Test method for testing water stability of drainage asphalt mixture
The hemispherical penetration method was used to evaluate the water stability of drainage asphalt mixtures, which solved the problem that existing technologies could not simulate tire pressure distribution and achieved a more accurate evaluation of water stability.
Patent Information
- Application Number
- CN202411077749.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
AI Technical Summary
Existing technologies cannot simulate the uneven pressure distribution of tires on the road surface when evaluating the water stability of drainage asphalt mixtures, resulting in limitations in the evaluation.
The hemispherical penetration method was used to form specimens by compaction. After immersion in water or freeze-thaw treatment, pressure was applied using an electronic universal testing machine to obtain force-displacement curves and calculate the hemispherical penetration work and penetration work ratio to evaluate the water stability of drainage asphalt mixtures.
By simulating the uneven distribution of contact pressure between car tires and asphalt pavement, the accuracy of water stability evaluation for drainage asphalt mixtures is improved.
Smart Images

Figure CN118913901A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt mixture detection, and in particular to a test method for testing the water stability of drainage asphalt mixture. Background Art
[0002] Asphalt mixture is a composite material, mainly composed of asphalt, coarse aggregate, fine aggregate, mineral powder, and sometimes polymers and wood cellulose. These materials of different qualities and quantities are mixed to form different structures and have different mechanical properties.
[0003] At present, the evaluation of the water stability of drained asphalt mixture is mainly based on the standard test methods in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011) - freeze-thaw splitting test and immersion Marshall test. The water damage resistance of drained asphalt mixture is mainly evaluated from the strength aspect, which cannot simulate the unevenly distributed pressure of tires on the road surface. In addition, the void ratio of drained asphalt mixture (18%~25%) is much larger than the void ratio of dense-graded asphalt mixture (2%~6%), resulting in limitations in the standard test method for evaluating the water stability of drained asphalt mixture.
[0004] Therefore, the hemispherical penetration ratio was proposed to evaluate the water stability of drained asphalt mixtures. Summary of the invention
[0005] The purpose of the present invention is to provide a test method for testing the water stability of drained asphalt mixture, aiming to solve the problem that the standard test method cannot simulate the unevenly distributed pressure condition of tires on the road surface, resulting in limitations in the evaluation of the water stability of drained asphalt mixture by the standard test method.
[0006] To achieve the above object, the present invention provides a test method for testing the water stability of drainage asphalt mixture, comprising the following steps:
[0007] Based on the compaction method, drainage asphalt mixture specimens were formed, and the physical indicators of the specimens were measured and set into a test group and a comparison group;
[0008] The test group and the control group are subjected to water immersion or freeze-thaw treatment;
[0009] Pressurizing the treated test pieces in the test group and the comparison group by a hemispherical indenter to obtain force-displacement curves of the test group and the comparison group;
[0010] The hemispherical penetration work of the test group, the hemispherical penetration work of the comparison group and the penetration work ratio are calculated based on the force-displacement curves of the test group and the comparison group, and the water stability of the drainage asphalt mixture is evaluated by the penetration work ratio.
[0011] Among them, the diameter of the specimen is 101.6±0.2mm and the height is 63.5±1.3mm.
[0012] The specific method of water immersion treatment for the test group and the control group is as follows:
[0013] The comparison group test pieces were placed in a constant temperature water bath at a temperature of 60°C ± 0.5°C for 30 to 40 minutes;
[0014] The test group specimens were placed in a constant temperature water bath at 60°C ± 0.5°C for 48 hours.
[0015] The specific method of freeze-thaw treatment of the test group and the control group is as follows:
[0016] The test pieces of the comparison group are stored at room temperature for future use;
[0017] The test group specimens were vacuum-filled with water, maintained at a vacuum degree of 97.3 to 98.7 for 15 minutes, the valve was opened, and normal pressure was restored. The test group specimens were placed in water for 30 minutes;
[0018] Take out the test group specimens and put them into a cylindrical plastic box, add water until they are submerged, and put them into a constant temperature refrigerator at a freezing temperature of -18°C ± 2°C for 16h ± 1h;
[0019] After taking out the test pieces of the comparison group, immediately put them together with the plastic box into a constant temperature water bath at a temperature of 60°C ± 0.5°C and keep them warm for 24 hours;
[0020] All the test specimens of the test group and the control group were immersed in a constant temperature water bath at a temperature of 25°C±0.5°C for no less than 2 hours.
