature is raised to 530℃ at a heating rate of 1℃ / min for 3h of secondary sintering, and the flow rate during the secondary sintering process is 36m 3 / h of air, the exhaust frequency is 40Hz, and then the temperature is raised to 1100℃ at a heating rate of 2℃ / min for 5h of three-stage sintering, and the flow rate during the three-stage sintering is 32m 3 / h of air, the exhaust frequency is 40Hz, and then the temperature is raised to 1410°C at a heating rate of 1°C / min, and four-stage sintering is performed in a protective atmosphere, and the four-stage sintering time is 8h;

[0049] Wherein, the gas in the protective atmosphere includes nitrogen and oxygen, and the content of oxygen is 15 vol%;

[0050] (3) Cooling the sintered green body to 50° C., wherein the cooling is performed in an atmosphere of balanced oxygen partial pressure and the cooling rate is 3° C. / min, to obtain low stress-sensitive manganese-zinc ferrite.

[0051] Example 2

[0052] This embodiment provides a sintering method for low stress-sensitive manganese-zinc ferrite, the sintering method comprising the following steps:

[0053] (1) pressing a manganese-zinc ferrite powder having an initial magnetic permeability of 10,000 to obtain a sintered blank having a size of 50 mm×20 mm×25 mm, wherein the sintered blank is a standard sample ring blank;

[0054] (2) The blank to be sintered is subjected to primary sintering at 160° C. for 5 h, and the flow rate during the primary sintering is 30 m 3 / h of air, the exhaust frequency is 35Hz, and then the temperature is raised to 530℃ at a heating rate of 2℃ / min for 3h of secondary sintering, and the flow rate during the secondary sintering is 36m 3 / h of air, the exhaust frequency is 40Hz, and then the temperature is raised to 900℃ at a heating rate of 1℃ / min for 5h of three-stage sintering, and the flow rate during the three-stage sintering is 32m 3 / h of air, the exhaust frequency is 40Hz, and then the temperature is increased to 1410°C at a heating rate of 2°C / min, and four-stage sintering is performed in a protective atmosphere, and the four-stage sintering time is 8h;

[0055] Wherein, the gas in the protective atmosphere includes nitrogen and oxygen, and the content of oxygen is 15 vol%;

[0056] (3) Cooling the sintered green body to 50° C., wherein the cooling is performed in an atmosphere of balanced oxygen partial pressure and the cooling rate is 3° C. / min, to obtain low stress-sensitive manganese-zinc ferrite.

[0057] Example 3

[0058] This embodiment provides a sintering method for low stress-sensitive manganese-zinc ferrite, the sintering method comprising the following steps:

[0059] (1) pressing a manganese-zinc ferrite powder having an initial magnetic permeability of 10,000 to obtain a sintered blank having a size of 50 mm×20 mm×25 mm, wherein the sintered blank is a standard sample ring blank;

[0060] (2) The blank to be sintered is subjected to primary sintering at 160° C. for 5 h, and the flow rate during the primary sintering is 30 m 3 / h of air, the exhaust frequency is 35Hz, and then the temperature is raised to 700℃ at a heating rate of 1.5℃ / min for 2h of secondary sintering, and the flow rate during the secondary sintering process is 36m 3 / h of air, the exhaust frequency is 40Hz, and then the temperature is raised to 900℃ at a heating rate of 1.5℃ / min for 5h of three-stage sintering, and the flow rate during the three-stage sintering is 32m 3 / h of air, the exhaust frequency is 40Hz, and then the temperature is raised to 1410°C at a heating rate of 1.5°C / min, and four-stage sintering is performed in a protective atmosphere, and the four-stage sintering time is 8h;

[0061] Wherein, the gas in the protective atmosphere includes nitrogen and oxygen, and the content of oxygen is 15 vol%;

[0062] (3) Cooling the sintered green body to 50° C., wherein the cooling is performed in an atmosphere of balanced oxygen partial pressure and the cooling rate is 3° C. / min, to obtain low stress-sensitive manganese-zinc ferrite.

