Magnetron sputtering equipment for preparing gradient medium gray scale mirror, gradient medium gray scale mirror and preparation method and application of gradient medium gray scale mirror

By using adjustable baffle components in magnetron sputtering equipment to affect the movement of target particles, the problem of insufficient density and scratch resistance of GND Filter film layer is solved, and efficient optical gradient and film layer uniformity are achieved, which extends the lengthening of the film layer. Product lifespan.

CN118910569APending Publication Date: 2024-11-08SUZHOU WUFANG PHOTOELECTRIC MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411010516.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing GND Filter film layer is not dense enough, has low surface hardness, is not scratch-resistant, and has relatively low adhesion, resulting in a short life, and is difficult to sputtering process, and the movement trajectory of the target particles is difficult to control, resulting in a film layer. Uneven thickness affects product use.

Method used

Design a magnetron sputtering equipment. By setting up a baffle assembly in a vacuum chamber, using electric field and magnetic force to affect the movement of target particles, forming a gradient optical spectrum curve, and realizing the optical gradient requirements of the grayscale mirror in the gradient. The baffle material is Aluminum, aluminum alloy, stainless steel, hollow parts can be adjusted to achieve hard gradient or soft gradient, and the baffle position is automatically or manually adjusted by the driving mechanism to optimize film deposition.

Benefits of technology

The optical gradient effect of GND Filter is realized, which improves the density, adhesion and friction resistance of the film layer, extends the product life, and solves the problems of uneven film layer thickness and difficulty in controlling the motion trajectory.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910569A_ABST
    Figure CN118910569A_ABST
Patent Text Reader

Abstract

The magnetron sputtering equipment comprises a vacuum chamber, a target material assembly, a vacuum chamber door and a bearing part located in the vacuum chamber, the bearing part is used for bearing a substrate, and the substrate and the target material assembly are oppositely arranged; a baffle plate assembly for forming a gradual change area of the gradual change medium gray scale mirror is arranged between the substrate and the target material assembly, and the baffle plate assembly comprises a baffle plate and a fixing mechanism for fixing the baffle plate. According to the magnetron sputtering equipment for preparing the gradual change medium gray scale mirror, the baffle is additionally arranged, the position, not needing to be plated with an attenuation film, on the substrate is shielded, and the requirement for optical gradual change of the gradual change medium gray scale mirror is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of gradient medium gray mirror and PVD coating, and in particular to a magnetron sputtering device for preparing gradient medium gray mirror, a method for coating a GND filter (gradient medium gray mirror) based on a magnetron sputtering coating process, and a GND filter prepared by the method and its application in an imaging module or an imaging product such as a camera. Background Art

[0002] Since the advent of the camera, humans have tried to replicate the prosperous and beautiful world seen by the naked eye. However, there are still great differences between the camera imaging and the scene seen by the human eye, whether in terms of color, light brightness, contrast, etc.; so that even the most tolerant camera cannot produce the same imaging effect as the human eye, and therefore cannot perfectly record the ever-changing nature. However, people are still working hard to develop various technical solutions to solve these problems. For example, in response to the situation where overexposure is easy to occur when shooting under sunlight, people have developed the GND Filter (Graduated Neutral Density Filter) solution to make the picture clearer.

[0003] GND Filter is one of the most important filters in photography. The human eye can capture a wide range of brightness and shadows. This is often referred to as "dynamic range", but current camera sensor technology is not yet able to reach the dynamic range of the human eye. Therefore, using a gradient neutral density filter can capture the maximum dynamic range of the scene in a single exposure, without the need for multiple exposures with different shutter speeds.

[0004] For example, when people enjoy the beautiful sunrise or sunset with their eyes, they can see all the details of the sky and land in the scene. However, once they try to freeze such a beautiful moment with a camera, the photo they take will become a picture of overexposed sky or underexposed foreground. At this time, you can choose a suitable GND Filter to solve the problem of light ratio balance.

[0005] GND Filter is mainly divided into the following categories:

[0006] 1. Hard gradient: Its characteristic is that there is a clear boundary between the transparent and dark areas, so hard gradient is generally used in situations where the transition between light and dark areas of the picture is very obvious, such as shooting the sea level.

[0007] 2. Soft gradient: Its characteristic is a smoother transition (the gradient area is smoother), so soft gradient is applicable in more situations and can be used in scenes where the transition between light and dark is not so obvious, such as shooting in mountainous areas.

[0008] 3. Reverse gradient: From the calendering area in the middle of the filter, there is a process of slowly fading from grayscale upwards or downwards (the darkest part of the reverse gradient is in the middle), so the reverse gradient is generally used at sunset or sunrise.

[0009] At present, the GND Filter on the market is basically made by evaporation coating process, and its film layer is not dense enough, the surface hardness is low, it is not scratch-resistant, the film layer adhesion is relatively low, and the life is short. Researchers also tried to use sputtering process for coating, but it is more difficult, mainly reflected in the following aspects:

[0010] 1. According to the characteristics of magnetron sputtering, the particles sputtered from the target material move in a directional manner under the influence of the electric field and the magnetic field. The moving distance is short, and it becomes very difficult to change its moving trajectory.

[0011] 2. Compared with evaporation equipment, the distance between the target material and the substrate loading position of the sputtering equipment is closer, which limits the feasibility of most modifications.

[0012] 3. Compared with evaporation equipment, when sputtering equipment is depositing thin films, if there is a mask blocking it, sputtered particles will accumulate at the boundary where the mask and the substrate contact (uneven film thickness). At this time, the eyes will see a glare light, affecting the use of the product.

