Hard mask composition, hard mask layer, and method of forming pattern
By forming a hard mask layer using a hard mask composition of a specific compound and solvent, the problem of insufficient etch resistance during pattern transfer in lithography technology is solved, and fine pattern transfer and etch resistance at high temperatures are achieved. Improves the quality and accuracy of semiconductor patterns.
Patent Information
- Application Number
- CN202410528195.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2024-04-29
- Publication Date
- 2024-11-08
AI Technical Summary
The existing lithography technology is difficult to form fine patterns with excellent profiles, especially between the material layer and the photoresist layer. The etch resistance of the hard mask layer is not sufficient to resist the etching process, which affects the accuracy of pattern transfer and quality.
Using a hard mask composition containing a specific compound and solvent, a hard mask layer is formed by heat treatment and selectively removed after photoresist pattern formation to expose the material layer, etching resistance of the hard mask layer is employed. and heat resistance to improve the pattern transfer process.
It is realized that the hard mask layer with excellent etch resistance and heat resistance is formed at high temperatures, ensuring the accuracy and quality of pattern transfer, and improving the fineness and etch resistance of semiconductor patterns.
Smart Images

Figure CN118915385A_ABST
Abstract
Description
[0001] CROSS REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2023-0059328 filed in the Korean Intellectual Property Office on May 8, 2023, the entire contents of which are incorporated herein by reference. Technical Field
[0003] Embodiments relate to a hard mask composition, a hard mask layer, and a method of forming a pattern. Background Art
[0004] In recent years, the semiconductor industry has developed ultra-fine technology with patterns ranging from a few nanometers to tens of nanometers in size. This ultra-fine technology can utilize photolithography technology.
[0005] Some photolithography techniques may include: providing a material layer on a semiconductor substrate; coating a photoresist layer on the material layer; exposing and developing the photoresist layer to provide a photoresist pattern; and etching the material layer using the photoresist pattern as a mask.
[0006] Depending on the small size of the pattern to be formed, it may be difficult to provide a fine pattern with an excellent profile by using only some photolithography techniques. Therefore, an auxiliary layer called a hard mask layer may be formed between the material layer and the photoresist layer to provide a fine pattern. Summary of the invention
[0007] Embodiments may be implemented by providing a hard mask composition including a compound represented by Chemical Formula 1 and a solvent:
[0008] [Chemical formula 1]
[0009]
[0010] In chemical formula 1, Ar 1 and Ar 2 are each independently a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a group in which two or more substituted or unsubstituted C6 to C30 aromatic hydrocarbon groups are linked by a single bond or a substituted or unsubstituted C1 to C30 alkylene group,
[0011] R 1 and R 2 are each independently hydrogen, deuterium, a substituted or unsubstituted monovalent C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted monovalent C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a combination thereof, and
[0012] n is an integer of 2 to 6.
[0013] Ar in chemical formula 1 1 and Ar 2 The substituted or unsubstituted groups which may each independently be moieties of Group 1 are:
[0014] [Group 1]
[0015]
[0016] Ar in Formula 1 1 and Ar 2 The substituted or unsubstituted groups which may each independently be part of Group 1-1 are:
[0017] [Group 1-1]
[0018]
[0019] R in Formula 1 1 and R 2 Each may independently be hydrogen, deuterium, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a combination thereof.
[0020] R in Formula 1 1 and R 2 Each may independently be hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C6 to C20 aromatic hydrocarbon group, or a combination thereof.
[0021] Ar in Formula 1 1 and Ar 2 may be independently a substituted or unsubstituted group of Group 1-2, R 1 and R 2 may each independently be hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C6 to C20 aromatic hydrocarbon group, or a combination thereof, and n may be an integer from 2 to 4,
[0022] [Group 1-2]
[0023]
[0024] In Chemical Formula 1, n may be 2 or 3, and R 1 , R 2 and Ar 2 Can be the same.
[0025] The compound represented by Chemical Formula 1 may be represented by one of Chemical Formulas 2 to 10:
[0026] [Chemical formula 2]
[0027]
[0028] [Chemical formula 3]
[0029]
[0030] [Chemical formula 4]
[0031]
[0032] [Chemical formula 5]
[0033]
[0034] [Chemical formula 6]
[0035]
[0036] [Chemical formula 7]
[0037]
[0038] [Chemical formula 8]
[0039]
[0040] [Chemical formula 9]
[0041]
[0042] [Chemical formula 10]
[0043]
[0044] The compound may have a molecular weight of about 300 g / mole to about 10,000 g / mole.
[0045] The compound may be included in an amount of about 0.1 wt % to about 30 wt % based on the total weight of the hardmask composition.
[0046] The solvent may include propylene glycol, propylene glycol diacetate, methoxypropylene glycol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, acetylacetone or ethyl 3-ethoxypropionate.
[0047] Embodiments may be implemented by providing a hard mask layer including a cured product of the hard mask composition according to embodiments.
