Aerogel composition for battery insulating sheet, method for manufacturing aerogel composition, battery insulating sheet formed using aerogel composition, and battery module including battery insulating sheet

By using aerogel composition insulating sheet material with high BET specific surface area in lithium-ion secondary batteries, the thermal runaway and flame propagation problems between battery cells are solved, and good thermal insulation and fire protection are achieved, which improves the Safety of the battery module.

CN118909373APending Publication Date: 2024-11-08SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410561341.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In lithium-ion secondary batteries, thermal runaway between multiple battery cells may lead to heat propagation and flame, and existing insulating materials have problems such as insufficient thermal insulation performance and prone to ignition.

Method used

Aerogel composition with a high BET specific surface area is used as the battery insulating sheet material, including binders, dispersants, phosphorus-based materials and flame retardants, to form thermal insulation between the battery cells by uniformly dispersing the aerogel layer. and fire barriers.

Benefits of technology

It significantly improves the thermal insulation performance and fire resistance of the battery insulating sheet, effectively prevents heat propagation and flame propagation between the battery cells, and improves the safety of the battery module.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909373A_ABST
    Figure CN118909373A_ABST
Patent Text Reader

Abstract

The present invention relates to an aerogel composition for a battery insulating sheet, a method of manufacturing the aerogel composition, a battery insulating sheet formed using the aerogel composition, and a battery module including the battery insulating sheet. Example embodiments include an aerogel composition for a battery insulation sheet, the aerogel composition comprising: an aerogel; a functional material including a binder, a dispersant or a combination thereof; a flame retardant including a phosphorus-based material; and a solvent. Example embodiments also include a method of manufacturing the aerogel composition, a battery insulating sheet formed using the aerogel composition, and a battery module including the battery insulating sheet.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0059100 filed on May 8, 2023, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field

[0003] Example embodiments relate to an aerogel composition for a battery insulating sheet, a method of manufacturing the aerogel composition, a battery insulating sheet formed using the aerogel composition, and a battery module including the battery insulating sheet. Background Art

[0004] Secondary batteries are power storage systems that convert electrical energy into chemical energy, store chemical energy, and provide high energy density. Compared with primary batteries that cannot be recharged, secondary batteries are generally rechargeable and are widely used in information technology (IT) devices such as, for example, smart phones, mobile phones, laptop computers, tablet computers, etc. At present, there is an increasing interest in electric vehicles to reduce or prevent environmental pollution, and high-capacity secondary batteries are generally used in electric vehicles. Secondary batteries generally exhibit desired characteristics such as, for example, high density, high output, and stability.

[0005] As in a lithium ion secondary battery, when a plurality of high-capacity battery cells are included, one battery cell may overheat and may cause thermal runaway for various reasons, which may adversely affect other adjacent battery cells, and so it is desirable to thermally separate adjacent battery cells from each other.

[0006] Conventionally, a plate or an insulating resin sheet is placed between the battery cells to separate and insulate adjacent battery cells from each other. Summary of the invention

[0007] Example embodiments provide an aerogel composition for a battery insulating sheet having desired, advantageous or improved thermal insulation performance and fire resistance, a method of manufacturing the aerogel composition, a battery insulating sheet formed using the aerogel composition, and a battery module including the battery insulating sheet.

[0008] Example embodiments provide an aerogel composition for a battery insulating sheet, the aerogel composition including: an aerogel; a functional material including a binder, a dispersant, or a combination thereof; a flame retardant including a phosphorus-based material; and a solvent.

[0009] Aerogels can have a diameter of about 500 m 2 / g~1,000m 2 The Brunauer-Emmett-Teller (BET) specific surface area is in the range of 1.1747 W / g.

[0010] The aerogel may be included in a range of about 30 wt % to 90 wt % based on the total amount of solids in the aerogel composition.

[0011] The binder may include a water-based polymer binder.

[0012] The aqueous polymer binder may include at least one of an aqueous polymer, an anionic water-soluble polymer, a cationic water-soluble polymer, and a water-dispersible polymer.

[0013] The dispersant may include at least one of a surfactant and a phosphate ester salt.

[0014] The functional material may be included in a range of about 5 wt % to 55 wt % based on the total amount of solids in the aerogel composition.

[0015] The phosphorus-based material may include at least one of phosphate-based ammonium salt, red phosphorus, and compounds represented by Chemical Formula 1 and Chemical Formula 2 below.

[0016] [Chemical formula 1]

[0017]

[0018] In the above chemical formula 1, Ar 1 ~Ar 3 are each independently a substituted or unsubstituted C6-C20 aryl group, and

[0019] [Chemical formula 2]

[0020]

[0021] In the above chemical formula 2, Ar 4 ~Ar 10 Each is independently a substituted or unsubstituted C6-C20 aryl group.

[0022] The phosphate-based ammonium salt may include at least one of diammonium phosphate, diammonium hydrogen phosphate, and ammonium polyphosphate.

[0023] The flame retardant may be included in an amount ranging from about 0.01 wt % to about 20 wt % based on the total amount of solids in the aerogel composition.

[0024] The flame retardant may be included in an amount ranging from about 0.1 parts by weight to about 20 parts by weight based on 100 parts by weight of the functional material.

[0025] The solvent may include at least one of a polar solvent and a non-polar solvent.

[0026] The weight ratio of the solvent to the total amount of solids in the aerogel composition may be in the range of about 1:1 to 1:90.