[0013] In order to solve these problems, there are also related research reports. For example, patent CN 110221372 A, two-in-one gradient mirror and its preparation method, discloses the use of evaporation equipment to coat the attenuation film, without coating the anti-reflection film (losing transmittance to enhance the friction resistance). Another example is patent CN 117665997 A, neutral grayscale mirror and its production method, which discloses the production of neutral grayscale mirrors, and its products do not have a gradient function. These solutions are all products plated with evaporation equipment. However, these methods either do not coat the anti-reflection film (losing light transmittance) to avoid scratches on the film layer (the coated part of the attenuation film is still not friction-resistant), or do not have a gradient function, and cannot solve the defects of physical properties such as film density, film adhesion, friction resistance, and short life.

[0014] The disclosure of the above background technology content is only used to assist in understanding the inventive concept and technical solution of the present invention. It does not necessarily belong to the prior art of this patent application. In the absence of clear evidence that the above content has been disclosed before the filing date of this patent application, the above background technology should not be used to evaluate the novelty and creativity of the present application. Summary of the invention

[0015] In view of this, in order to overcome the defects of the prior art, an object of the present invention is to provide a magnetron sputtering device for preparing a gradient medium grayscale mirror, a gradient medium grayscale mirror, and a preparation method and application thereof.

[0016] In order to achieve the above object, the present invention adopts the following technical solutions:

[0017] A magnetron sputtering device for preparing a gradient medium grayscale mirror comprises a vacuum chamber, a target assembly, a vacuum chamber door and a bearing part located in the vacuum chamber, wherein the bearing part is used to bear a substrate, the substrate and the target assembly are arranged opposite to each other, and a baffle assembly for forming a gradient region of the gradient medium grayscale mirror is provided between the substrate and the target assembly, wherein the baffle assembly comprises a baffle and a fixing mechanism for fixing the baffle. The baffle can be a single plate or a plurality of plates can be stacked to realize the corresponding function.

[0018] The target particles sputtered by magnetron are affected by the electric field and the Lorentz magnetic force, and are directed and quickly shot toward the substrate. When passing through the baffle, diffraction will occur at the edge of the baffle. By changing the edge shape of the baffle and the distance from the substrate, the number of particles reaching the substrate is reasonably changed, thereby forming a gradual and smooth optical spectrum curve. That is, in this application, the baffle is used to block the position on the substrate where the attenuation film does not need to be plated, so as to achieve the optical gradient requirement of the gradient medium grayscale mirror.

[0019] According to some preferred implementation aspects of the present invention, the baffle is made of aluminum, aluminum alloy, stainless steel, etc., and has a thickness of 0.1 to 3 mm.

[0020] According to some preferred embodiments of the present invention, the baffle is provided with a flat portion for forming a hard gradient and / or a hollow portion for forming a soft gradient, the hollow portion runs through the thickness direction of the baffle, and the hollow portion is located in the middle or at the edge of the baffle in the width direction.

[0021] According to some preferred implementation aspects of the present invention, the hollow portion includes a plurality of hollow units, each of which is a combination of one or more of a circular, continuous or discontinuous V-shaped, and an arc. The hollow portion is circular, sawtooth-shaped, or wavy. When the hollow unit is V-shaped, the angle of the sharp corner on the baffle is preferably 30°.

[0022] According to some preferred embodiments of the present invention, the baffle is fixed to the end of the fixing mechanism; and a through hole is provided on the baffle for the fixing mechanism to pass through. In some embodiments, the fixing mechanism includes a threaded rod or a screw, one end of which is connected to the target chamber, and the other end is connected to the baffle, and the position of the baffle can be adjusted by the installation position of the threaded rod or the screw, and the rotation of the threaded rod or the screw. This structure is suitable for manual installation of the baffle, and is suitable for magnetron sputtering equipment that does not have additional space in the target chamber for accommodating the baffle.

[0023] According to some preferred embodiments of the present invention, the baffle assembly includes a driving mechanism for driving the fixing mechanism to move. In some embodiments, the driving mechanism is used to drive the baffle to move in the horizontal direction (X and / or Y direction) and the vertical direction (Z direction), which is suitable for automatic adjustment of the baffle and for magnetron sputtering equipment with additional space for accommodating the baffle and the driving mechanism in the target chamber.

[0024] Specifically, the driving mechanism can be a conventional screw assembly structure: the driver (corresponding to one direction) or the baffle is fixed on the threaded block, the threaded block cooperates with the screw, and the driver (corresponding to the other direction) drives the screw to rotate, and through several groups of screws and drivers, the baffle can be moved in two or three dimensions in the target chamber to adjust the position of the baffle.

[0025] Preferably, when the gradient of the gradient grayscale mirror is a hard gradient, the distance between the baffle and the substrate is 0.

[0026] According to some preferred embodiments of the present invention, the baffle includes a plate portion and a rod portion, the plate portion is arranged on the rod portion, the length of the rod portion is greater than the plate portion, the through hole is opened on the rod portion, and the hollow portion is arranged on the plate portion.

[0027] According to some preferred implementation aspects of the present invention, a correction component for correcting the uniformity of multiple film layers is included, and the correction component is disposed between the substrate and the target assembly.

[0028] According to some preferred implementation aspects of the present invention, the baffle is disposed between the substrate and the correction component.

[0029] According to some preferred implementation aspects of the present invention, a target chamber is provided on the side of the vacuum chamber, the target assembly and the baffle assembly are arranged in the target chamber, and a protective door is provided between the target chamber and the vacuum chamber.