[0048] According to some embodiments, a method of forming a pattern may include: providing a material layer on a substrate; applying a hard mask composition according to an embodiment to the material layer to form a hard mask layer; thermally treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer; and etching the exposed portion of the material layer.
[0049] Forming the hard mask layer may include performing a heat treatment at about 100°C to about 1,000°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Features will be readily apparent to those skilled in the art by describing exemplary embodiments in detail with reference to the accompanying drawings, in which:
[0051] Figure 1 Reference diagrams illustrating level differences of a hard mask layer to explain a method of evaluating planarization characteristics and calculation formulas for evaluating planarization characteristics are shown. DETAILED DESCRIPTION
[0052] Example embodiments will now be described more fully hereinafter with reference to the accompanying drawings; however, they may be embodied in different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and these embodiments will fully convey exemplary implementations to those skilled in the art.
[0053] In the various drawings, the dimensions of layers and regions may be exaggerated for clarity of illustration. It is also understood that when a layer or element is referred to as being "on" another layer or substrate, it may be directly on the other layer or substrate, or there may be intervening layers. Furthermore, it is understood that when a layer is referred to as being "below" another layer, it may be directly below, and there may also be one or more intervening layers. In addition, it is also understood that when a layer is referred to as being "between" two layers, it may be the only layer between the two layers, or there may also be one or more intervening layers. The same reference numerals refer to the same elements throughout.
[0054] As used herein, when no definition is otherwise provided, 'substituted' may refer to that a hydrogen atom of a compound is replaced by a substituent selected from the group consisting of a halogen atom (F, Br, Cl or I), a hydroxyl group, an alkoxy group, a nitro group, a cyano group, an amino group, an azido group, a carbamimido group, a hydrazine group, a hydrazo group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphate group or a salt thereof, a vinyl group, a C1 to C20 alkyl group, a C2 to C20 alkenyl group, a C2 to C20 alkynyl group, a C6 to C30 aryl group, a C7 to C30 aralkyl group, a C9 to C30 allylaryl group, a C1 to C30 alkoxy group, a C1 to C20 heteroalkyl group, a C3 to C20 heteroaralkyl group, a C3 to C30 cycloalkyl group, a C3 to C15 cycloalkenyl group, a C6 to C15 cycloalkynyl group, a C3 to C30 heterocycloalkyl group, or a combination thereof. As used herein, hydrogen substitution (-H) may include deuterium substitution (-D) or tritium substitution (-T). For example, any hydrogen in any compound described herein may be protium, deuterium, or tritium (e.g., based on natural substitution or artificial substitution). As used herein, the term "or" is not necessarily an exclusive term, for example, "A or B" will include A, B, or A and B. As used herein, * is a point of attachment unless otherwise described.
[0055] In addition, two adjacent substituents of a substituted halogen atom (F, Br, Cl or I), a hydroxyl group, a nitro group, a cyano group, an amino group, an azido group, a carbamimido group, a hydrazine group, a hydrazone group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphate group or a salt thereof, a C1 to C30 alkyl group, a C2 to C30 alkenyl group, a C2 to C30 alkynyl group, a C6 to C30 aryl group, a C7 to C30 aralkyl group, a C1 to C30 alkoxy group, a C1 to C20 heteroalkyl group, a C3 to C20 heteroaralkyl group, a C3 to C30 cycloalkyl group, a C3 to C15 cycloalkenyl group, a C6 to C15 cycloalkynyl group, or a C2 to C30 heterocyclyl group may be condensed to form a ring.
[0056] As used herein, when no definition is otherwise provided, "aromatic hydrocarbon group" refers to a group having one or more hydrocarbon aromatic moieties, including a form in which the hydrocarbon aromatic moieties are connected by a single bond, a non-aromatic condensed ring form in which the hydrocarbon aromatic moieties are directly or indirectly condensed, or a combination thereof, as well as a non-condensed aromatic hydrocarbon ring, a condensed aromatic hydrocarbon ring.
[0057] More specifically, the substituted or unsubstituted aromatic hydrocarbon group may be a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthrenyl group, a substituted or unsubstituted fused tetraphenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted terphenyl group, a substituted or unsubstituted quaterphenyl group, a substituted or unsubstituted chrysene group, a substituted or unsubstituted triphenylenyl group, a substituted or unsubstituted peryl group, a substituted or unsubstituted indenyl group, a combination thereof, or a combined fused ring of the foregoing groups, but is not limited thereto.
[0058] Unless otherwise specified in the specification, the "molecular weight" is measured by dissolving a powder sample in tetrahydrofuran (THF) and then using Agilent Technologies' 1200 series Gel Permeation Chromatography (GPC) (column: Shodex Company LF-804, standard sample: Showa Company polystyrene).
[0059] The hard mask composition according to some embodiments may include a compound represented by Chemical Formula 1 and a solvent.