[0027] Based on the total amount of solids in the aerogel composition, the aerogel may be included in a range of about 55 wt % to 75 wt %, the binder may be included in a range of about 20 wt % to 40 wt %, and the phosphorus material may be included in a range of about 0.1 wt % to 8 wt %.

[0028] Based on the total amount of solids in the aerogel composition, aerogel may be included in a range of about 55wt% to 75wt%, binder may be included in a range of about 20wt% to 40wt%, dispersant may be included in a range of about 0.1wt% to 5wt%, and phosphorus material may be included in a range of about 0.1wt% to 8wt%.

[0029] Another example embodiment provides a method of manufacturing an aerogel composition for a battery insulating sheet, the method comprising mixing a solvent with a functional material including a binder, a dispersant or a combination thereof and a flame retardant including a phosphorus-based material to manufacture a solvent mixture, and mixing the solvent mixture with an aerogel to manufacture the aerogel composition.

[0030] Another example embodiment provides a battery insulating sheet including a first substrate, a second substrate, and an aerogel layer between the first substrate and the second substrate, wherein the aerogel layer is formed using an aerogel composition or includes the aerogel composition.

[0031] A further example embodiment provides a battery module including a plurality of battery cells and a battery insulation sheet between the plurality of battery cells, wherein a first substrate and a second substrate face adjacent battery cells, respectively. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The attached drawings incorporated in this specification illustrate example embodiments and are used to further illustrate the technical concept of the present disclosure in conjunction with the detailed description of the following example embodiments, and the present disclosure is not to be construed as being limited to the contents shown in these drawings. In the drawings:

[0033] Figure 1 is a schematic diagram showing the structure of a battery insulation sheet according to an example embodiment; and

[0034] Figure 2 To illustrate a structure formed between a plurality of battery cells according to an example embodiment Figure 1 Schematic diagram of a battery insulation sheet. DETAILED DESCRIPTION

[0035] Hereinafter, example embodiments will be described in detail so that those skilled in the art can easily implement the example embodiments. However, example embodiments may be implemented in many different forms and are not limited to the example embodiments described herein.

[0036] When the term "about" or "substantially" is used in conjunction with a numerical value in this specification, it is expected that the relevant numerical value includes a tolerance of ±10% around the stated numerical value. Moreover, when percentages are mentioned in this specification, it is expected that those percentages are based on concentration or weight, for example, concentration percentage or weight percentage. When a range is indicated, the range includes all values ​​in increments therebetween, such as 0.1%.

[0037] Insulation materials, which are materials that hinder or block the flow of heat from a higher temperature to a lower temperature, are used not only in refrigerators and buildings (such as cold storage), but also in a variety of other industries, including the aviation, electronics and automotive industries.

[0038] Insulating materials desirably and advantageously have significant thermal insulating properties through low thermal conductivity, as well as mechanical strength to maintain the thermal insulating properties over time.

[0039] Aerogel, which is a transparent or translucent advanced material with a nanoporous structure, exhibits significantly low density and low thermal conductivity, and so aerogel is highly desired as an insulating material and is considered to be a highly efficient super insulating material that can be used in various industrial applications.

[0040] Significant advantages of aerogels are that aerogels have lower thermal conductivity than conventional organic insulating materials such as, for example, Styrofoam, and aerogels can solve or overcome key weaknesses of organic insulating materials such as, for example, easy ignition and generation of harmful gases when ignited.

[0041] An aerogel composition for a battery insulating sheet according to example embodiments may include: an aerogel; a functional material including a binder, a dispersant, or a combination thereof; a flame retardant including a phosphorus-based material; and a solvent.

[0042] A battery insulation sheet manufactured using an aerogel composition including the above components may have desirable, advantageous or improved thermal insulation performance and fire resistance, and may reduce, hinder or inhibit the propagation of heat and flame occurring in a battery cell to adjacent battery cells due to thermal runaway of the battery cell.

[0043] In an example embodiment, the aerogel may have a diameter of about 500 m 2 / g~1,000m 2 The BET specific surface area of ​​the aerogel can be in the range of about 500 m / g. 2 / g~950m 2 / g, 550m 2 / g~950m 2 / g or 600m 2 / g~900m 2Because the aerogel having a BET specific surface area within any of the above ranges is included, a battery insulating sheet capable of effectively reducing, hindering or preventing heat migration and heat propagation between a plurality of battery cells can be provided.

[0044] The average particle size D50 of the aerogel may be in the range of about 5 to 200 μm, 10 to 100 μm, or 20 to 50 μm. By including the aerogel having the average particle size D50 in any of the above ranges, thermal insulation performance may be improved, thereby delaying thermal migration between a plurality of battery cells.

[0045] The average particle size D50 can be measured, for example, using laser diffraction or scanning electron microscopy (SEM), where the average particle size D50 of the particles can be defined as the particle size at 50% of the particle size distribution (the particle size corresponding to the cumulative 50% volume of the particle size distribution).

[0046] The content of aerogel may be in the range of about 30 wt % to 90 wt %, 55 wt % to 75 wt % or 60 wt % to 70 wt % based on the total amount of solids in the aerogel composition. When the aerogel composition including aerogel in the above range is used to manufacture a battery insulating sheet, the thermal insulation performance of the battery insulating sheet (also referred to as an insulating sheet) may be improved.

[0047] In example embodiments, the binder may include an aqueous polymer binder. For example, the aqueous polymer binder may include at least one of an aqueous polymer, an anionic water-soluble polymer, a cationic water-soluble polymer, and a water-dispersible polymer.