[0030] According to some preferred implementation aspects of the present invention, the length of the baffle is less than or equal to the width between the inner walls of the target chamber; and / or the length of the hollow portion is less than or equal to the length of the baffle.

[0031] The present invention also provides a method for preparing a gradient medium grayscale mirror, comprising the following steps:

[0032] Determining the gradient region and optical film design of the gradient medium grayscale mirror;

[0033] The structure of the baffle is designed according to the gradient range; the baffle is used to form a gradient area of ​​the gradient medium grayscale mirror;

[0034] Anti-reflection film coating is carried out according to the designed optical film;

[0035] The baffle is arranged between the target assembly and the substrate;

[0036] The attenuation film system is plated according to the designed optical film to obtain the gradient neutral grayscale mirror. That is, after the anti-reflection film is plated, the baffle is moved to a suitable position to shield a specific area when the attenuation film is plated to form a gradient area.

[0037] According to some preferred implementation aspects of the present invention, the parameters of the baffle structure design include the shape of the hollow unit and the distance between the baffle and the substrate, and the shape of the hollow unit includes the opening size and depth.

[0038] According to some preferred implementation aspects of the present invention, when the gradient area of ​​the gradient medium grayscale mirror becomes narrower, the opening size of the hollow unit increases and the depth becomes smaller, and the distance between the baffle and the substrate becomes smaller.

[0039] According to some preferred implementation aspects of the present invention, when the gradient of the gradient medium grayscale mirror is a hard gradient, the distance between the baffle and the substrate is 0.

[0040] According to some preferred implementation aspects of the present invention, the step further includes: testing the obtained gradient medium grayscale mirror, and adjusting the structure of the baffle according to the test result; until the parameters of the obtained gradient medium grayscale mirror meet the requirements.

[0041] According to some preferred implementation aspects of the present invention, when designing the optical film, an anti-reflection film system is designed first, and then an attenuation film system is designed based on the anti-reflection film system.

[0042] The present invention also provides a gradient neutral grayscale mirror prepared by the preparation method as described above and application of the gradient neutral grayscale mirror in an imaging module.

[0043] Due to the adoption of the above technical scheme, compared with the prior art, the benefit of the present invention lies in that the magnetron sputtering equipment for preparing a gradient medium grayscale mirror of the present invention, by adding a baffle, blocks the position on the substrate where the attenuation film does not need to be plated, thereby achieving the optical gradient requirement of the gradient medium grayscale mirror. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0045] Figure 1 It is a schematic diagram of the three-dimensional structure of a magnetron sputtering device for preparing a gradient medium grayscale mirror according to a preferred embodiment of the present invention;

[0046] Figure 2 A schematic diagram of the cross-sectional structure of a magnetron sputtering device in a preferred embodiment of the present invention;

[0047] Figure 3 A schematic diagram of the top view of the magnetron sputtering device in a preferred embodiment of the present invention;

[0048] Figure 4 It is a schematic diagram of the three-dimensional structure of the target chamber in a preferred embodiment of the present invention;

[0049] Figure 5 It is a structural schematic diagram of the relationship between the target chamber and the bearing part in a preferred embodiment of the present invention;

[0050] Figure 6-Figure 13 is a schematic diagram of a preferred baffle structure in an embodiment; wherein, Figure 7 , 9 , 11 corresponding to the baffle can achieve hard gradient and single soft gradient (one end of high transparency, one end of attenuation of the smooth gradient transition), corresponding to embodiment 2; Figure 8 , 13 It can realize products with attenuation in the middle and high transparency at both ends, and a smooth gradual transition, corresponding to Example 3; Figure 6 , 10 12 can realize a product with high transmittance in the middle and attenuation at both ends, and a smooth gradual transition, corresponding to Example 4;

[0051] Figure 14-17 This is a schematic diagram of the gradient spectrum of the gradient medium grayscale mirror prepared in the preferred embodiment of the present invention (taking the GND8 product as an example);

[0052] Figure 18-Figure 21 This is a schematic diagram of a gradient medium grayscale mirror product prepared in a preferred embodiment of the present invention, in which the black part is the attenuation area, the gray part is the gradient area, and the white part is the anti-reflection area, corresponding to the area blocked by the baffle;

[0053] Among them, the figure markings are: vacuum chamber-1, target chamber-2, baffle-21, hollow part-211, through hole-212, flat part-213, plate part-214, rod part-215, fixing mechanism-22, correction assembly-23, threaded hole-231, target assembly-24, protective door-25, glow discharge area-3, vacuum chamber door-4, bearing part-5. DETAILED DESCRIPTION

[0054] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0055] In view of the shortcomings of the GND Filter (gradient medium grayscale mirror) currently on the market, which is basically made using an evaporation coating process, the present application provides a method for making a GND Filter using a magnetron sputtering coating process. From the perspective of improving the physical properties of the product, the method of influencing the movement trajectory of some magnetron sputtering particles allows the particles to be deposited at specified locations on the substrate, thereby cleverly solving the problem of poor physical properties of the GND Filter.

[0056] The principle is generally as follows: the target particles sputtered by magnetron are affected by the electric field and the Lorentz magnetic force, and are directed rapidly toward the substrate. When passing through the baffle 21, diffraction will occur at the edge of the baffle 21. By changing the edge shape of the baffle 21 and the distance from the substrate, the number of particles reaching the substrate is reasonably changed, thereby forming a gradual and smooth optical spectrum curve. Visually, the smooth transition of light and dark colors can be seen (the smooth transition of transmittance of the same optical wavelength or different optical wavelengths can be achieved). In this application, the baffle 21 is used to block the position on the substrate where the attenuation film does not need to be plated, so as to achieve the optical gradient requirement of the gradient grayscale mirror.