[0060] [Chemical formula 1]
[0061]
[0062] In Chemical Formula 1, Ar 1 and Ar 2 They may each independently be or include, for example, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a group in which two or more substituted or unsubstituted C6 to C30 aromatic hydrocarbon groups may be linked via a single bond or a substituted or unsubstituted C1 to C30 alkylene group.
[0063] R 1 and R 2 Each independently may be or include, for example, hydrogen, deuterium, a substituted or unsubstituted monovalent C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted monovalent C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a combination thereof.
[0064] n may be an integer from 2 to 6.
[0065] The compound according to some embodiments may include an aromatic hydrocarbon group as shown in Chemical Formula 1, and at the same time may have a triple bond directly connected to a central aromatic hydrocarbon ring, thereby increasing the carbon content of the composition and improving crosslinking characteristics when curing a hard mask composition including the compound according to some embodiments.
[0066] Chemical formula 1 may include -OR 2 The substituent represented by , makes it possible to improve the solubility of the compound in a solvent, and the hard mask composition containing it can be effectively applied to a spin coating process. In addition, since the compound can be cross-linked into a high molecular weight polymer form in a short period of time after heat treatment, a hard mask layer formed therefrom can have excellent heat resistance and excellent etching resistance.
[0067] Ar in Formula 1 1 and Ar 2 The groups which may each independently be part of Group 1 are substituted or unsubstituted.
[0068] [Group 1]
[0069]
[0070] In an embodiment, Ar in Formula 1 1 and Ar 2 Each independently may be a substituted or unsubstituted group of the part of Group 1-1.
[0071] [Group 1-1]
[0072]
[0073] In an embodiment, Ar in Formula 1 1 and Ar 2 Each independently may be a substituted or unsubstituted group of a part of Group 1-2.
[0074] [Group 1-2]
[0075]
[0076] R in Formula 1 1 and R 2 may be each independently hydrogen, deuterium, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a combination thereof. 1 and R 2may be independently hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C6 to C20 aromatic hydrocarbon group, or a combination thereof. 1 and R 2 It may be hydrogen, methyl, ethyl, propyl, butyl, phenyl, naphthyl, phenanthrenyl, anthracenyl or pyrenyl, for example hydrogen, methyl or phenyl.
[0077] In an embodiment, in the compound represented by Chemical Formula 1, Ar 1 and Ar 2 may be independently a substituted or unsubstituted group of Group 1-2, R 1 and R 2 Each of them may independently be hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C6 to C20 aromatic hydrocarbon group, or a combination thereof, and n may be an integer of 2 to 4.
[0078] In an embodiment, in Chemical Formula 1, n may be an integer of 2 to 6. In an embodiment, n may be an integer of 2 to 4, for example, n may be 2 or 3. In an embodiment, if n in Chemical Formula 1 is 2 or 3, the solubility of the compound according to some embodiments in a solvent may be optimized, and the etching resistance of a hard mask layer formed of a hard mask composition containing the compound may be maximized.
[0079] In an embodiment, if n in Chemical Formula 1 is 2 or 3, then R 1 , R 2 and Ar 2 Each of R may be the same or different from each other. In an embodiment, if n is 2 or 3, then two or three R 1 Each of the R 2 Each of Ar may be the same or different from each other, and two or three Ar 2 Each of can be the same as or different from each other.
[0080] In the embodiment, the compound represented by Chemical Formula 1 may be represented by one of Chemical Formulas 2 to 10.
[0081] [Chemical formula 2]
[0082]
[0083] [Chemical formula 3]
[0084]
[0085] [Chemical formula 4]
[0086]
[0087] [Chemical formula 5]
[0088]
[0089] [Chemical formula 6]
[0090]
[0091] [Chemical formula 7]
[0092]
[0093] [Chemical formula 8]
[0094]
[0095] [Chemical formula 9]
[0096]
[0097] [Chemical formula 10]
[0098]
[0099] The compound may have a molecular weight of, for example, about 300 g / mol to about 10,000 g / mol. In an embodiment, the molecular weight of the compound may be about 400 g / mol to about 10,000 g / mol, such as about 500 g / mol to about 10,000 g / mol, about 500 g / mol to about 9,500 g / mol, about 500 g / mol to about 9,000 g / mol, about 600 g / mol to about 8,500 g / mol, about 600 g / mol to about 8,000 g / mol, about 700 g / mol to about 7,500 g / mol, or about 700 g / mol to about 7,000 g / mol. By having a molecular weight within the above range, the carbon content and solubility in a solvent of a hard mask composition containing the above compound can be adjusted and optimized.
[0100] The compound may be included, for example, in an amount of about 0.1 wt % to about 30 wt % based on the total weight of the hard mask composition. In an embodiment, the compound may be included, for example, in an amount of about 0.2 wt % to about 30 wt %, about 0.5 wt % to about 30 wt %, about 1 wt % to about 30 wt %, about 1 wt % to about 25 wt %, or about 1 wt % to about 20 wt %. By including the compound within the above range, the thickness, surface roughness, and planarization degree of the hard mask may be easily adjusted.