[0048] The waterborne polymer may include, for example, but not limited to, at least one of polyvinyl alcohol, polyethylene oxide, polyacrylamide, and polyvinyl pyrrolidone.

[0049] The anionic water-soluble polymer may include a polymer having at least one of a carboxylic acid group, a sulfonic acid group, a sulfate group, a phosphate group, and a salt thereof. For example, the anionic water-soluble polymer may be a polymer having a carboxylic acid group, and may include, but is not limited to, polymaleic acid as an example.

[0050] The cationic water-soluble polymer may include a polymer having at least one of an amine group, an ammonium group, a phosphonium group, a sulfonium group, and a salt thereof. For example, the cationic water-soluble polymer may be a polymer having an amine group, and may include, but is not limited to, at least one of polyvinylamine and polyamine as an example.

[0051] The water-dispersible polymer may include, but is not limited to, at least one of a water-dispersible polyurethane and a water-dispersible polyester.

[0052] The binder may include an aqueous polymer and a water-dispersible polymer. For example, the binder may include an aqueous polymer having a binder property and a dispersible property and a water-dispersible polyurethane having a fire-resistant property. As an example, the binder may include polyvinyl alcohol and a water-dispersible polyurethane.

[0053] The weight ratio of the aqueous polymer to the water-dispersible polymer may be in the range of about 1:1 to 1:5, 1:1 to 1:4, or 1:2 to 1:3. When the weight ratio of the aqueous polymer to the water-dispersible polymer is within the above range, in addition to the thermal insulation performance, dust content, and compression characteristics of the insulation sheet, the fire resistance and mechanical properties of the insulation sheet may be further improved.

[0054] The content of the binder may be in the range of about 5 wt% to 55 wt%, 20 wt% to 40 wt% or 25 wt% to 35 wt% based on the total amount of solids in the aerogel composition. When the aerogel composition including the binder in the above range is used to manufacture a battery insulating sheet, the durability and dust content of the battery insulating sheet may be improved.

[0055] In example embodiments, the dispersant may include at least one of a surfactant and a phosphate salt. For example, the dispersant may include, but is not limited to, at least one of a nonionic surfactant, an anionic surfactant, an amphoteric surfactant, a natural surfactant (such as lecithin), and a phosphate ester.

[0056] Further including a dispersant can further improve the dispersion of the aerogel in the aerogel composition, making the aerogel uniformly dispersed and improving thermal insulation performance.

[0057] The content of the dispersant may be in the range of about 0.1 wt% to 6 wt%, 0.1 wt% to 5 wt%, or 0.1 wt% to 3 wt%, based on the total amount of solids in the aerogel composition. When the dispersant is included within the above range, it is possible to manufacture the aerogel composition at a low cost, and to manufacture a battery insulating sheet having favorable thermal insulation performance, durability, and dust content using the aerogel composition.

[0058] In example embodiments, the binder and the dispersant may be included in a weight ratio in the range of about 1:0.001 to 1:0.67, 1:0.001 to 1:0.5, or 1:0.001 to 1:0.3. Mixing the binder and the dispersant in a weight ratio in any of the above ranges may allow aerogel to be more uniformly dispersed in the aerogel composition.

[0059] The functional material may be included in a range of about 5 wt % to 55 wt %, 15 wt % to 50 wt %, or 20 wt % to 40 wt %, based on the total amount of solids in the aerogel composition.

[0060] In example embodiments, the phosphorus-based material may include any material that is a flame retardant and contains phosphorus.

[0061] The phosphorus-based material may include, for example, at least one of a phosphate-based ammonium salt, red phosphorus, and compounds represented by Chemical Formula 1 and Chemical Formula 2 below.

[0062] The phosphate ester ammonium salt may include at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and ammonium polyphosphate. For example, the phosphorus material may include ammonium dihydrogen phosphate. The included phosphate ester ammonium salt may reduce or block the propagation of heat from a battery cell to other battery cells by forming char due to phosphorylation when the ambient temperature rises due to thermal runaway in the battery cell.

[0063] Any commercially available red phosphorus may be used as a flame retardant. For example, red phosphorus is an allotrope of elemental phosphorus, P, and is available as a red-purple amorphous powder.

[0064] Red phosphorus can be microencapsulated in a polymer, such as a phenol formaldehyde resin. When red phosphorus is stored with a catalytic component, microencapsulation can hinder or prevent direct contact between the red phosphorus and external components, thereby extending the storage time. The hydrolysis of microencapsulated red phosphorus into unstable volatile compounds, such as phosphine, can be hindered or prevented.

[0065] [Chemical formula 1]

[0066]

[0067] In the above chemical formula 1, Ar 1 ~Ar 3 Each is independently a substituted or unsubstituted C6-C20 aryl group. 1 ~Ar 3 Each is independently a substituted or unsubstituted C6-C18 aryl group or a C6-C12 aryl group.

[0068] [Chemical formula 2]

[0069]

[0070] In the above chemical formula 2, Ar 4 ~Ar 10 Each is independently a substituted or unsubstituted C6-C20 aryl group. 4 ~Ar 10 Each is independently a substituted or unsubstituted C6-C18 aryl group or a C6-C12 aryl group.