[0021] The specific method of applying pressure to the treated test pieces in the test group and the comparison group by a hemispherical indenter to obtain the force-displacement curves of the test group and the comparison group is as follows:
[0022] Take out the treated test pieces in the test group and the comparison group, quickly place them on the loading base of the electronic universal testing machine, place the hemispherical indenter above the test pieces, and adjust the height of the loading head of the testing machine;
[0023] The specimen was loaded and the force-displacement curve was observed. When the penetration force decayed to a basically unchanged state, the specimen was unloaded and removed, and the force-displacement curve obtained during the penetration process was saved to obtain the force-displacement curves of the test group and the comparison group.
[0024] The present invention discloses a test method for testing the water stability of a drainage asphalt mixture. The method comprises the following steps: forming a drainage asphalt mixture specimen by a compaction method, measuring the physical indexes of the specimen, and setting the specimens in a test group and a comparison group; subjecting the test group and the comparison group to water immersion or freeze-thaw treatment; applying pressure to the specimens in the treated test group and the comparison group by a hemispherical pressure head, and obtaining the force-displacement curves of the test group and the comparison group; calculating the hemispherical penetration work of the test group, the hemispherical penetration work of the comparison group, and the penetration work ratio based on the force-displacement curves of the test group and the comparison group, and evaluating the water stability of the drainage asphalt mixture by the penetration work ratio. The method forms a drainage asphalt mixture by a Marshall compaction instrument. A standard Marshall specimen is prepared, and a loading test is performed on the specimen at a speed of 50 mm / min using an 80 mm diameter hemisphere through an electronic universal testing machine, and a force-displacement curve is obtained. The hemisphere penetration work and the penetration work ratio are calculated based on the force-displacement curve, and the water stability of the drained asphalt mixture is evaluated with the penetration work ratio. The uneven distribution of contact pressure between automobile tires and asphalt pavement is simulated by pressurizing the hemisphere, so that the water stability evaluation of the drained asphalt mixture is more accurate, and the problem that the standard test method cannot simulate the uneven distribution of tire pressure on the pavement, resulting in limitations in the standard test method for evaluating the water stability of drained asphalt mixture, is solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 It is a diagram of a hemispherical installation.
[0027] Figure 2 This is a schematic diagram of the hemispherical penetration test.
[0028] Figure 3 It is a schematic diagram of the results of the submerged hemisphere penetration test, where (a) is the control group and (b) is the comparison group.
[0029] Figure 4 It is a schematic diagram of the freeze-thaw hemispherical penetration test results, where (a) is the control group and (b) is the comparison group.
[0030] Figure 5 It is a typical force-displacement curve of hemispherical penetration test.
[0031] Figure 6 A flow chart of a test method for testing the water stability of drained asphalt mixtures. DETAILED DESCRIPTION
[0032] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0033] See also Figures 1 to 6 The present invention provides a test method for testing the water stability of drainage asphalt mixture, comprising the following steps:
[0034] S1: Based on the compaction method, drainage asphalt mixture specimens were formed, the physical indicators of the specimens were measured, and they were set in the test group and the control group;
[0035] Specifically, the drainage asphalt mixture specimens are formed by the compaction method in accordance with the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011) T0704. The specimen size should meet the requirements of diameter 101.6±0.2mm and height 63.5±1.3mm. After the specimen is formed and completely cooled, it can be demoulded, and the specimen height is measured. For the specimens that meet the requirements, a test group and a comparison group are set, with no less than 5 specimens in each group. The density, porosity and other physical indicators of the specimens are measured.