[0101] The hardmask composition may include a solvent. In an embodiment, the solvent may include, for example, propylene glycol, propylene glycol diacetate, methoxypropylene glycol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, acetylacetone, ethyl 3-ethoxypropionate, or the like. In an embodiment, the solvent may be a suitable solvent having sufficient solubility or dispersibility for the compound.
[0102] In an embodiment, the hardmask composition may further include additives such as a surfactant, a crosslinking agent, a thermal acid generator, or a plasticizer.
[0103] The surfactant may include, for example, fluoroalkyl compounds, alkylbenzene sulfonates, alkylpyridinium salts, polyethylene glycol, quaternary ammonium salts, and the like.
[0104] The crosslinking agent may be, for example, melamine, a substituted urea or a polymer crosslinking agent. In an embodiment, it may be a crosslinking agent having at least two crosslinking substituents, such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea or butoxymethylated thiourea.
[0105] In the embodiment, as the crosslinking agent, a crosslinking agent having high heat resistance may be used. The crosslinking agent having high heat resistance may include a compound having a crosslinking substituent having an aromatic ring (eg, a benzene ring or a naphthalene ring) in a molecule.
[0106] In an embodiment, the thermal acid generator may be, for example, an acid compound such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, hydroxybenzoic acid, naphthoic acid or 2,4,4,6-tetrabromocyclohexadienonone, benzoin tosylate, 2-nitrobenzyl tosylate, or other organic sulfonic acid alkyl esters.
[0107] According to some embodiments, a hard mask layer including a cured product of the foregoing hard mask composition may be provided.
[0108] Hereinafter, a method of forming a pattern using the aforementioned hard mask composition is described.
[0109] According to some embodiments, the method of forming a pattern may include: providing a material layer on a substrate; applying a hard mask composition including the aforementioned compound and a solvent to the material layer; thermally treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer; and etching the exposed portion of the material layer.
[0110] The substrate may be, for example, a silicon wafer, a glass substrate, or a polymer substrate. The material layer may be a material to be finally patterned, such as a metal layer (e.g., an aluminum layer or a copper layer), a semiconductor layer (e.g., a silicon layer), or an insulating layer (e.g., a silicon oxide layer or a silicon nitride layer). The material layer may be formed by a method such as a chemical vapor deposition (CVD) process.
[0111] The hard mask composition may be the same as described above and may be applied by spin coating in solution form. In an embodiment, the coating thickness of the hard mask composition may be, for example, about to about 200,000 angstroms.
[0112] The heat treatment of the hard mask composition may be performed, for example, at about 100° C. to about 1,000° C. for about 10 seconds to about 1 hour. In an embodiment, the heat treatment of the hard mask composition may include a plurality of heat treatment processes, such as a first heat treatment process and a second heat treatment process.
[0113] In an embodiment, heat treatment of the hard mask composition may include, for example, a heat treatment process at about 100° C. to about 1,000° C. for about 10 seconds to about 1 hour, and the heat treatment may be performed, for example, in an atmosphere of air or nitrogen, or an atmosphere having an oxygen concentration of 1 wt % or less.
[0114] In an embodiment, heat treatment of the hard mask composition may include a first heat treatment process, for example, at about 100°C to about 1,000°C, about 100°C to about 800°C, about 100°C to about 500°C, or about 150°C to about 400°C for about 30 seconds to about 1 hour, e.g., about 30 seconds to about 30 minutes, about 30 seconds to about 10 minutes, or about 30 seconds to about 5 minutes.
[0115] In embodiments, the heat treatment of the hard mask composition may include, for example, a second heat treatment process continuously performed at about 100° C. to about 1,000° C., about 300° C. to about 1,000° C., about 500° C. to about 1,000° C., or about 500° C. to about 600° C. for about 30 seconds to about 1 hour, for example, about 30 seconds to about 30 minutes, about 30 seconds to about 10 minutes, about 30 seconds to about 5 minutes. In embodiments, the first heat treatment process and the second heat treatment process may be performed in an air or nitrogen atmosphere, or may be performed in an atmosphere having an oxygen concentration of 1 wt % or less.
[0116] By performing at least one of the steps of heat-treating the hard mask composition at a high temperature, for example, 200° C. or higher, high etching resistance capable of withstanding etching gas and chemical liquid exposed in a subsequent process including an etching process may be exhibited.
[0117] In an embodiment, forming the hard mask layer may include a UV / Vis curing process or a near IR curing process.
[0118] In an embodiment, forming the hard mask layer may include a first heat treatment process, a second heat treatment process, a UV / Vis curing process, or a near IR curing process, or may include two or more processes in succession.
[0119] In an embodiment, the method may further include forming a silicon-containing thin layer on the hard mask layer. The silicon-containing thin layer may include, for example, SiCN, SiOC, SiON, SiOCN, SiC, SiO, SiN, or the like.
[0120] In an embodiment, the method may further include forming a bottom antireflective coating (BARC) on the silicon-containing thin layer or on the hard mask layer before forming the photoresist layer.