[0071] When the ambient temperature rises, the phosphorus-based materials represented by the above Chemical Formulas 1 and 2 may form polyphosphoric acid, which undergoes esterification and dehydrogenation reactions to form a carbon layer, and the carbon layer thus generated may exhibit a flame retardant effect by hindering or blocking oxygen and latent heat.

[0072] In this disclosure, "aryl" is defined as a monovalent substituent derived from an aromatic hydrocarbon.

[0073] Examples of the aryl group may include phenyl, naphthyl, anthracenyl, phenanthryl, naphthacene, tolyl, biphenyl, terphenyl, fluoranthenyl, fluorenyl, perylenyl, indenyl, azulenyl, heptalenyl, phenaltenyl, and phenanthryl.

[0074] In the above chemical formula 1 and chemical formula 2, Ar 1 ~Ar 10 Each may be unsubstituted or substituted with an alkyl group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a halogen group, a cyano group or a trimethylsilyl group.

[0075] In the present disclosure, the term "C#" where "#" is a positive integer refers to any hydrocarbon having # carbon atoms. Thus, the term "C6" refers to a hydrocarbon compound having 6 carbon atoms, and the term "C20" refers to a hydrocarbon compound having 20 carbon atoms.

[0076] The flame retardant may be included in a range of about 0.01 wt% to 20 wt%, 0.1 wt% to 10 wt%, or 0.25 wt% to 5 wt%, based on the total amount of solids in the aerogel composition. Including the flame retardant in any of the above ranges can improve the fire resistance of the insulation sheet and the thermal insulation performance of the insulation sheet, thereby reducing or preventing heat propagation between battery cells.

[0077] Based on 100 parts by weight of the functional material, the flame retardant may be included in an amount of about 0.1 to 20 parts by weight, 0.5 to 17 parts by weight, or 1 to 10 parts by weight. Controlling the content of the flame retardant relative to the content of the functional material within the above range may allow the insulating sheet to form char that may act as a flame barrier when exposed to a high temperature environment, thereby improving the fire resistance of the insulating sheet and reducing or preventing heat and flames occurring in a battery cell due to thermal runaway of the battery cell from propagating to adjacent battery cells.

[0078] In example embodiments, the solvent may include at least one of a polar solvent and a non-polar solvent.

[0079] The polar solvent may include water, an alcohol solvent, or a combination thereof.

[0080] The water can include, for example, purified water, deionized water, or a combination thereof.

[0081] The alcohol solvent may include, for example, but not limited to, at least one of methanol, ethanol, propanol, pentanol, butanol, hexanol, ethylene glycol, propylene glycol, diethylene glycol, and glycerol.

[0082] The non-polar solvent may include a hydrocarbon solvent. For example, the hydrocarbon solvent may include at least one of hexane, pentane, heptane, toluene and benzene, and may be, but is not limited to, an alkane solvent (such as hexane) or a mixture including an alkane solvent.

[0083] The solvent may include water. Using water as a solvent can effectively reduce the cost of raw materials and post-processing costs. However, when water is used as a solvent, water may not mix well with the hydrophobic aerogel. In an example embodiment, the aerogel can be uniformly dispersed by controlling the design of the mixing process, the mixing conditions, the addition of the binder and the dispersant, and the amount of the binder and the dispersant. This uniform dispersion of the aerogel in the aerogel composition can ensure the formation of a thin thickness of a battery insulating sheet with favorable thermal insulation performance, durability and dust content without using a large amount of binder.

[0084] The solvent may be included such that the weight ratio of the solvent to the total amount of solids in the aerogel composition is in the range of about 1:1 to 1:90. For example, the weight ratio of the solvent to the total amount of solids in the aerogel composition may be in the range of about 1:50 to 1:70, 1:20 to 1:30, or 1:2 to 1:10. By controlling the weight ratio of the solvent to the total amount of solids in the aerogel composition within the above range, the viscosity may be controlled to coat the aerogel composition.

[0085] In example embodiments, based on the total amount of solids in the aerogel composition, the aerogel may be included in a range of about 55 wt % to 75 wt %, the binder may be included in a range of about 20 wt % to 40 wt %, and the phosphorus-based material may be included in a range of about 0.1 wt % to 8 wt %.

[0086] As an example, based on the total amount of solids in the aerogel composition, the aerogel may be included in a range of about 60 wt% to 70 wt%, the binder may be included in a range of about 25 wt% to 35 wt%, and the phosphorus material may be included in a range of about 0.25 wt% to 5 wt%. The configuration of the aerogel composition within any of the above ranges may produce desired or advantageous thermal insulation properties and improved fire resistance, which may reduce, hinder or block heat propagation between battery cells.

[0087] In an example embodiment, based on the total amount of solids in the aerogel composition, the aerogel may be included in a range of about 55 wt% to 75 wt%, the binder may be included in a range of about 20 wt% to 40 wt%, the dispersant may be included in a range of about 0.1 wt% to 5 wt%, and the phosphorus material may be included in a range of about 0.1 wt% to 8 wt%.

[0088] As an example, based on the total amount of solids in the aerogel composition, the aerogel may be included in a range of about 60 wt% to 70 wt%, the binder may be included in a range of about 25 wt% to 35 wt%, the dispersant may be included in a range of about 0.1 wt% to 3 wt%, and the phosphorus material may be included in a range of about 0.25 wt% to 5 wt%. The configuration of the aerogel composition within any of the above ranges can improve the dispersibility of the aerogel, can achieve desired or advantageous thermal insulation properties, and can improve fire resistance, thereby more effectively reducing, hindering or blocking heat propagation between battery cells.