[0057] Based on this principle, the present application provides a magnetron sputtering device for preparing a gradient medium grayscale mirror and a method for preparing a gradient medium grayscale mirror. The structure of the magnetron sputtering device is detailed in Example 1. The method for preparing a gradient medium grayscale mirror based on a magnetron sputtering coating process of the present invention specifically includes the following steps:

[0058] Step 1: Determine the gradient area and optical film design of the gradient medium grayscale mirror according to the product specifications

[0059] When designing optical thin films, the coating order of the functional film system should be considered, that is, the anti-reflection film system should be designed first, and then the attenuation film system or other colored films should be designed based on this. The film layer on the final gradient neutral grayscale mirror has both anti-reflection and attenuation functions.

[0060] Select the film material according to the needs, and use the commercial film design software to design the anti-reflection film system first; based on this, design other functional film systems, such as attenuation film systems, colored film systems, etc. Whether they are plated separately or superimposed together, they can achieve their respective functions. The coating process is also carried out in the same order as the design. This can avoid the abnormal optical and physical properties of the product due to the superposition of spectral design during the coating process.

[0061] Step 2: Design the structure of the baffle 21 according to the gradient range

[0062] The present application adds a special mask, namely the GND Mask (baffle 21), between the target material and the substrate. The baffle 21 is used to form a gradient area of ​​the gradient medium grayscale mirror. The baffle 21 is provided with a flat portion 213 for forming a hard gradient and / or a hollow portion 211 for forming a soft gradient. The hollow portion 211 includes a plurality of hollow units. The parameters of the structural design of the baffle 21 include the shape of the hollow unit and the distance between the baffle 21 and the substrate. The shape of the hollow unit includes the opening size and depth. The baffle 21 can be a single plate or multiple plates can be stacked to achieve corresponding functions and effects.

[0063] Generally speaking, the distance between the baffle 21 and the substrate is 0-20 mm; the opening depth-to-width ratio of the hollow unit is ≥ 1:1. However, due to different coating machine models and different internal spaces of the equipment, the distance and opening size need to be adjusted accordingly.

[0064] According to the different requirements of product gradient, the shape and position of Mask (the distance between the target, baffle 21 and substrate) are changed accordingly. When the gradient of the grayscale mirror is hard gradient, the distance between baffle 21 and substrate is 0. If the gradient range is required to be relatively wide, the hollow unit of baffle 21 will be narrower and longer, that is, the aspect ratio will be increased, and it will be further away from the substrate; if the gradient range is relatively narrow, the opening size of the hollow unit of baffle 21 will be larger and the depth will be shallower, that is, the aspect ratio will be reduced, and it will be closer to the substrate.

[0065] The hollow unit includes a combination of one or more of a circular, continuous or discontinuous V-shaped, and an arc. The hollow portion 211 is circular, serrated, or wavy. When the hollow unit is V-shaped, the angle of the sharp corner on the baffle 21 is preferably 30°. When the product requires a gradual transition from an anti-reflection film to an attenuation film, a baffle 21 with a hollowed edge (such as Figure 7 , 9 , 11); when the product requires a gradual transition from the attenuation film to the anti-reflection film and then to the attenuation film, the middle hollow baffle 21 (such as Figure 8 , 13). According to the product requirements, select the baffle 21 with corresponding structural parameters. For example, if the baffle 21 is hard gradient, it cannot have a notch or irregular edge hollowing part 211, and must be a regular flat edge (flat part 213) (such as Figure 7 , 9 , 11), and the distance between the baffle 21 and the substrate is 0. Products with gradient requirements require masks of different shapes and parameter adjustments, such as Figure 6 to Figure 13 As shown, the requirements of different product specifications can be met by selecting a suitable baffle 21 .

[0066] Preferably, when the hollow portion 211 includes a plurality of hollow units, the size of the hollow units gradually increases along the gradual transition direction from the anti-reflection film to the attenuation film, and it may be more preferred that the hollow units in two adjacent rows are staggered to better control the number of particles reaching the substrate and form a better gradual anti-reflection effect, such as Figure 11-13 As shown, it includes wave-shaped and circular hollow units of various sizes.

[0067] Preferably, the baffle 21 includes a plate portion 214 and a rod portion 215, the plate portion 214 is disposed on the rod portion 215, and the hollow portion 211 is disposed on the plate portion 214. Figure 9-10 As shown, the plate portion 214 includes a plurality of plate units, each of which is fixed to the rod portion 215 by fasteners such as screws, and the ends of the plate units form a hollow portion 211 or a flat portion 213. This structure is more flexible than a single plate structure. For example, when adjusting the gradual position, it is not necessary to replace the baffle 21 of different sizes, but only to adjust the number or shape of the plate units.

[0068] The material of GND Mask is generally hard aluminum, aluminum alloy, stainless steel, etc.; its thickness range is generally 0.1 to 3 mm (selected according to actual product and process parameters).

[0069] Specifically, Figure 7 , 9 , 11, one side of the baffle 21 in the width direction is a flat portion 213, and the other side is a continuous V-shaped hollow portion 211. The baffle 21 with the hollow portion 211 on one side can achieve a soft gradient of a single lens. The product effect diagram is shown in Fig.19 , the spectrum is shown in Fig.15 When a flat side is used and the distance between the baffle 21 and the substrate is 0, a hard gradient can be achieved. The schematic diagram of the product effect is as follows Fig.18 , baffle 21 corresponds to the white (high transmittance) area of ​​the product, and the spectrum is as follows Fig.14 shown.