[0121] In an embodiment, the exposure of the photoresist layer may be performed using, for example, ArF, KrF, or EUV. After the exposure, a heat treatment may be performed at about 100° C. to about 700° C.
[0122] In an embodiment, the etching process of the exposed portion of the material layer may be performed by a dry etching process using an etching gas, and the etching gas may be, for example, N2 / O2, CHF3, CF4, Cl2, BCl3 or a mixed gas thereof.
[0123] The etched material layer may be formed in a plurality of patterns, and the plurality of patterns may be metal patterns, semiconductor patterns, insulating patterns, or the like, such as different patterns of a semiconductor integrated circuit device.
[0124] The following examples and comparative examples are provided to highlight the features of one or more embodiments, but it should be understood that the examples and comparative examples should not be interpreted as limiting the scope of the embodiments, and the comparative examples should not be interpreted as being outside the scope of the embodiments. In addition, it should be understood that the embodiments are not limited to the specific details described in the examples and comparative examples.
[0125] Synthesis of compounds
[0126] Synthesis Example 1
[0127] 24.7 grams of potassium tert-butoxide was added to a mixed solution of 12.6 grams of 1,3-diethynylbenzene, 21.2 grams of benzaldehyde and 200 grams of tetrahydrofuran (THF) cooled under a nitrogen atmosphere, and then stirred until all of the 1,3-diethynylbenzene reacted. After stirring, water was added thereto to stop the reaction. Subsequently, 200 grams of tetrahydrofuran (THF) was added thereto, and then washed and concentrated under reduced pressure, and the solid produced therein was filtered with n-hexane and dried under reduced pressure to obtain compound A represented by chemical formula 2-1.
[0128] [Chemical formula 2-1]
[0129]
[0130] Synthesis Example 2
[0131] Compound B represented by Chemical Formula 3-1 was obtained in the same manner as in Synthesis Example 1, except that 24.0 g of acetophenone was used instead of 21.2 g of benzaldehyde.
[0132] [Chemical formula 3-1]
[0133]
[0134] Synthesis Example 3
[0135] Compound C represented by Chemical Formula 4-1 was obtained in the same manner as in Synthesis Example 1, except that 37.6 g of benzophenone was used instead of 21.2 g of benzaldehyde.
[0136] [Chemical formula 4-1]
[0137]
[0138] Synthesis Example 4
[0139] Compound D represented by Chemical Formula 5-1 was obtained in the same manner as in Synthesis Example 1, except that 46.0 g of pyrenecarboxaldehyde was used instead of 21.2 g of benzaldehyde.
[0140] [Chemical formula 5-1]
[0141]
[0142] Synthesis Example 5
[0143] 31.1 grams of potassium tert-butoxide was added to a mixed solution of 12.6 grams of 1,3,5-triethynylbenzene, 58.0 grams of pyrene carboxaldehyde and 600 grams of tetrahydrofuran (THF) cooled under a nitrogen atmosphere, and then stirred in an ice bath until all of the 1,3,5-triethynylbenzene reacted. After stirring, water was added to stop the reaction. 600 grams of tetrahydrofuran (THF) was added thereto, and then washed and concentrated under reduced pressure, and the solid produced therefrom was filtered with n-hexane and dried under reduced pressure to obtain compound E represented by chemical formula 6-1.
[0144] [Chemical formula 6-1]
[0145]
[0146] Synthesis Example 6
[0147] 18.6 grams of potassium tert-butoxide was added to a mixed solution of 12.6 grams of diacetylpyrene, 21.2 grams of benzaldehyde and 240 grams of tetrahydrofuran (THF) cooled under a nitrogen atmosphere, and then stirred in an ice bath until all the diacetylpyrene reacted. After stirring, water was added thereto to stop the reaction. 240 grams of tetrahydrofuran (THF) was added thereto, and then washed and concentrated under reduced pressure, and the solid produced therein was filtered with n-hexane and dried under reduced pressure to obtain a compound F represented by chemical formula 7-1.
[0148] [Chemical formula 7-1]
[0149]
[0150] Synthesis Example 7
[0151] Compound G represented by Chemical Formula 8-1 was obtained in the same manner as in Synthesis Example 6, except that 12.1 g of acetophenone was used instead of 21.2 g of benzaldehyde.
[0152] [Chemical formula 8-1]
[0153]
[0154] Synthesis Example 8
[0155] Compound H represented by Chemical Formula 9-1 was obtained in the same manner as in Synthesis Example 6, except that 18.6 g of benzophenone was used instead of 21.2 g of benzaldehyde.
[0156] [Chemical formula 9-1]
[0157]
[0158] Synthesis Example 9
[0159] Compound I represented by Chemical Formula 10-1 was obtained in the same manner as in Synthesis Example 6, except that 23.2 g of pyrenecarboxaldehyde was used instead of 21.2 g of benzaldehyde.