[0063] Example 4

[0064] This embodiment provides a sintering method for low stress-sensitive manganese-zinc ferrite, the sintering method comprising the following steps:

[0065] (1) pressing a manganese-zinc ferrite powder having an initial magnetic permeability of 10,000 to obtain a sintered blank having a size of 50 mm×20 mm×25 mm, wherein the sintered blank is a standard sample ring blank;

[0066] (2) The blank to be sintered is subjected to primary sintering at 160° C. for 5 h, and the flow rate during the primary sintering is 30 m 3 / h of air, the exhaust frequency is 35Hz, and then the temperature is raised to 530℃ at a heating rate of 2℃ / min for 3h of secondary sintering, and the flow rate during the secondary sintering is 36m 3 / h of air, the exhaust frequency is 40Hz, and then the temperature is raised to 1200℃ at a heating rate of 2℃ / min for 3h of three-stage sintering, and the flow rate during the three-stage sintering is 32m 3 / h of air, the exhaust frequency is 40Hz, and then the temperature is increased to 1410°C at a heating rate of 2°C / min, and four-stage sintering is performed in a protective atmosphere, and the four-stage sintering time is 8h;

[0067] Wherein, the gas in the protective atmosphere includes nitrogen and oxygen, and the content of oxygen is 15 vol%;

[0068] (3) Cooling the sintered green body to 50° C., wherein the cooling is performed in an atmosphere of balanced oxygen partial pressure and the cooling rate is 3° C. / min, to obtain low stress-sensitive manganese-zinc ferrite.

[0069] Example 5

[0070] The difference between this embodiment and embodiment 1 is that the primary sintering time is 2 hours.

[0071] The rest of the sintering methods and parameters were the same as those in Example 1.

[0072] Example 6

[0073] The difference between this embodiment and embodiment 1 is that the secondary sintering time is 1.5 hours.

[0074] The rest of the sintering methods and parameters were the same as those in Example 1.

[0075] Example 7

[0076] The difference between this embodiment and embodiment 1 is that the time of the third-stage sintering is 2.5 hours.

[0077] The rest of the sintering methods and parameters were the same as those in Example 1.

[0078] Example 8

[0079] The difference between this embodiment and embodiment 1 is that the temperature of the fourth-stage sintering is 1280°C.

[0080] The rest of the sintering methods and parameters were the same as those in Example 1.

[0081] Example 9

[0082] The difference between this embodiment and embodiment 1 is that the temperature of the fourth-stage sintering is 1450°C.

[0083] The rest of the sintering methods and parameters were the same as those in Example 1.

[0084] Example 10

[0085] The difference between this embodiment and embodiment 1 is that during the four-stage sintering process, the oxygen content is 25 vol%.

[0086] The rest of the sintering methods and parameters were the same as those in Example 1.

[0087] Performance Testing

[0088] The manganese-zinc ferrite material prepared by the sintering method in the above embodiment was subjected to a magnetic permeability test and a stress sensitivity test.

[0089] The conditions for the magnetic permeability test are: 0.25V, 25°C; the formula for the stress sensitivity test is μi(10KHz / 10MPa) / μi(10MPa / 0MPa).

[0090] The test results are shown in Table 1.

[0091] Table 1

[0092]

[0093]

[0094] analyze:

[0095] It can be seen from the above table that the sintering method provided by the present invention can prepare a manganese-zinc ferrite with low stress sensitivity, broadband high impedance and high conductivity.

[0096] It can be seen from Example 1 and Examples 8-9 that if the temperature of the four-stage sintering is too low, it is not conducive to the improvement of magnetic permeability; if the temperature of the four-stage sintering is too high, it is not conducive to the improvement of stress sensitivity.

[0097] It can be seen from Example 1 and Example 10 that if the oxygen content is too high during the four-stage sintering process, it is not conducive to improving the stress sensitivity.

[0098] The applicant declares that the present invention illustrates the process of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A sintering method for low stress sensitive manganese zinc ferrite, It is characterized in that The sintering method comprises the following steps: (1) pressing the manganese zinc ferrite powder into a shape to obtain a sintered blank; (2) performing multi-stage sintering on the blank to be sintered, and then cooling the blank to obtain the low stress-sensitive manganese-zinc ferrite; The multi-stage sintering process consists of primary sintering, secondary sintering, tertiary sintering and fourth stage sintering with the temperature increasing in a gradient.