[0089] In example embodiments, the aerogel composition may further include a silane compound. The silane compound may include, for example, at least one of 3-(trimethoxysilyl)propyl methacrylate, methyltriethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, octadecyltrimethoxysilane, ethyltriethoxysilane, and 3-glycidoxypropyltrimethoxysilane. Further including a silane compound may further improve dispersibility.

[0090] In example embodiments, additives may be optionally further included, such as, for example, wetting agents, emulsifiers, extenders, viscosity modifiers, pH modifiers, stabilizers, antioxidants, acid or base capture agents, metal deactivators, defoamers, antistatic agents, tackifiers, adhesion improvers, coupling agents, flame retardants excluding phosphorus materials, impact modifiers, pigments, dyes, colorants, or deodorants.

[0091] A method of manufacturing an aerogel composition according to example embodiments may include mixing a solvent with a functional material including a binder, a dispersant, or a combination thereof and a flame retardant including a phosphorus-based material to manufacture a solvent mixture; and mixing the solvent mixture with an aerogel to manufacture the aerogel composition.

[0092] When the solvent is mixed with the functional material and the flame retardant to produce a solvent mixture, the solvent may be mixed with a binder as the functional material or may be mixed with a binder and a dispersant. The detailed description of the solvent, binder, dispersant and phosphorus-based material may be the same as above.

[0093] When the solvent mixture is mixed with the aerogel to produce the aerogel composition, the aerogel may be added in a powder form, and the detailed description of the aerogel may be similar or the same as above.

[0094] Mixing the solvent with the functional material including the binder, the dispersant or a combination thereof and the flame retardant including the phosphorus material to produce the solvent mixture, and mixing the solvent mixture with the aerogel to produce the aerogel composition can be performed using a mixer. For example, the mixer may include, but is not limited to, a planetary mixer and a Thinky mixer. TM mixer.

[0095] As an example, a planetary mixer can be used to mix the solvent mixture with the aerogel. Using a planetary mixer to mix the solvent mixture with the aerogel can allow the aerogel to be substantially uniformly dispersed in the solvent.

[0096] A planetary mixer may be a device that can be used to mix or stir different substances in order to produce a homogenous mixture. A planetary mixer may include blades that are capable of planetary motion.

[0097] In example embodiments, the planetary mixer may include at least one of one or more planetary blades and one or more high-speed dispersing blades. As an example, the planetary mixer may include at least one planetary blade and at least one high-speed dispersing blade.

[0098] Each of the planetary blades and the high-speed dispersion blades can be continuously rotated around its axis. The rotation speed can be expressed in revolutions per minute (rpm).

[0099] In an example embodiment, the planetary mixer may include a first blade and a second blade having different rotation axes. For example, the first blade may be a low-speed blade, and the second blade may be a high-speed blade. Low speed and high speed refer to the relative rotation speed between the first blade and the second blade. As an example, the first blade may be an open blade, and the second blade may be a Despa TM blade.

[0100] The rotation speed of the first blade may, for example, be in the range of about 10 rpm to 100 rpm, 10 rpm to 60 rpm, or 30 rpm to 70 rpm. The rotation speed of the second blade may, for example, be in the range of about 100 rpm to 2000 rpm, 100 rpm to 1000 rpm, 300 rpm to 1700 rpm, or 500 rpm to 1700 rpm.

[0101] When the functional material and the flame retardant are added to the solvent and mixed with the solvent, the rotation speed of the first blade of the mixer may be in the range of about 10 rpm to 60 rpm, 20 rpm to 50 rpm, or 30 rpm to 40 rpm, and the rotation speed of the second blade may be in the range of about 300 rpm to 1700 rpm, 600 rpm to 1000 rpm, or 700 rpm to 800 rpm. As described above, when the solvent is mixed with the functional material and the flame retardant, a solvent mixture in which the binder, the dispersant, or a combination thereof and the flame retardant are substantially uniformly dispersed can be produced to facilitate mixing of the aerogel in a subsequent process.

[0102] When the solvent mixture and the aerogel are mixed with each other, the rotation speed of the first blade of the mixer may be in the range of about 30 rpm to 70 rpm, 40 rpm to 70 rpm, or 60 rpm to 70 rpm, and the rotation speed of the second blade may be in the range of about 500 rpm to 1700 rpm, 600 rpm to 1600 rpm, or 800 rpm to 1500 rpm. As described above, when the aerogel is added to the solvent mixture and mixed with the solvent mixture, the aerogel can be hindered or prevented from aggregating together, so that it is substantially uniformly dispersed.

[0103] A battery insulation sheet according to example embodiments may include a first substrate, a second substrate, and an aerogel layer formed between the first substrate and the second substrate, wherein the aerogel layer may use the above-described aerogel composition form.

[0104] Figure 1 is a schematic diagram illustrating a structure of a battery insulation sheet according to an example embodiment.

[0105] refer to Figure 1 In an example embodiment, the battery insulating sheet 100 may have a structure including a first substrate 110, an aerogel layer 120 formed or placed on the first substrate 110, and a second substrate 130 formed or placed on the aerogel layer 120. The first substrate 110 and the second substrate 130 may be disposed to face adjacent battery cells, respectively. In this case, the first substrate 110 and the second substrate 130 may be made of or include the same material or different materials.