[0160] [Chemical formula 10-1]
[0161]
[0162] Comparative Synthesis Example 1
[0163] Terephthalaldehyde (13.4 g, 0.1 mol) was dissolved in tetrahydrofuran (THF, 300 ml), and then cooled to 0°C under a nitrogen atmosphere. Subsequently, a THF mixed solution (0.5 molar concentration, 30 ml) in which ethynylmagnesium bromide was dissolved was slowly added thereto in a dropwise manner over 1 hour to react. After its temperature was increased to ambient temperature and further reacted for 12 hours, the resultant was quenched with a saturated aqueous ammonium chloride solution (saturated NH4Cl(aq)) while stirring. When the reaction was complete, the mixed solution was separated (combined) into an aqueous solution layer and an organic layer with ethyl acetate, and the organic layer was obtained after removing the aqueous solution layer. The compound represented by chemical formula 12-1 was obtained by removing the solvent of the separated organic layer. (yield: 90%)
[0164] [Chemical formula 12-1]
[0165]
[0166] The compound represented by Chemical Formula 12-1 (5.3 g, 0.09 mol) was dissolved in propylene glycol monomethyl ether acetate (PGMEA, 200 ml), and hydroxypyrene (HO-pyrene, 43 g, 0.2 mol) was added thereto. The mixed solution was heated to 90° C. until no compound represented by Chemical Formula 12-1 remained. After the reaction, Compound J represented by Chemical Formula 12 was obtained by purification.
[0167] [Chemical formula 12]
[0168]
[0169] Comparative Synthesis Example 2
[0170] 27.6 grams (0.1 mole) of benzoperylene and 42 grams (0.22 mole) of naphthoyl chloride are placed in a 2-liter 3-necked flask together with a mixed solution of 500 grams of chloroform / dichloromethane, and then reacted by adding 61.2 grams (0.35 mole) of aluminum chloride little by little thereto, while stirring by using a stirring rod. When the reaction is complete, water is used to remove aluminum trichloride. The product obtained in powder form is dissolved in tetrahydrofuran, and then reacted, while adding 18.98 grams (0.5 mole) of lithium aluminum hydride little by little thereto. When the reaction is complete, the by-product of the reaction is removed by using a mixture of water / methanol to obtain a comparative compound K represented by chemical formula 13.
[0171] [Chemical formula 13]
[0172]
[0173] Preparation of hard mask composition
[0174] Examples and Comparative Examples
[0175] Compounds A to I and Comparative Compounds J and K according to Synthesis Examples 1 to 9 and Comparative Synthesis Examples 1 to 2 were respectively dissolved in cyclohexanone and then filtered to prepare hard mask compositions having a compound content of 10.0 wt %.
[0176] Assessment 1: Heat resistance
[0177] Each of the hard mask compositions of Examples 1 to 9 and Comparative Examples 1 to 2 was spin-coated on a silicon wafer and heat-treated on a hot plate at 160°C for 1 minute to form a hard mask layer. The thickness of the hard mask layer was measured by using a film thickness meter manufactured by K-MAC Co., Ltd. Subsequently, the hard mask layer was heat-treated again at 400°C for 2 minutes, and then measured again with respect to the thickness. After calculating the thickness change ratio of the two thicknesses before and after reheat treatment at 400°C for 2 minutes, when the ratio before and after reheat treatment at 400°C for 2 minutes is less than 5%, "A" (excellent) is given, when greater than or equal to 5% and less than 10%, "B" (good) is given, and when greater than or equal to 10%, "C" (poor) is given. The results are shown in Table 1.
[0178] [Table 1]
[0179] Heat resistance Example 1 A Example 2 A Example 3 A Example 4 A Example 5 A Example 6 A Example 7 A Example 8 A Example 9 A Comparative Example 1 B Comparative Example 2 C
[0180] Referring to Table 1, the hard mask layers formed from the compositions of Examples 1 to 9 exhibited a thickness change ratio of less than 5% before and after reheat treatment, and the hard mask layer formed from the composition of the comparative example exhibited a thickness change ratio of greater than or equal to 5% before and after reheat treatment. In other words, the hard mask layer formed from the composition of the example exhibited excellent heat resistance compared to the hard mask layer formed from the composition of the comparative example.
[0181] Assessment 2: Gap Filling Features
[0182] The hard mask compositions of Examples 1 to 9 and Comparative Examples 1 to 2 were spin-coated on patterned silicon wafers, respectively, and heat-treated at 400° C. for 60 seconds to form hard mask layers. Each pattern cross-sectional image of the hard mask layer was detected by using a field emission scanning electron microscope (FE-SEM) to check whether voids were generated. The results are shown in Table 2.