[0070] Specifically, Figure 6 , 10As shown in 12, both sides of the baffle 21 in the width direction are hollow parts 211 with continuous V-shaped, circular, arc-shaped, etc., which can achieve the function of attenuation of the light transmittance of the product at both ends, high transmittance in the middle, and smooth transition. Fig. 20 , the spectrum is as follows Fig.16 shown.

[0071] Specifically, Figure 8 , 13 As shown, the baffle 21 is hollowed out in the middle, and the hollow edge is a hollow portion 211 with a continuous V-shaped, circular, arc-shaped, etc., which can achieve the functions of anti-reflection at both ends of the product, attenuation in the middle, and smooth transition. Fig.21 , the spectrum is as follows Fig.17 shown.

[0072] Step 3: Anti-reflection coating

[0073] Anti-reflection film system is coated according to the designed optical film.

[0074] Step 4: Set a baffle 21 between the target assembly 24 and the substrate

[0075] The baffle 21 is set between the substrate and the uniformity correction component 23, and is divided into manual setting and automatic setting. The details are as follows:

[0076] The correction component 23 of the target chamber 2 is provided with a plurality of threaded holes 231 in the vertical direction, and the fixing mechanism 22 includes a threaded rod or a screw, one end of which is connected to the threaded hole 231 of the correction component 23 of the target chamber 2, and the other end is connected to the baffle 21. The manual setting is as follows: when the anti-reflection film is coated, the vacuum coating chamber needs to be broken, and the coated substrate is taken out for ultrasonic cleaning. The position of the baffle 21 is adjusted by the installation position of the threaded rod or the screw, and the rotation of the threaded rod or the screw, and then the vacuum system is started and the substrate to be coated is loaded for coating of the attenuation film. The manual setting is suitable for magnetron sputtering equipment in which there is no additional space in the target chamber 2 for accommodating the baffle 21.

[0077] The automatic setting is as follows: a baffle assembly, including a baffle 21, a fixing mechanism 22 and a driving mechanism, is already provided in the target chamber 2 before or while the substrate is placed. When the anti-reflection film is coated, the baffle 21 is located in the extra space of the target chamber 2 and will not affect the coating of the anti-reflection film. When the anti-reflection film is coated, the fixing mechanism 22 and the GND Mask are driven by the driving mechanism to automatically move to the set position to block the position of the substrate where the attenuation film does not need to be coated. At this time, the vacuum coating chamber does not need to break the vacuum, and the attenuation film system part continues to be deposited directly. The automatic adjustment of the baffle 21 is suitable for magnetron sputtering equipment with additional space for accommodating the baffle 21 and the driving mechanism in the target chamber 2.

[0078] The driving mechanism can be a conventional screw assembly structure: the driver (corresponding to one direction) or the baffle 21 (fixing mechanism 22) is fixed on the threaded block, the threaded block cooperates with the screw, and the driver (corresponding to the other direction) drives the screw to rotate, and the baffle 21 is moved in two or three dimensions in the target chamber 2 through several groups of screws and drivers, so as to automatically adjust the position of the baffle 21 after the anti-reflection film is plated. The driver is selected from stepping motors, etc.

[0079] The distance between the mask and the substrate is adjusted appropriately according to product requirements. For example, if a hard gradient is required, the distance between the mask and the substrate is zero; and if a soft gradient is required, the appropriate distance needs to be adjusted to the appropriate distance through a threaded rod or a lead screw according to the gradient range and with a suitable mask.

[0080] The position of the mask is not limited to the middle, upper half, or lower half of the corresponding substrate. The position of the corresponding substrate can be adjusted through the threaded hole 231 according to actual needs. Refer to several products with different relative positions of the mask and the substrate. Take GND8 as an example. The product spectrum is as follows Figure 14 to Figure 17 , product pictures as follows Figure 18-21 GND8 is a product of the gradient medium density grayscale filter (GND filter). GND8 means the transmittance is attenuated from high transmittance to 12.5%, optical 3rd gear, optical density 0.9. Common grades include GND2, GND4, GND8, GND16, and GND32.

[0081] Figure 6 to Figure 13 The structure of the baffle 21 (GND Mask) is shown to gradually reduce the deposition of magnetron sputtering particles on the substrate. According to the requirements of the width of the gradient area, the sawtooth depth and density of the hollow portion 211 of the Mask in the present invention need to match. The selection can be made according to the test data, including but not limited to the width, shape, size of the hollow area, etc. of the Mask.

[0082] Specifically, when considering cost and production efficiency, the carrier 5 can be filled with substrates. At this time, multiple GND Masks need to be set, and corresponding adjustments are made for substrates of different turns, such as the cooperation between single-sided gradient Mask and double-sided gradient Mask. Of course, multiple types of suitable GND Masks can be selected according to needs.

[0083] Step 4: Coat the attenuation film according to the designed optical film to obtain a preliminary gradient medium grayscale mirror

[0084] According to the optical thin film design, the program is imported and run to deposit the target particles onto the substrate to grow the corresponding film layer.

[0085] In the actual plating process, after the substrate is entirely coated with the anti-reflection film system, the baffle 21 is set, and then the attenuation film system or other colored film system is selectively plated, thereby forming a partial attenuation effect and a partial anti-reflection effect of the substrate.

[0086] Step 5: Take out the preliminary gradient neutral grayscale mirror from the vacuum chamber 1 and test it. The product performance test includes optical performance and physical performance. And according to the test results, decide whether to further adjust the structure (size, position, shape, etc.) of the baffle 21 until the parameters of the gradient neutral grayscale mirror meet the requirements.