[0106] Since the aerogel layer 120 including the aerogel composition according to the example embodiment is formed between the first substrate 110 and the second substrate 130, the thermal insulation performance and durability of the battery insulation sheet 100 may be improved, and the battery insulation sheet 100 may have favorable fire resistance, thereby possibly reducing or blocking heat propagation between battery cells.

[0107] In the battery insulating sheet 100 , the detailed description of the aerogel composition constituting the aerogel layer 120 may be the same as described above.

[0108] A substrate of various materials such as, but not limited to, resin, metal, inorganic material other than metal, or a composite thereof may be used as each of the first substrate 110 and the second substrate 130. The substrate may be in the form of, but not limited to, a film, a membrane, a sheet, or the like.

[0109] The resin may include, for example, at least one of polyethylene, polypropylene, polystyrene, polyethylene terephthalate, and polyamide.

[0110] The metal may include, for example, at least one of copper, nickel, cobalt, iron, chromium, vanadium, palladium, ruthenium, rhodium, molybdenum, tungsten, iridium, silver, gold, and platinum. When a substrate made of or including the above metal is used, the substrate may be subjected to an anti-corrosion treatment or an insulation treatment as required.

[0111] The inorganic material other than the metal may include at least one of calcium carbonate (CaCO 3 ), talc, and mica.

[0112] As an example, each of the first substrate 110 and the second substrate 130 may include an inorganic material other than metal, and as another example, each of the first substrate 110 and the second substrate 130 may include mica. In this case, thermal insulation performance, durability, etc. of the insulating sheet may be improved.

[0113] In example embodiments, the aerogel layer 120 may be formed to have a single layer structure or a multi-layer structure. When the aerogel layer 120 is formed to have a multi-layer structure, the aerogel layer 120 may be formed to have approximately 2 to 10 layers, 2 to 7 layers, or 2 to 5 layers.

[0114] A method of manufacturing a battery insulating sheet according to example embodiments may include applying an aerogel composition to a first substrate, laminating a second substrate on the applied aerogel composition to form a laminate, pressing the laminate, and drying the laminate.

[0115] In the method of manufacturing the battery insulating sheet, the detailed descriptions of the first substrate and the second substrate may be the same as described above.

[0116] When applying the aerogel composition to the first substrate, the aerogel composition may be directly applied to the first substrate.

[0117] Applying the aerogel composition to the first substrate may be performed using the method of applying a slurry to a normal substrate.

[0118] Applying the aerogel composition to the first substrate may be performed once or repeated two or more times.

[0119] In example embodiments, the aerogel composition may be applied to a first substrate, and the second substrate may be laminated to the applied aerogel composition, thereby forming a structure in which the first substrate, the aerogel layer, and the second substrate are laminated, for example, sequentially laminated.

[0120] In example embodiments, the laminate may be pressed using a conventional pressing method.

[0121] In example embodiments, when drying the laminate, the drying may be performed at a temperature in the range of, for example, about 25° C. to 100° C., 45° C. to 90° C., or 60° C. to 85° C. When drying is performed under the above temperature conditions, a solid aerogel layer may be formed on the substrate without a separate adhesive member or adhesive, while hindering or preventing the substrate and the aerogel layer from peeling off.

[0122] In example embodiments, pressing the laminate and drying the laminate may be performed as separate processes or may be performed simultaneously or concurrently.

[0123] A battery module according to example embodiments may include a plurality of battery cells and a battery insulation sheet disposed between the plurality of battery cells, wherein the first substrate and the second substrate may face adjacent battery cells, respectively.

[0124] Figure 2 To illustrate a structure formed between a plurality of battery cells according to an example embodiment Figure 1 Schematic diagram of a battery insulation sheet.

[0125] refer to Figure 2 , the battery insulating sheet 100 according to the example embodiment may be formed between a plurality of battery cells 200 included in a battery module. The battery insulating sheet 100 may have a structure including a first substrate 110, an aerogel layer 120 formed or placed on the first substrate 110, and a second substrate 130 formed or placed on the aerogel layer 120. One surface of the battery insulating sheet 100 on which the first substrate 110 is formed and another surface of the battery insulating sheet 100 on which the second substrate 130 is formed may be disposed to face adjacent battery cells 200, respectively. When the battery insulating sheet 100 according to the example embodiment is formed between a plurality of battery cells 200, a battery module and a battery pack including the battery module may be provided, which is capable of obstructing or blocking a flame in one battery cell in advance, thereby significantly suppressing the propagation of the flame to another battery cell with a higher safety level.

[0126] Hereinafter, embodiments will be described. However, the following embodiments are only used to illustrate or describe the present disclosure and should not be construed as limiting the present disclosure. Those skilled in the art can fully infer technically that the contents not described herein will therefore be omitted.

[0127] (Manufacture of battery insulation sheets)

[0128] Example 1

[0129] 1. Manufacture of aerogel compositions

[0130] The mixture was prepared by adding polyvinyl alcohol (Sigma Aldrich) as a binder and ammonium dihydrogen phosphate (Sigma Aldrich, 7722-76-1) as a phosphorus material to deionized water as a solvent and stirring at 30 rpm using an open blade and Despa TM The blades were mixed at 700 rpm to produce a solvent mixture. 2 / g of aerogel was added to the solvent mixture and the mixture was stirred at 70 rpm using an open blade and Despa TM The blade was mixed at 1500 rpm to produce the aerogel composition. A planetary mixer (DNTEK, PT-005) was used for mixing.