[0183] [Table 2]
[0184] Is there a gap? Example 1 No gaps appear Example 2 No gaps appear Example 3 No gaps appear Example 4 No gaps appear Example 5 No gaps appear Example 6 No gaps appear Example 7 No gaps appear Example 8 No gaps appear Example 9 No gaps appear Comparative Example 1 A gap appears Comparative Example 2 No gaps appear
[0185] Referring to Table 2, voids were not generated in the hard mask layers formed from the compositions according to Examples 1 to 9, but voids were found in the hard mask layer formed from the composition according to Comparative Example 1. Therefore, the hard mask layer formed from the composition according to the Examples exhibited equivalent or excellent gap-filling characteristics compared to the hard mask layer formed from the composition according to the Comparative Example.
[0186] Evaluation 3: Flattening Features
[0187] Each of the hard mask compositions of Examples 1 to 9 and Comparative Examples 1 to 2 was spin-coated on a patterned silicon wafer and heat-treated at 400° C. for 60 seconds, and its pattern cross-sectional image was detected by using a field emission scanning electron microscope (FE-SEM). The hard mask layer on the pattern cross-sectional image was measured with respect to thickness, and according to Figure 1 The calculation equation digitizes its flattening degree. Figure 1 In the above table, h1 is obtained by measuring each thickness at three random points in the unpatterned region of the hard mask layer and calculating the average value thereof, and h2 is obtained by measuring each thickness at three random points in the patterned region of the hard mask layer and calculating the average value thereof. If the numerical result of the flattening degree is less than 5, "A" (excellent) is given, if it is between 5 and 10, "B" (good) is given, and if it exceeds 10, "C" (poor) is given. The results are shown in Table 3.
[0188] [Table 3]
[0189] Flattening feature Example 1 A Example 2 A Example 3 A Example 4 A Example 5 A Example 6 A Example 7 A Example 8 A Example 9 A Comparative Example 1 B Comparative Example 2 C
[0190] Referring to Table 3, the hard mask layers formed from the hard mask compositions of Comparative Examples 1 to 2 exhibited good or poor planarization degrees, but the hard mask layers formed from the hard mask compositions of Examples 1 to 9 exhibited excellent planarization degrees and thus exhibited extremely superior planarization characteristics.
[0191] Evaluation 4: Etching resistance
[0192] Each of the hard mask compositions of Examples 1 to 9 and Comparative Examples 1 to 2 was spin-coated on a silicon wafer and heat-treated on a hot plate at 160° C. for 1 minute to form a hard mask layer. The hard mask layer was dry-etched for 30 seconds using a CF4 / Ar mixed gas, and then before and after the dry etching, the film thickness meter manufactured by Komei Co., Ltd. was measured relative to each thickness, and then the bulk etch rate (BER) was calculated according to the calculation equation 2. The ratio of each etching rate of the hard mask layer of the composition of Examples 1 to 9 and Comparative Example 2 to the etching rate of the hard mask layer of the composition of Comparative Example 1 was calculated to evaluate the etching resistance. Specifically, when the etching rate is less than 0.95, "A" (excellent) is given, when greater than or equal to 0.95 and less than 1.00, "B" (good) is given, and when greater than or equal to 1.00, "C" (poor) is given. The results are shown in Table 4.
[0193] [Calculation equation 2]
[0194] Etching rate (angstroms / second) = (initial film thickness - film thickness after etching) / etching time (seconds)
[0195] [Table 4]
[0196] Etching resistance Example 1 A Example 2 A Example 3 A Example 4 A Example 5 A Example 6 A Example 7 A Example 8 A Example 9 A Comparative Example 1 - Comparative Example 2 C
[0197] Referring to Table 4, since each etching rate of the hard mask layer of the compositions of Examples 1 to 9 exhibits a ratio of less than 0.95 to the etching rate of the hard mask layer formed from the composition of Comparative Example 1, the hard mask layer of the compositions of Examples 1 to 9 exhibits excellent etching resistance compared to the hard mask layer formed from the composition of the Comparative Example.
[0198] In summary, there is a constant trend in the semiconductor industry to reduce the size of wafers. In response to this, the line width of the photoresist pattern in the photolithography technology can have a size of tens of nanometers. Therefore, the height of the line width that can withstand the photoresist pattern can be limited, and there are situations where the photoresist may not have sufficient resistance in the etching step. In order to compensate for this, an auxiliary layer called a hard mask layer can be used between the etched material layer and the photoresist layer. This hard mask layer can act as an interlayer for the fine pattern of the photoresist transferred by selective etching. Therefore, it may be necessary for the hard mask layer to have sufficient etching resistance to withstand the etching process during the pattern transfer.
[0199] Some hard mask layers may be formed in chemical or physical deposition methods, and may have low economic efficiency due to large-scale equipment and high process costs. Therefore, spin coating techniques for forming hard mask layers have recently been developed. Spin coating techniques may be a process that is easier to perform than conventional methods, and hard mask layers formed therefrom may exhibit more excellent gap filling characteristics and planarization characteristics. However, hard mask layers formed using spin coating techniques may have slightly reduced desired etch resistance. Therefore, it may be desirable for a hard mask composition to be applied to a spin coating technique and to ensure an etch resistance comparable to that of a hard mask layer formed in a chemical or physical deposition method.