2. The sintering method according to claim 1, It is characterized in that The initial magnetic permeability of the manganese-zinc ferrite powder in step (1) is ≥10000; Preferably, the blank to be sintered is a standard sample ring blank with a size of 50 mm×20 mm×25 mm.

3. The sintering method according to claim 1 or 2, It is characterized in that The primary sintering temperature is 120-220°C; Preferably, the primary sintering time is 3-5h; Preferably, during the primary sintering process, an oxygen-containing gas is introduced, and the flow rate of the oxygen-containing gas is 20-40 m 3 / h.

4. The sintering method according to any one of claims 1 to 3, It is characterized in that The temperature of the secondary sintering is 500-700°C; Preferably, the secondary sintering time is 2-3h; Preferably, during the secondary sintering process, an oxygen-containing gas is introduced, and the flow rate of the oxygen-containing gas is 30-40 m / s. 3 / h.

5. The sintering method according to any one of claims 1 to 4, It is characterized in that The temperature of the three-stage sintering is 900-1200°C, preferably 1050-1150°C; Preferably, the three-stage sintering time is 3-5h; Preferably, during the three-stage sintering process, an oxygen-containing gas is introduced, and the flow rate of the oxygen-containing gas is 30-35m 3 / h.

6. The sintering method according to any one of claims 1 to 5, It is characterized in that The temperature of the fourth stage sintering is 1300-1420°C; Preferably, the time of the fourth-stage sintering is 6-10 hours; Preferably, the four-stage sintering is performed in a protective atmosphere, and the gas in the protective atmosphere includes nitrogen.

7. The sintering method according to claim 6, It is characterized in that The gas in the protective atmosphere also includes oxygen, and the content of the oxygen is ≤21 vol%.

8. The sintering method according to any one of claims 1 to 7, It is characterized in that The cooling process in step (2) is carried out in an atmosphere of balanced oxygen partial pressure; Preferably, the cooling rate of step (2) is 0-3°C / min.

9. The sintering method according to any one of claims 1 to 8, It is characterized in that The sintering method comprises the following steps: (1) pressing a manganese-zinc ferrite powder having an initial magnetic permeability of ≥10,000 to obtain a sintered blank having a size of 50 mm×20 mm×25 mm, wherein the sintered blank is a standard sample ring blank; (2) The blank to be sintered is subjected to primary sintering at 120-220° C. for 3-5 hours, and the flow rate during the primary sintering is 20-40 m 3 / h of oxygen-containing gas, and then heated to 500-700°C at a heating rate of 0-2°C / min for 2-3h of secondary sintering, and the flow rate during the secondary sintering process is 30-40m 3 / h of oxygen-containing gas, and then heated to 900-1200°C at a heating rate of 1-2°C / min for 3-5h of three-stage sintering, and the flow rate during the three-stage sintering process is 30-35m 3 / h of oxygen-containing gas, then heating to 1300-1420°C at a heating rate of 0-2°C / min, and performing four-stage sintering in a protective atmosphere, wherein the four-stage sintering time is 6-10h; Wherein, the gas in the protective atmosphere includes nitrogen and oxygen, and the content of oxygen is ≤21 vol%; (3) Cooling the sintered green body to 40-60° C. in an atmosphere of balanced oxygen partial pressure at a cooling rate of 0-3° C. / min to obtain low stress-sensitive manganese-zinc ferrite.

10. A low stress-sensitive manganese-zinc ferrite prepared by the sintering method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Sintering process for preventing blank bonding during stacked sintering of manganese zinc ferrites

    CN103408308A

  • High-frequency and low-power-consumption manganese zinc ferrite sintering technology

    CN106747393A

  • Manganese-zinc ferrite material with wide temperature range and low power consumption and preparation method thereof

    CN112408969A

  • Manufacture of mnzn ferrite

    JP1993159919A

  • High-magnetic permeability, high-frequency, high-impedance, and high-curie temperature manganese-zinc ferrite material and preparation method therefor

    WO2022095577A1