[0036] S2: subjecting the test group and the control group to water immersion or freeze-thaw treatment;
[0037] Specifically, the specific way of immersion treatment of the test group and the control group is:
[0038] S201: placing the comparison group test piece in a constant temperature water bath at a temperature of 60°C ± 0.5°C and keeping the temperature for 30 to 40 minutes;
[0039] S202: Place the test group specimens in a constant temperature water bath at 60°C ± 0.5°C for 48 hours.
[0040] The specific method of freeze-thaw treatment of the test group and the control group is as follows:
[0041] S211: storing the comparison group test pieces at room temperature for future use;
[0042] S212: vacuum saturating the test pieces in the test group with water, maintaining the vacuum degree at 97.3-98.7 for 15 minutes, opening the valve, restoring the normal pressure, and placing the test pieces in water for 30 minutes;
[0043] Specifically, the test group specimens were vacuum-saturated with water, maintained at a vacuum degree of 97.3-98.7 (730-740 mmHg) for 15 minutes, the valve was opened, and normal pressure was restored, and the test group specimens were placed in water for 30 minutes.
[0044] S213: Take out the test group specimens and put them into a cylindrical plastic box, add water until they are submerged, and put them into a constant temperature refrigerator at a freezing temperature of -18°C ± 2°C for 16h ± 1h;
[0045] S214: After taking out the comparison group test piece, immediately put it together with the plastic box into a constant temperature water bath at a temperature of 60°C ± 0.5°C and keep it warm for 24 hours;
[0046] S215: Immerse all the test specimens of the test group and the control group in a constant temperature water bath at a temperature of 25°C±0.5°C for no less than 2 hours.
[0047] S3: applying pressure to the treated test pieces in the test group and the comparison group by a hemispherical indenter to obtain force-displacement curves of the test group and the comparison group;
[0048] Specifically, the treated test pieces in the test group and the comparison group are pressurized by a hemispherical indenter to obtain the force-displacement curves of the test group and the comparison group:
[0049] S31: taking out the treated test pieces from the test group and the comparison group, quickly placing them on the loading base of the electronic universal testing machine, placing a hemispherical indenter on the test pieces, and adjusting the height of the loading head of the testing machine;
[0050] S32 loads the specimen and observes the force-displacement curve. When the penetration force decays to a substantially constant value, the specimen is unloaded and removed, and the force-displacement curve obtained during the penetration process is saved to obtain the force-displacement curves of the test group and the comparison group.
[0051] Specifically, the specimen was loaded at a rate of 50 mm / min.
[0052] S4: Calculate the hemispherical penetration work of the test group, the hemispherical penetration work of the comparison group and the penetration work ratio based on the force-displacement curves of the test group and the comparison group, and use the penetration work ratio to evaluate the water stability of the drainage asphalt mixture.
[0053] Specifically, the hemispherical penetration work was calculated by multiplying the maximum force in the force-displacement curve by the corresponding penetration displacement. The penetration work ratio was obtained by dividing the penetration work of the control group by the penetration work of the test group. The water stability of the drainage asphalt mixture was evaluated by the penetration work ratio.
[0054] The penetration work and penetration work ratio of drainage asphalt mixture are calculated as follows:
[0055] Q=F max ×L
[0056]
[0057] Where:
[0058] Q——hemisphere penetration work (N·mm);
[0059] F max ——The maximum value of the force generated during hemispherical penetration (N);
[0060] L——Penetration displacement corresponding to the maximum force (mm);
[0061] GR——hemisphere penetration ratio (%);
[0062] ——average value of hemispherical penetration work of effective specimens in the test group (N·mm);
[0063] ——Average value of hemispherical penetration work of effective specimens in the comparison group (N·mm).
[0064] The average value of each group of test pieces is taken as the test result. When the difference between a test data in a group of test values and the average value is greater than k times the standard deviation, the test value is discarded and the average value of the remaining test values is taken as the test result.
[0065] When the number of samples m is 3, 4, 5, and 6, the k values are 1.15, 1.46, 1.67, and 1.82, respectively.