[0200] In order to improve the etching resistance of the hard mask layer, research on maximizing the carbon content of the hard mask composition is being conducted. When the carbon content of the polymer included in the hard mask composition is maximized, the solubility of the polymer in the solvent can be reduced. The carbon content of the polymer included in the hard mask composition can be maximized to improve the etching resistance of the hard mask layer formed therefrom, while the polymer can be fully soluble in the solvent.
[0201] The hard mask composition according to some embodiments may include a compound having an aromatic hydrocarbon group to increase the carbon content of the composition. Therefore, the hard mask layer obtained from the composition can ensure excellent etching resistance. In addition, by containing a specific functional group, the compound can increase the carbon content of the composition and ensure excellent solubility in a solvent.
[0202] One or more embodiments may provide a hard mask composition that may be effectively applied to a hard mask layer.
[0203] One or more embodiments may provide a hard mask layer including a cured product of a hard mask composition.
[0204] One or more embodiments may provide a method of forming a pattern using a hard mask composition.
[0205] The hard mask composition according to some embodiments may have excellent solubility in a solvent and may be efficiently applied to a hard mask layer.
[0206] The hard mask composition according to some embodiments may have excellent cross-linking characteristics when cured, and a hard mask layer formed therefrom may help ensure excellent heat resistance and excellent etching resistance.
[0207] Example embodiments have been disclosed herein, and although specific terms are employed, the terms are used and interpreted in a generic and descriptive sense only and not for purposes of limitation. In some cases, as would be apparent to one of ordinary skill in the art (as of the time of filing this application), features, characteristics, and / or elements described with respect to a particular embodiment may be used alone or in combination with features, characteristics, and / or elements described with respect to other embodiments, unless specifically noted otherwise. Accordingly, it should be understood by those skilled in the art that various changes in form and details may be made without departing from the spirit and scope of the present invention as set forth in the claims above.
Claims
1. A hard mask composition comprising: A compound represented by Chemical Formula 1; as well as Solvents, [Chemical formula 1] Wherein, in Chemical Formula 1, Ar 1 and Ar 2 are each independently a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a group in which two or more substituted or unsubstituted C6 to C30 aromatic hydrocarbon groups are linked by a single bond or a substituted or unsubstituted C1 to C30 alkylene group, R 1 and R 2 are each independently hydrogen, deuterium, a substituted or unsubstituted monovalent C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted monovalent C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a combination thereof, and n is an integer of 2 to 6.
2. The hard mask composition according to claim 1, wherein Ar in Chemical Formula 1 1 and Ar 2 Substituted or unsubstituted groups each independently being part of Group 1: [Group 1] 3. The hard mask composition according to claim 1, wherein Ar in Chemical Formula 1 1 and Ar 2 Each independently a substituted or unsubstituted group that is part of Group 1-1: [Group 1-1] 4. The hard mask composition according to claim 1, wherein R 1 and R 2 Each is independently hydrogen, deuterium, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a combination thereof.
5. The hard mask composition according to claim 1, wherein R in Chemical Formula 1 1 and R 2 Each is independently hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C6 to C20 aromatic hydrocarbon group, or a combination thereof.
6. The hard mask composition according to claim 1, wherein in Chemical Formula 1, Ar 1 and Ar 2 are each independently a substituted or unsubstituted group that is part of Group 1-2, R 1 and R 2 are each independently hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C6 to C20 aromatic hydrocarbon group, or a combination thereof, and n is an integer from 2 to 4: [Group 1-2] 7. The hard mask composition according to claim 1, wherein in Chemical Formula 1, n is 2 or 3, and R 1 , R 2 and Ar 2 The same for each of them.
8. The hard mask composition according to claim 1, wherein: The compound represented by Chemical Formula 1 is represented by one of Chemical Formulas 2 to 10: [Chemical formula 2] [Chemical formula 3] [Chemical formula 4] [Chemical formula 5] [Chemical formula 6] [Chemical formula 7] [Chemical formula 8] [Chemical formula 9] [Chemical formula 10] 9 . The hardmask composition of claim 1 , wherein the compound has a molecular weight of 300 to 10,000 g / mol. 10 . The hardmask composition of claim 1 , wherein the compound is included in an amount of 0.1 wt % to 30 wt % based on the total weight of the hardmask composition.
11. The hardmask composition according to claim 1, wherein the solvent comprises propylene glycol, propylene glycol diacetate, methoxypropylene glycol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, acetylacetone or ethyl 3-ethoxypropionate. 12 . A hard mask layer comprising a cured product of the hard mask composition according to claim 1 .
13. A method for forming a pattern, the method comprising: providing a material layer on a substrate; applying the hard mask composition according to claim 1 to the material layer; thermally treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer; as well as The exposed portion of the material layer is etched. 14 . The method of forming a pattern according to claim 13 , wherein forming the hard mask layer comprises performing the heat treatment at 100° C. to 1,000° C.