[0131] The solid content of the manufactured aerogel composition was found to be 69.75 wt% aerogel, 30 wt% polyvinyl alcohol and 0.25 wt% diammonium phosphate.

[0132] 2. Manufacturing of battery insulation sheets

[0133] The slurry of the aerogel composition was applied to a 0.1 mm thick mica sheet (Famica TM , Muscovite TM ), another 0.1 mm thick mica sheet was laminated thereon in a sandwich manner, and coated using a roll-rolling method. Subsequently, an aerogel layer was formed by drying at 60° C. for 24 hours to manufacture a battery insulating sheet. It was found that the total thickness of the manufactured battery insulating sheet was 1.38 mm.

[0134] Example 2

[0135] A battery insulating sheet was manufactured using substantially the same method as in Example 1, except that the input of raw materials was adjusted to manufacture an aerogel composition having a solid content of 69.5 wt % aerogel, 30 wt % polyvinyl alcohol, and 0.5 wt % diammonium phosphate.

[0136] Example 3

[0137] A battery insulating sheet was manufactured using substantially the same method as in Example 1, except that the input of raw materials was adjusted to manufacture an aerogel composition having a solid content of 67.5 wt % aerogel, 30 wt % polyvinyl alcohol, and 2.5 wt % diammonium phosphate.

[0138] Example 4

[0139] A battery insulating sheet was manufactured using substantially the same method as in Example 1, except that the input of raw materials was adjusted to manufacture an aerogel composition having a solid content of 65 wt % aerogel, 30 wt % polyvinyl alcohol, and 5 wt % diammonium phosphate.

[0140] Example 5

[0141] A battery insulating sheet was manufactured using substantially the same method as in Example 1, except that the input of raw materials was adjusted to manufacture an aerogel composition having a solid content of 69.95 wt % aerogel, 30 wt % polyvinyl alcohol, and 0.05 wt % diammonium phosphate.

[0142] Example 6

[0143] A battery insulating sheet was manufactured using substantially the same method as in Example 1, except that the input of raw materials was adjusted to manufacture an aerogel composition having a solid content of 60 wt % aerogel, 30 wt % polyvinyl alcohol, and 10 wt % diammonium phosphate.

[0144] Example 7

[0145] A battery insulating sheet was manufactured using substantially the same method as in Example 1, except that diammonium hydrogen phosphate was added instead of diammonium dihydrogen phosphate as the phosphorus-based material.

[0146] Example 8

[0147] A battery insulating sheet was manufactured using substantially the same method as in Example 1, except that triphenyl phosphate was added instead of diammonium dihydrogen phosphate as the phosphorus-based material.

[0148] Example 9

[0149] 1. Manufacture of aerogel compositions

[0150] Polyvinyl alcohol (Sigma Aldrich) as a binder, a surfactant (Triton-X100, Sigma Aldrich) as a dispersant, and ammonium dihydrogen phosphate (Sigma Aldrich, 7722-76-1) as a phosphorus material were added to deionized water as a solvent, and the mixture was stirred at 30 rpm using an open blade and Despa TM The blades were mixed at 700 rpm to produce a solvent mixture. 2 / g of aerogel was added to the solvent mixture and the mixture was stirred at 70 rpm using an open blade and Despa TM The blade was mixed at 1500 rpm to produce the aerogel composition. A planetary mixer (DNTEK, PT-005) was used for mixing.

[0151] The solid content of the manufactured aerogel composition was found to be 69.75 wt% aerogel, 29.5 wt% polyvinyl alcohol, 0.5 wt% dispersant and 0.25 wt% diammonium phosphate.

[0152] 2. Manufacturing of battery insulation sheets

[0153] The slurry of the aerogel composition was applied to a 0.1 mm thick mica sheet (Famica TM , Muscovite TM ), another 0.1 mm thick mica sheet was laminated thereon in a sandwich manner, and coated using a roll-rolling method. Subsequently, an aerogel layer was formed by drying at 60° C. for 24 hours to manufacture a battery insulating sheet. It was found that the total thickness of the manufactured battery insulating sheet was 1.38 mm.

[0154] Comparative Example 1

[0155] A battery insulating sheet was manufactured using substantially the same method as in Example 1, except that the input of raw materials was adjusted to manufacture an aerogel composition having a solid content of 70 wt % aerogel and 30 wt % polyvinyl alcohol.

[0156] (Experimental Example)

[0157] Experimental Example 1: Evaluation of thermal insulation performance

[0158] The thermal insulation performance of each of the insulating sheets produced in Examples 1 to 9 and Comparative Example 1 was evaluated.

[0159] Each insulating sheet was placed between a pair of opposing 1 mm thick aluminum plates and placed on a hot press. The upper plate of the hot press was heated to 350°C, and the lower plate of the hot press was not heated and maintained at a starting temperature of 40°C. Subsequently, a pressure of 20 kN was applied to the lower plate of the hot press, and the lower plate temperature of the hot press was measured at 11 minutes. The results are shown in Table 1 below.

[0160] Experimental Example 2: Evaluation of fire resistance

[0161] The burning resistance of each of the insulating sheets produced in Examples 1 to 9 and Comparative Example 1 was evaluated.

[0162] Cut the insulation sheet into 5×8cm 2 , a gas welding torch was used to emit a flame to the insulating sheet at a distance of about 5 cm from the insulating sheet, and the time until the insulating sheet on the opposite side was broken was measured to examine the fire resistance (ie, burn-through resistance).