[0066] The method uses a Marshall compactor to form a standard Marshall specimen of a drained asphalt mixture, and then uses an 80mm diameter hemisphere to load the specimen at a speed of 50mm / min through an electronic universal testing machine, and obtains a force-displacement curve diagram, and calculates the hemisphere penetration work and the penetration work ratio according to the force-displacement curve diagram, and evaluates the water stability of the drained asphalt mixture with the penetration work ratio. The hemisphere pressurization simulates the uneven distribution of contact pressure between automobile tires and asphalt pavement, so that the water stability evaluation of the drained asphalt mixture is more accurate, and solves the problem that the standard test method cannot simulate the unevenly distributed pressure condition of the tire on the pavement, resulting in the limitation of the standard test method in evaluating the water stability of the drained asphalt mixture.
[0067] What is disclosed above is only a preferred embodiment of a test method for testing the water stability of drained asphalt mixture of the present invention. Of course, it cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiments and equivalent changes made according to the claims of the present invention are still within the scope of the invention.
Claims
1. A test method for testing the water stability of drained asphalt mixture, characterized in that: The following steps are involved: Based on the compaction method, drainage asphalt mixture specimens were formed, and the physical indicators of the specimens were measured and set into a test group and a comparison group; The test group and the control group are subjected to water immersion or freeze-thaw treatment; Pressurizing the treated test pieces in the test group and the comparison group by a hemispherical indenter to obtain force-displacement curves of the test group and the comparison group; The hemispherical penetration work of the test group, the hemispherical penetration work of the comparison group and the penetration work ratio are calculated based on the force-displacement curves of the test group and the comparison group, and the water stability of the drainage asphalt mixture is evaluated by the penetration work ratio.
2. A test method for testing the water stability of drained asphalt mixture as claimed in claim 1, characterized in that: The specimen has a diameter of 101.6±0.2 mm and a height of 63.5±1.3 mm.
3. A test method for testing the water stability of drained asphalt mixture as claimed in claim 1, characterized in that: The specific method of water immersion treatment for the test group and the control group is as follows: The comparison group test pieces were placed in a constant temperature water bath at a temperature of 60°C ± 0.5°C for 30 to 40 minutes; The test group specimens were placed in a constant temperature water bath at 60°C ± 0.5°C for 48 hours.
4. A test method for testing the water stability of drained asphalt mixture as claimed in claim 1, characterized in that: The specific method of freeze-thaw treatment of the test group and the control group is as follows: The test pieces of the comparison group are stored at room temperature for future use; The test group specimens were vacuum-filled with water, maintained at a vacuum degree of 97.3 to 98.7 for 15 minutes, the valve was opened, and normal pressure was restored. The test group specimens were placed in water for 30 minutes; Take out the test group specimens and put them into a cylindrical plastic box, add water until they are submerged, and put them into a constant temperature refrigerator at a freezing temperature of -18°C ± 2°C for 16h ± 1h; After taking out the test pieces of the comparison group, immediately put them together with the plastic box into a constant temperature water bath at a temperature of 60°C ± 0.5°C and keep them warm for 24 hours; All the test specimens of the test group and the control group were immersed in a constant temperature water bath at a temperature of 25°C±0.5°C for no less than 2 hours.
5. A test method for testing the water stability of drained asphalt mixture as claimed in claim 1, characterized in that: The specific method of applying pressure to the treated test pieces in the test group and the comparison group by a hemispherical indenter to obtain the force-displacement curves of the test group and the comparison group is as follows: Take out the treated test pieces in the test group and the comparison group, quickly place them on the loading base of the electronic universal testing machine, place the hemispherical indenter above the test pieces, and adjust the height of the loading head of the testing machine; The specimen was loaded and the force-displacement curve was observed. When the penetration force decayed to a basically unchanged state, the specimen was unloaded and removed, and the force-displacement curve obtained during the penetration process was saved to obtain the force-displacement curves of the test group and the comparison group.