[0087] The prepared GND Filter achieves hard gradient and soft gradient effects of substrate transmittance, that is, the change of the spectrum between the high transmittance target value and the attenuation target value.

[0088] Example 1 Magnetron sputtering equipment

[0089] like Figure 1-13 As shown, the magnetron sputtering equipment for preparing a gradient medium grayscale mirror in this embodiment includes a vacuum chamber 1, a glow discharge area 3, a target chamber 2, a target assembly 24, a vacuum chamber door 4, a bearing portion 5 (a drum for loading a substrate) located in the vacuum chamber 1, a baffle assembly, and a correction assembly 23. The substrate includes but is not limited to optical glass, quartz, silicon wafers and other materials, and the corresponding material is selected according to the needs. The target includes but is not limited to a flat square target, a flat circular target, a cylindrical target, etc. The sputtering coating machine is not limited to a dual-target model, and a multi-target model can also be applied.

[0090] Among them, the bearing part 5 is used to bear the substrate, and the substrate is arranged opposite to the target assembly 24. The target assembly 24, the baffle assembly, and the correction assembly 23 are all contained in the target chamber 2. The baffle assembly is used to form the gradient area of ​​the gradient medium grayscale mirror, and the correction assembly 23 is used to correct the uniformity of multiple film layers. The film layer includes an anti-reflection film system, an attenuation film system, and preferably includes a colored film, etc. The baffle 21 and the correction assembly 23 of the baffle assembly are both arranged between the substrate and the target assembly 24, and the baffle 21 is arranged between the substrate and the correction assembly 23. The vacuum chamber door 4, the glow discharge area 3, and the target chamber 2 are arranged on the side of the vacuum chamber 1, and the vacuum chamber door 4 is used to take and place the substrate. There is a protective assembly (protective door 25) between the target chamber 2 and the vacuum chamber 1, which is opened when the target is sputtered and closed otherwise.

[0091] The baffle assembly includes a baffle 21 and a fixing mechanism 22 for fixing the baffle 21. When the position of the baffle 21 needs to be automatically adjusted, the baffle assembly also includes a driving mechanism for driving the fixing mechanism 22 to move, so as to realize the movement of the baffle 21. The baffle 21 is made of aluminum, aluminum alloy, stainless steel, etc., with a thickness of 0.1 to 3 mm.

[0092] In this embodiment, the correction component 23 of the target chamber 2 is provided with a plurality of threaded holes 231 in the vertical direction, and the fixing mechanism 22 includes a threaded rod or a screw, one end of which is connected to the threaded hole 231 of the correction component 23 of the target chamber 2, and the other end is connected to the baffle 21, and the position of the baffle 21 can be adjusted by the installation position of the threaded rod or the screw, and the rotation of the threaded rod or the screw. This structure is suitable for manual installation of the baffle 21, and is suitable for magnetron sputtering equipment in which there is no additional space in the target chamber 2 for accommodating the baffle 21.

[0093] In other embodiments, the baffle assembly includes a driving mechanism for driving the fixing mechanism 22 to move, which is used to drive the baffle 21 to move in the horizontal direction (X and / or Y direction) and the vertical direction (Z direction), and is suitable for automatic adjustment of the baffle 21, and is suitable for magnetron sputtering equipment with additional space for accommodating the baffle 21 and the driving mechanism in the target chamber 2.

[0094] Specifically, the driving mechanism can be a conventional screw assembly structure: the driver (corresponding to one direction) or the baffle 21 (fixing mechanism 22) is fixed on the threaded block, the threaded block cooperates with the screw, and the driver (corresponding to the other direction) drives the screw to rotate, and the baffle 21 is moved in two or three dimensions in the target chamber 2 through several groups of screws and drivers, so as to automatically adjust the position of the baffle 21 after the anti-reflection film is plated. The driver is selected from stepping motors and the like.

[0095] For example, when the gradient of the gradient grayscale mirror is hard gradient, the distance between the baffle 21 and the substrate is 0; when the gradient area of ​​the gradient grayscale mirror becomes narrower, the distance between the baffle 21 and the substrate is adjusted to become smaller.

[0096] like Figure 6-13 As shown, the baffle 21 is provided with a flattened portion 213 for forming a hard gradient and / or a hollowed portion 211 for forming a soft gradient, the hollowed portion 211 runs through the thickness direction of the baffle 21, and is located in the middle position or the edge in the width direction of the baffle 21. The hollowed portion 211 includes a plurality of hollowed units, and each hollowed unit is a combination of one or more of a circular, continuous or discontinuous V-shaped, and an arc. If the gradient range is required to be relatively wide, the hollowed units of the baffle 21 will be narrower and longer, that is, the aspect ratio is increased, and it is further away from the substrate; if the gradient range is relatively narrow, the opening size of the hollowed units of the baffle 21 will be larger and the depth will be shallower, that is, the aspect ratio is reduced, and it is closer to the substrate.

[0097] The length of the baffle 21 is less than or equal to the width between the inner walls of the target chamber 2 ; the hollow portion 211 extends along the length direction of the baffle 21 , and the length of the hollow portion 211 is less than or equal to the length of the baffle 21 .