[0163] [Table 1]

[0164]

[0165] With reference to Table 1 above, it can be seen that Examples 1 to 9 exhibit favorable thermal insulation properties. With reference to Examples 1 to 6, it can be seen that the fire resistance varies depending on the content of the components in the aerogel composition, and it can be seen that when 0.5 to 10 parts by weight of a flame retardant is included based on 100 parts by weight of the functional material, the fire resistance and thermal insulation properties are significant. In Example 5, it can be seen that the fire resistance is slightly reduced due to the low content of the flame retardant including the phosphorus material. In Example 6, it can be seen that the thermal insulation performance is slightly reduced due to the high content of the flame retardant including the phosphorus material. In Examples 1, 7, and 8, it can be seen that the physical properties (i.e., thermal insulation performance and fire resistance) vary depending on the type of flame retardant, and it can be seen that when a flame retardant including a phosphorus material is used, the thermal insulation performance and fire resistance are improved. In Example 9, it can be seen that when a binder and a dispersant are mixed, thermal insulation performance and fire resistance are improved.

[0166] In Comparative Example 1, it can be seen that since the flame retardant including the phosphorus-based material is not included, the fire resistance is greatly reduced.

[0167] Therefore, it can be seen that when the aerogel composition according to example embodiments is used, thermal insulation performance and characteristics of hindering or blocking heat propagation are advantageous.

[0168] As apparent from the above description, the battery insulating sheet according to the example embodiment may have thermal insulation performance and fire resistance. A battery module including the battery insulating sheet according to the example embodiment may reduce or inhibit the propagation of heat and flames started in a battery cell due to thermal runaway of the battery cell to adjacent battery cells.

[0169] Although example embodiments are described above, the present disclosure is not limited thereto, and it is contemplated that various modifications may be made within the scope of the claims, detailed description of example embodiments, and the accompanying drawings that also fall within the scope of the present disclosure.

Claims

1. An aerogel composition for a battery insulating sheet, the aerogel composition comprising: Aerogel; Functional materials including binders, dispersants, or combinations thereof; Flame retardants including phosphorus-based materials; as well as Solvent.

2. The aerogel composition according to claim 1, wherein the aerogel has a 2 / g~1,000m 2 / g in the range of BET specific surface area. 3 . The aerogel composition according to claim 1 , wherein the aerogel is included in an amount ranging from 30 wt % to 90 wt % based on the total amount of solids in the aerogel composition.

4. The aerogel composition of claim 1, wherein the binder comprises a water-based polymer binder. 5 . The aerogel composition according to claim 1 , wherein the dispersant comprises at least one of a surfactant and a phosphate ester salt. 6 . The aerogel composition according to claim 1 , wherein the functional material is included in an amount ranging from 5 wt % to 55 wt % based on the total amount of solids in the aerogel composition.

7. The aerogel composition according to claim 1, wherein the phosphorus-based material comprises at least one of a phosphate-based ammonium salt, red phosphorus, and a compound represented by the following Chemical Formula 1 and Chemical Formula 2, Chemical formula 1 In the above chemical formula 1, Ar 1 ~Ar 3 are each independently a substituted or unsubstituted C6-C20 aryl group, and Chemical formula 2 In the above chemical formula 2, Ar 4 ~Ar 10 Each is independently a substituted or unsubstituted C6-C20 aryl group.

8. The aerogel composition according to claim 7, wherein the phosphate-based ammonium salt comprises at least one of diammonium phosphate, diammonium hydrogen phosphate and ammonium polyphosphate. 9 . The aerogel composition according to claim 1 , wherein the flame retardant is included in an amount ranging from 0.01 wt % to 20 wt % based on the total amount of solids in the aerogel composition. 10 . The aerogel composition according to claim 1 , wherein the flame retardant is included in an amount ranging from 0.1 parts by weight to 20 parts by weight based on 100 parts by weight of the functional material. 11 . The aerogel composition according to claim 1 , wherein a weight ratio of the solvent to the total amount of solids in the aerogel composition is in the range of 1:1 to 1:

90.

12. The aerogel composition according to claim 1, wherein the aerogel is included in a range of 55 wt% to 75 wt%, the binder is included in a range of 20 wt% to 40 wt%, and the phosphorus material is included in a range of 0.1 wt% to 8 wt%, based on the total amount of solids in the aerogel composition.

13. The aerogel composition according to claim 1, wherein the aerogel is included in a range of 55 wt% to 75 wt%, the binder is included in a range of 20 wt% to 40 wt%, the dispersant is included in a range of 0.1 wt% to 5 wt%, and the phosphorus material is included in a range of 0.1 wt% to 8 wt%, based on the total amount of solids in the aerogel composition.

14. A method for producing an aerogel composition for a battery insulating sheet, the method comprising: mixing a solvent with a functional material including a binder, a dispersant, or a combination thereof and a flame retardant including a phosphorus-based material to produce a solvent mixture; as well as The solvent mixture is mixed with an aerogel to produce an aerogel composition.

15. A battery insulating sheet, comprising: a first substrate; a second substrate; as well as an aerogel layer between the first substrate and the second substrate, wherein The aerogel layer is formed using the aerogel composition according to any one of claims 1 to 13, or the aerogel layer includes the aerogel composition according to any one of claims 1 to 13.

16. A battery module, comprising: Multiple battery cells; as well as The battery insulating sheet according to claim 15 is provided between the plurality of battery cells, wherein The first substrate and the second substrate face adjacent battery cells, respectively.