[0098] Preferably, the baffle 21 includes a plate portion 214 and a rod portion 215, the plate portion 214 is arranged on the rod portion 215, the length of the rod portion 215 is greater than the plate portion 214, the through hole 212 is opened on the rod portion 215, and the hollow portion 211 is arranged on the plate portion 214. Figure 9-10 As shown, the plate portion 214 includes a plurality of plate units, each of which is fixed to the rod portion 215 by fasteners such as screws, and the ends of the plate units form a hollow portion 211 or a flat portion 213. This structure is more flexible than a single plate structure. For example, when adjusting the gradual position, it is not necessary to replace the baffle 21 of different sizes, but only to adjust the number or shape of the plate units.

[0099] Example 2

[0100] The method for preparing a gradient neutral grayscale mirror based on a magnetron sputtering coating process in this embodiment specifically includes the following steps:

[0101] Conduct film system design and first coat the clean substrate with an anti-reflection film to test whether the optical performance meets the requirements.

[0102] Then select the appropriate GND Mask according to the gradient width (such as Figure 7 , Fig. 9 , Fig.11 ) and load it into the appropriate location.

[0103] Here, manual installation is used as an example to explain the coating process: select a suitable Mask (baffle 21) according to product requirements, load it onto the screw, and do not affect the uniformity correction component 23 and the protection component. Compare the position of the substrate to be plated on the Drum (5), use a caliper to measure (or laser distance measurement) the distance between the two, and adjust the movement of the Mask in the up, down, front, and back directions until it moves to the appropriate position and then fixes. After completion, close the target hatch. Start the running program, clean the target, load the clean substrate onto the Drum, and fix it to start the coating process of the attenuation film system.

[0104] Start the target cleaning program. After completion, load the good product coated with anti-reflection film, cover the end that does not need to be coated with attenuation film, and run the attenuation film coating program for coating.

[0105] After completion, the product is tested and judged whether it is qualified according to the index requirements.

[0106] If the requirements are not met, such as the gradient width exceeds the specification, reduce the distance between the GND Mask and the substrate and test the coating again. Generally, according to the pre-designed distance, there will not be a big difference, so just fine-tune the distance. If the requirements are still not met after adjusting to the distance limit, choose a GND Mask with a smaller hollow.

[0107] Taking the GND8 product as an example, the side of the baffle 21 with the hollow portion 211 can realize the soft gradient of a single lens. See the schematic diagram of the product effect. Fig.19 , the spectrum is shown in Fig.15 When a flat side is used and the distance between the baffle 21 and the substrate is 0, a hard gradient can be achieved. The schematic diagram of the product effect is as follows Fig.18 , baffle 21 corresponds to the white (high transmittance) area of ​​the product, and the spectrum is as follows Fig.14 shown.

[0108] Example 3

[0109] The method for preparing a gradient neutral grayscale mirror based on a magnetron sputtering coating process in this embodiment specifically includes the following steps:

[0110] Design the film system and first coat the clean substrate with an anti-reflection film to test whether the optical performance meets the requirements. Then select a suitable GND Mask according to the gradient width (see Figure 8 , Fig.13 , or use Figure 7 , Fig. 9 , Fig.11 Any two of them are spliced ​​together to form a hollowed-out form in the middle) and loaded to the appropriate position. Start the target cleaning program, and after completion, load the good products coated with anti-reflection film, cover the position that does not need to be coated with attenuation film, and run the attenuation film coating program for coating. After completion, test the product and judge whether the product is qualified according to the index requirements.

[0111] The obtained product has anti-reflection at both ends, attenuation in the middle, and smooth transition. The product effect diagram is as follows Fig.21 , product spectrum curve see Fig.17 (Take GND8 as an example).

[0112] Example 4

[0113] The method for preparing a gradient neutral grayscale mirror based on a magnetron sputtering coating process in this embodiment specifically includes the following steps:

[0114] Design the film system and first coat the clean substrate with an anti-reflection film to test whether the optical performance meets the requirements. Then select a suitable GND Mask according to the gradient width (see Figure 6 , Fig.10 , Fig.12 ) and load it to the appropriate position. Start the target cleaning program, and after completion, load the good products coated with anti-reflection film, cover the position that does not need to be coated with attenuation film, and run the attenuation film coating program for coating. After completion, test the product and judge whether the product is qualified according to the index requirements.

[0115] The light transmittance of the obtained product is attenuated at both ends, highly transparent in the middle, and has a smooth transition. The product effect diagram is shown as follows Fig. 20 , product spectrum curve see Fig.16 (Take GND8 as an example).

[0116] The GND Filters currently on the market are basically made using an evaporation coating process. The film layer is not dense enough, the surface hardness is low, it is not scratch-resistant, and the resistance to acid, alkali, temperature and humidity is insufficient. The film layer adhesion is relatively low, resulting in a short life. It is also difficult to directly use commercial magnetron sputtering coating equipment and processes to produce a gradient spectrum, mainly because the space in the vacuum chamber is limited. According to the characteristics of the magnetron sputtering process, the distance between the substrate and the target material cannot be increased too much, otherwise it will affect the growth of the thin film and thus affect the optical performance of the product. The present invention adds a GND Mask component in a limited space and makes its position adjustable, shape and size variable, thereby ensuring that the film thickness changes as needed, thereby achieving the purpose of gradually smoothing the spectral curve and greatly improving the product defects caused by the evaporation process.

[0117] The method of manufacturing a GND filter using a magnetron sputtering coating process of the present invention includes a film system design for depositing a functional film, that is, the same film system includes an anti-reflection film system and an attenuation film system; when coating, the anti-reflection film system is first coated, and then the attenuation film system is coated. By changing the shape of the GND Mask (such as Figure 6 to Figure 13 The thickness and gradient range of the thin film deposition can be changed by adjusting the distance between the GND Mask and the substrate (as shown in the figure) and adjusting the distance between the GND Mask and the substrate. Through the hollowing out of the edge of the GND Mask, the target particles are gradually reduced on the motion path, and the diffracted particles are disturbed, eventually forming a uniform and gradually decreasing thin film. There are two schemes for adjusting the distance between the GND Mask and the substrate: automatic control and manual control. Automatic control is that the stepper motor controls the movement of the GND Mask at this position (when the attenuation film is plated, the Mask moves to the specified position; when the attenuation film is not plated, the GND Mask leaves the position between the target and the substrate to avoid blocking the movement of the target particles to the substrate). Manual control is to open the vacuum chamber to manually install and adjust the GND Mask. The Mask can be adjusted up and down through the threaded hole; the distance between the substrate, the Mask, and the target can be adjusted by rotating the fixed screw. The hollow design of the Mask includes but is not limited to the shape of the hollow unit being a sawtooth, inclined sawtooth, bar, arc, diamond, fishing net, etc. The hollow size is designed according to product requirements. Generally, the sawtooth tip angle is about 30°, and the hollow area gradually decreases from one end of the attenuation film to the anti-reflection film. The attenuation film layer will be deposited in the hollow part, and there is no attenuation film layer in the non-hollow area (originally coated with an anti-reflection film layer). Only in this way can the installation of the Mask achieve the transition from attenuation to anti-reflection; and then the spacing between the Mask (baffle) and the substrate can be combined to achieve the gradient width required in practice.

[0118] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A magnetron sputtering device for preparing a gradient medium grayscale mirror, comprising a vacuum chamber, a target assembly, a vacuum chamber door and a bearing portion located in the vacuum chamber, wherein the bearing portion is used to bear a substrate, and the substrate is arranged opposite to the target assembly, characterized in that: A baffle assembly for forming a gradient region of a gradient medium grayscale mirror is provided between the substrate and the target assembly. The baffle assembly comprises a baffle and a fixing mechanism for fixing the baffle.

2. The magnetron sputtering device according to claim 1, characterized in that: The baffle is provided with a flat portion for forming a hard gradient and / or a hollow portion for forming a soft gradient, the hollow portion runs through the thickness direction of the baffle, and the hollow portion is located in the middle or at the edge of the baffle in the width direction.

3. The magnetron sputtering device according to claim 2, characterized in that: The hollow portion includes a plurality of hollow units, and each of the hollow units is a combination of one or more of a circular shape, a continuous or discontinuous V-shape, and an arc shape.

4. The magnetron sputtering device according to claim 1, characterized in that: The baffle is fixed to the end of the fixing mechanism; and a through hole is provided on the baffle for the fixing mechanism to pass through.

5. The magnetron sputtering device according to claim 1 or 4, characterized in that: The baffle assembly includes a driving mechanism for driving the fixing mechanism to move.

6. The magnetron sputtering device according to claim 4, characterized in that: The baffle comprises a plate portion and a rod portion, the plate portion is arranged on the rod portion, the length of the rod portion is greater than the plate portion, the through hole is opened on the rod portion, and the hollow portion is arranged on the plate portion.

7. The magnetron sputtering device according to claim 1, characterized in that: The invention comprises a correction component for correcting the uniformity of the film layer, wherein the correction component is arranged between the substrate and the target material component.

8. The magnetron sputtering device according to claim 7, characterized in that: The baffle is disposed between the substrate and the correction assembly.

9. The magnetron sputtering device according to claim 2, characterized in that: A target chamber is provided on the side of the vacuum chamber, the target assembly and the baffle assembly are arranged in the target chamber, and a protective door is provided between the target chamber and the vacuum chamber.

10. The magnetron sputtering device according to claim 9, characterized in that: The length of the baffle is less than or equal to the width between the inner walls of the target chamber; and / or the length of the hollow portion is less than or equal to the length of the baffle.

11. A method for preparing a gradient medium grayscale mirror, characterized in that: The steps include: Determining the gradient region and optical film design of the gradient medium grayscale mirror; The structure of the baffle is designed according to the gradient range; the baffle is used to form a gradient area of ​​the gradient medium grayscale mirror; Anti-reflection film coating is carried out according to the designed optical film; The baffle is arranged between the target assembly and the substrate; The attenuation film system is plated according to the designed optical film to obtain the gradient neutral gray mirror.

12. The preparation method according to claim 11, characterized in that: The parameters of the baffle structure design include the shape of the hollow unit and the distance between the baffle and the substrate. The shape of the hollow unit includes the opening size and depth.

13. The preparation method according to claim 12, characterized in that: When the gradient area of ​​the gradient medium grayscale mirror becomes narrower, the opening size of the hollow unit increases, the depth becomes smaller, and the distance between the baffle and the substrate becomes smaller.

14. The preparation method according to claim 12, characterized in that: When the gradient of the gradient medium grayscale mirror is a hard gradient, the distance between the baffle and the substrate is 0.

15. The preparation method according to claim 11, characterized in that: The step also includes: testing the obtained gradient medium grayscale mirror, and adjusting the structure of the baffle according to the test result; until the parameters of the obtained gradient medium grayscale mirror meet the requirements.

16. The preparation method according to claim 11, characterized in that: When designing the optical film, the anti-reflection film system is designed first, and then the attenuation film system is designed based on the anti-reflection film system.

17. A gradient neutral grayscale mirror prepared by the preparation method according to any one of claims 11 to 16.

18. Application of the gradient neutral grayscale mirror as claimed in claim 17 in an imaging module.